Seed crystal bonding process for inhibiting back sublimation of SiC
By using a multi-layer composite structure of graphene film and carbide film in the SiC crystal growth process, combined with graphite ring packaging, the problems of sublimation and uneven bonding on the back of SiC are solved, and the quality and bonding stability of the crystal are significantly improved. .
Patent Information
- Application Number
- CN202410989055.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing SiC crystal growth process, thermal mismatch and uneven bonding between seed crystals and seed storks lead to the sublimation of SiC back and hexagonal hole defects. The mechanical strength of graphite paper is low, making it easy to delaminate or crack. question.
The graphene film is used as the flexible buffer layer on the back of the seed crystal, and the graphene film is bonded by spin coating and bonding glue, and vacuum hot pressing is carried out to form a multi-layer composite material of carbide film/graphene film/carbide film, and is combined with a graphite ring. Packaging to improve the stability of seed crystal bonding and the quality of SiC crystals.
The suppression of SiC back sublimation is achieved, the success rate of seed crystal bonding and crystal quality is improved, stress and defects are reduced, the uniformity and density of the film layer are ensured, and the layering or cracking problems of graphite paper are avoided.
Smart Images

Figure CN118932481A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular relates to a seed crystal bonding process for inhibiting SiC back sublimation. Background Art
[0002] As a third-generation semiconductor material, silicon carbide has many excellent properties, such as high critical breakdown field strength, saturated electron mobility, high thermal conductivity, etc., which give silicon carbide materials an irreplaceable position in high-power, high-frequency and high-temperature scenarios. The growth processes of silicon carbide crystals include physical vapor transport (PVT), high-temperature chemical vapor deposition (HTCVD) and top-seed solution growth (TSSG). Existing process technologies all need to be matched with a suitable seed crystal bonding process. Since the crystal growth temperature of SiC is relatively high, usually at 2000-2400°C, considering the high temperature tolerance, corrosion resistance and process compatibility, the industry generally uses flexible graphite materials as the bonding carrier between the seed crystal and the seed crystal holder.
[0003] In the early growth process, the seed crystal was bonded to the seed crystal holder by an organic adhesive, and after high-temperature vacuum carbonization, the adhesive was converted into a carbonized film. This method has two major disadvantages. First, there is a large thermal mismatch between the seed crystal and the seed crystal holder, which leads to large thermal stress. Second, the adhesive is usually prepared by spin coating, and the carbonized film layer is thin, while the machining flatness of the crucible cover is low. After the two are bonded, the graphite film layer is uneven, resulting in weak bonding, bubbles, excessive stress and sublimation of the back of the seed crystal during the crystal growth process. The existing technology uses graphite paper as a bonding buffer medium to bond the seed crystal to the graphite paper, and then bonds the other side of the graphite paper to the seed crystal holder. Graphite paper has a relatively low density (about 0.7-1.3 g / cm 3 ), based on the theoretical density of graphite 2.25g / cm 3 In terms of conversion, its porosity is as high as 50%, and the airtightness of the back of the seed crystal is poor. In addition, the mechanical strength of graphite paper is low, and under the thermal stress of the seed crystal and the seed crystal holder, the graphite paper is very likely to be delaminated or cracked. In areas where there are pores, delamination or cracks in the graphite paper, due to differences in heat transfer, the temperature distribution on the back of the seed crystal is uneven, and evaporation occurs near the pores, resulting in sublimation on the back of the seed crystal and the generation of hexagonal hole defects. Summary of the invention
[0004] The present invention aims to provide a seed crystal bonding process for inhibiting sublimation of the back of SiC, using a graphene film as a flexible buffer layer on the back of the seed crystal, fixing the graphene film on the back of the seed crystal by bonding, forming a carbonized film / graphene film / carbonized film multilayer composite material between the seed crystal and the seed crystal holder by hot pressing, and then cooperating with the packaging treatment of a graphite ring, thereby solving the sublimation problem of the back of SiC growth, and improving the success rate of seed crystal bonding and the quality of SiC crystals.
[0005] In order to achieve the above purpose, the technical solutions adopted are as follows:
[0006] A seed crystal bonding process for inhibiting SiC back sublimation comprises the following steps:
[0007] (1) applying adhesive glue on the back side of the seed crystal and the first side of the graphene film by spin coating, and then drying the adhesive film;
[0008] (2) placing the back side of the seed crystal and the first side of the graphene film dried adhesive film face to face, and performing a first vacuum hot pressing treatment;
[0009] (3) applying adhesive glue on the wafer-type seed crystal holder and the second surface of the graphene film by spin coating, and then drying the adhesive film;
[0010] (4) placing the wafer-type seed crystal holder and the adhesive film dried on the second side of the graphene film face to face, and performing a second vacuum hot pressing process to form a carbonized film / graphene film / carbonized film multilayer composite material between the seed crystal and the seed crystal holder to obtain a SiC seed crystal bonding sheet;
[0011] (5) The SiC seed crystal bonding sheet is encapsulated using a graphite ring of matching size to complete the bonding process.
[0012] According to the above scheme, the viscosity of the bonding glue in step 1 and step 3 is 10-1000mPa·s, the spin coating speed is 500-4000rpm, the spin coating time is 20-60s, the drying temperature is 50-120℃, the drying time is 2-20min, the thickness of the obtained film after drying is 0.5-50μm, and the uniformity of the film thickness is ±5%.
[0013] According to the above scheme, the temperature of the first vacuum hot pressing treatment in step 2 is 150-260°C, the heating time is 30-120min, the vacuum degree is less than 5Pa, the pressure is 600-1500N, and the hot pressing time is 30-120min.
[0014] According to the above scheme, the second vacuum hot pressing treatment in step 4 is carried out in two stages; the hot pressing temperature in the first stage is 150-260°C, the heating time is 30-120min, the vacuum degree is less than 5Pa, the pressure is 600-1500N, and the hot pressing time is 30-120min; the hot pressing temperature in the second stage is 500-800°C, the heating time is 60-240min, the vacuum degree is less than 5Pa, the pressure is 600-1500N, and the hot pressing time is 60-240min.
[0015] According to the above scheme, the bonding glue is an organic solution of an adhesive; the adhesive is one or more of epoxy resin, polyimide, polyamic acid, phenolic resin, and polymethyl methacrylate; the organic solvent is one or more of propylene glycol methyl ether acetate, N,N-dimethylacetamide, N-methylpyrrolidone, methanol, ethanol, acetone, and chloroform; the mass percentage concentration of the adhesive is 20 to 50%.
[0016] According to the above scheme, the graphene film has a film thickness of 50-500 μm and a density of 2.00-2.15 g / cm 3 , porosity is less than 10%; wherein the size of the graphene microscopic sheet is greater than 50nm, the angle between the graphene microscopic sheet and the surface of the graphene film is less than 20°, and the roughness Ra of both sides of the graphene film is less than 3.2μm.
[0017] According to the above solution, the wafer-type seed crystal holder adopts graphite paper or graphene thick film.
[0018] According to the above scheme, the diameter D2 of the graphene film is greater than or equal to the diameter D1 of the seed crystal, and the diameter D3 of the disc-type seed crystal holder is greater than or equal to the diameter D2 of the graphene film, satisfying the numerical relationship: D2-D1=0~40mm, D3-D2=0~40mm; the inner diameter D4 and outer diameter D5 of the graphite ring satisfy the numerical relationship: D4-D2=-10~10mm, D5-D3=-10~10mm; the end face of the graphite ring that cooperates with the SiC seed crystal bonding sheet is provided with 1~3 steps.
[0019] According to the above solution, the gap between the SiC seed crystal bonding sheet and the crucible cover is 0.1 to 30 mm.
[0020] According to the above scheme, the SiC crystal growth method applicable to the seed crystal bonding process is PVT, HTCVD or TSSG; the crystal structure of the seed crystal is one of 3C, 4H, 6H, and 15R, which is a single crystal phase.
[0021] The present invention obtains a glue film with excellent film uniformity through a spin coating process, which can ensure good bonding between the seed crystal and the graphene film. After high-temperature carbonization, the amorphous glue carbonized film is thin and does not affect the effect of the graphene film in inhibiting back sublimation.
[0022] The present invention uses a graphene film as a bonding transition layer on the back side of a seed crystal, adopts a low-viscosity bonding glue to bond the seed crystal and the graphene film, and after hot pressing and curing, bonds the other side of the graphene film to a disc-type seed crystal holder, and after a second hot pressing and high-temperature carbonization, forms a SiC seed crystal bonding sheet having a sandwich structure of a seed crystal, a carbonized film / graphene film / carbonized film multilayer composite material, and a seed crystal holder.
[0023] Graphene film plays an important role in improving the quality of crystals in the following aspects. First, the density of graphene film is close to the theoretical density of graphite, the porosity is low, and the graphene microscopic sheets are almost parallel to the surface of the seed crystal. The continuous and dense graphene film greatly reduces the sublimation channel on the back of the seed crystal; second, under the crystal growth temperature, the difference in thermal expansion coefficient between the seed crystal cover and the seed crystal will produce a large stress, and the strained seed crystal will induce the proliferation of various defects such as basal plane dislocation (BPD), and the interaction between the parallel arranged graphene film layers is van der Waals force. The layers can slide under the action of stress, and the graphene film acts as a strain buffer. The stress and defect levels of the crystal are reduced synchronously. The SiC seed crystal bonding sheet and the crucible graphite piece are softly connected, and a gap is reserved between the SiC seed crystal bonding sheet and the crucible cover. This structure can greatly optimize the temperature field in the seed crystal area and reduce internal stress.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1) By adopting the seed crystal bonding scheme of the present invention, a uniform, continuous, dense and well-bonded seed crystal bonding sheet can be obtained, and there is no sublimation phenomenon on the back of the crystal after the crystal growth is completed.
[0026] 2) The graphene film used in the present invention has a lamellar structure, which can buffer the strain caused by thermal expansion between the seed crystal and the seed crystal holder, greatly reduce the stress in the seed crystal area, and reduce the crystal defect index and cracking risk.
[0027] 3) The SiC seed crystal bonding sheet cooperates with the designed graphite ring or graphite expansion ring. The graphite ring is used to support the seed crystal. A gap is left between the back of the SiC seed crystal bonding sheet and the crucible cover. This gap has the function of homogenizing the temperature field, reducing the radial temperature gradient in the seed crystal area, and further reducing the internal stress of the seed crystal. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 : Schematic diagram of the top view of graphene membrane.
[0029] Figure 2 : Schematic diagram of the side view of graphene membrane.
[0030] Figure 3 : Schematic diagram of the SiC seed crystal bonding sheet structure.
[0031] Figure 4 : Schematic diagram of the structure of SiC seed crystal bonding sheet encapsulated by graphite ring.
[0032] Figure 5 : Actual photo of the back side of the SiC ingot prepared in Example 1.
[0033] Figure 6 : Actual photo of the back side of the SiC ingot prepared in Example 2.
[0034] Figure 7 : Actual photo of the back side of the SiC ingot prepared in Example 3.
[0035] Figure 8 : Actual photo of the back side of the SiC ingot prepared in Comparative Example 1.
[0036] 1-graphene sheet; 2-graphene sheet boundary; 3-SiC seed crystal; 4-carbonized film; 5-graphene film; 6-seed crystal holder; 7-graphite ring. DETAILED DESCRIPTION
[0037] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.
[0038] The graphene film provided in the specific embodiment is prepared by liquid phase exfoliation of graphite oxide, followed by coating film formation, high temperature reduction, hot pressing and purification, and can also be prepared by chemical vapor deposition. Figure 1 and Figure 2 Schematic diagram of the top view and side view of the graphene film, where 1 is a graphene sheet, 2 is a graphene sheet boundary, and the graphene sheet is nearly parallel to the surface of the graphene film.
[0039] The specific embodiment provides a seed crystal bonding process for suppressing SiC back sublimation:
[0040] (1) applying adhesive glue on the back side of the seed crystal and the first side of the graphene film by spin coating, and then drying the adhesive film;
[0041] (2) placing the back side of the seed crystal and the first side of the graphene film dried adhesive film face to face, and performing a first vacuum hot pressing treatment;
[0042] (3) applying adhesive glue on the wafer-type seed crystal holder and the second surface of the graphene film by spin coating, and then drying the adhesive film;
[0043] (4) placing the wafer-type seed crystal holder and the dried adhesive film on the second side of the graphene film face to face, and performing a second vacuum hot pressing process to form a carbonized film / graphene film / carbonized film multilayer composite material between the seed crystal and the seed crystal holder to obtain a SiC seed crystal bonding sheet; refer to the attached Figure 3 As shown, from bottom to top are SiC seed crystal 3, carbonized film 4, graphene film 5, carbonized film 4, seed crystal holder 6;
[0044] (5) Use a graphite ring 7 of matching size to encapsulate the SiC seed crystal bonding sheet to complete the bonding process, see the attached Figure 4 shown.
[0045] Example 1
[0046] This embodiment provides a seed crystal bonding process for suppressing SiC back sublimation, and the process steps are as follows:
[0047] 1) Prepare bonding glue, the adhesive is polyimide, the solvent is N,N-dimethylacetamide, and the mass ratio of the adhesive to the solvent is 1:4;
[0048] 2) Take a 6-inch 4H silicon carbide seed crystal with a thickness of 350 μm and a diameter of 153 mm;
[0049] 3) Select the graphene film prepared by liquid phase exfoliation method, the graphene sheet size is 120nm, and the density is 2.10g / cm 3 , the angle between the graphene sheet and the graphene film surface is less than 10°, the surface roughness Ra = 1.6 μm, the graphene film is cut, the film thickness is 100 μm, and the diameter is 160 mm;
[0050] 4) Spin-coat the bonding glue on the Si surface of the silicon carbide seed crystal and the first surface of the graphene film, first at 500 rpm for 10 seconds, then at 1500 rpm for 30 seconds, and then bake at 100° C. for 10 minutes;
[0051] 5) placing the seed crystal coated surface and the first coated surface of the graphene film face to face for the first vacuum hot pressing treatment, the first vacuum hot pressing treatment temperature is 200° C., the heating time is 90 min, the vacuum degree is less than 5 Pa, the pressure is 1000 N, and the hot pressing time is 90 min;
[0052] 6) After the hot pressing is completed, the seed crystal is taken out, and graphite paper with a thickness of 0.50 mm is selected. The diameter of the seed crystal holder bonding the seed crystal is 170 mm. The bonding glue is spin-coated on the second side of the graphene film and the surface of the seed crystal holder. The glue is first spread at a speed of 500 rpm for 10 seconds, then spread at a speed of 1500 rpm for 30 seconds, and then baked at 100 ° C for 10 minutes;
[0053] 7) The seed crystal support glue-coated surface and the second glue-coated surface of the graphene film are placed face to face for a second vacuum hot pressing treatment. The second vacuum hot pressing treatment is carried out in two stages. The hot pressing temperature of the first stage is 200° C., the heating time is 90 min, the vacuum degree is less than 5 Pa, the pressure is 1000 N, and the hot pressing time is 90 min; the hot pressing temperature of the second stage is 600° C., the heating time is 180 min, the vacuum degree is less than 5 Pa, the pressure is 1000 N, and the hot pressing time is 180 min;
[0054] 8) After the hot pressing is completed, the temperature is slowly cooled to room temperature, and the cooling time is 180 minutes to complete the seed crystal bonding process;
[0055] 9) Select a graphite ring with an outer diameter of 157 mm, an inner diameter of 151 mm, and a height of 35 mm, and match it with the SiC seed crystal bonding sheet. The gap between the back of the assembly and the crucible cover is 5 mm;
[0056] 10) Performing SiC crystal growth experiments by PVT method using the above seed crystal bonding and fixing scheme;
[0057] 11) After the crystal growth is completed, the graphite material on the back of the ingot is scraped off with a scraper, and the back of the ingot is sublimated without back. Figure 5 shown.
[0058] Example 2
[0059] This embodiment provides a seed crystal bonding process for suppressing SiC back sublimation, and the process steps are as follows:
[0060] 1) preparing bonding glue, wherein the adhesive is phenolic resin, the solvent is N-methylpyrrolidone, and the mass ratio of the adhesive to the solvent is 1:3.5;
[0061] 2) Take a 6-inch 4H silicon carbide seed crystal with a thickness of 350 μm and a diameter of 153 mm;
[0062] 3) Select the graphene film prepared by liquid phase exfoliation method, the graphene sheet size is 100nm, and the density is 2.05g / cm 3 , the angle between the graphene sheet and the graphene film surface is less than 10°, the surface roughness Ra = 1.6 μm, the graphene film is cut, the film thickness is 150 μm, and the diameter is 160 mm;
[0063] 4) Spin-coat the bonding glue on the Si surface of the silicon carbide seed crystal and the first surface of the graphene film, first at 500 rpm for 10 seconds, then at 1200 rpm for 40 seconds, and then bake at 120° C. for 20 minutes;
[0064] 5) placing the seed crystal coated surface and the first coated surface of the graphene film face to face for the first vacuum hot pressing treatment, the first vacuum hot pressing treatment temperature is 170° C., the heating time is 90 min, the vacuum degree is less than 5 Pa, the pressure is 1200 N, and the hot pressing time is 90 min;
[0065] 6) After the hot pressing is completed, the seed crystal is taken out, and graphite paper with a thickness of 0.75 mm and a diameter of 165 mm is selected. The bonding glue is spin-coated on the second side of the graphene film and the surface of the graphite paper. The glue is first spread at a speed of 500 rpm for 10 seconds, then spread at a speed of 1200 rpm for 40 seconds, and then baked at 120° C. for 20 minutes;
[0066] 7) The glue-coated surface of the graphite paper and the second glue-coated surface of the graphene film are placed face to face for a second vacuum hot pressing treatment. The second vacuum hot pressing treatment is carried out in two stages. The hot pressing temperature of the first stage is 170° C., the heating time is 90 min, the vacuum degree is less than 5 Pa, the pressure is 1200 N, and the hot pressing time is 90 min; the hot pressing temperature of the second stage is 650° C., the heating time is 150 min, the vacuum degree is less than 5 Pa, the pressure is 1200 N, and the hot pressing time is 150 min;
[0067] 8) After the hot pressing is completed, the temperature is slowly cooled to room temperature, and the cooling time is 180 minutes to complete the seed crystal bonding process;
[0068] 9) Select a graphite ring with an outer diameter of 168 mm, an inner diameter of 153 mm, and a height of 38 mm, and match it with the SiC seed crystal bonding sheet. The gap between the back of the assembly and the crucible cover is 2 mm;
[0069] 10) Performing SiC crystal growth experiments by PVT method using the above seed crystal bonding and fixing scheme;
[0070] 11) After the crystal growth is completed, the graphite material on the back of the ingot is scraped off with a scraper, and the back of the ingot is sublimated without back. Figure 6 shown.
[0071] Example 3
[0072] This embodiment provides a seed crystal bonding process for suppressing SiC back sublimation, and the process steps are as follows:
[0073] 1) Prepare bonding glue, the adhesive is epoxy resin, the solvent is acetone, and the mass ratio of the adhesive to the solvent is 1:3;
[0074] 2) Take a 6-inch 4H silicon carbide seed crystal with a thickness of 350 μm and a diameter of 153 mm;
[0075] 3) Select chemical vapor deposition graphene film, graphene sheet size 150nm, density 2.12g / cm3 , the angle between the graphene sheet and the graphene film surface is less than 10°, the surface roughness Ra = 1.6 μm, the graphene film is cut, the film thickness is 100 μm, and the diameter is 160 mm;
[0076] 4) Spin-coat the bonding glue on the Si surface of the silicon carbide seed crystal and the first surface of the graphene film, first at 500 rpm for 10 seconds, then at 1000 rpm for 20 seconds, and then bake at 50°C for 15 minutes;
[0077] 5) placing the seed crystal coated surface and the first coated surface of the graphene film face to face for the first vacuum hot pressing treatment, the first vacuum hot pressing treatment temperature is 160° C., the heating time is 90 min, the vacuum degree is less than 5 Pa, the pressure is 800 N, and the hot pressing time is 90 min;
[0078] 6) After the hot pressing is completed, the seed crystal is taken out, and a graphene thick film with a thickness of 0.5 mm and a diameter of 170 mm is selected. The bonding glue is spin-coated on the second surface of the graphene film and the first surface of the graphene thick film. The glue is first spread at a speed of 500 rpm for 10 seconds, then spread at a speed of 1000 rpm for 20 seconds, and then baked at 50° C. for 15 minutes;
[0079] 7) Placing the graphene thick film glue-coated surface and the graphene film second glue-coated surface face to face for a second vacuum hot pressing treatment, the second vacuum hot pressing treatment is carried out in two stages, the first stage hot pressing temperature is 200°C, the heating time is 90min, the vacuum degree is less than 5Pa, the pressure is 800N, and the hot pressing time is 90min; the second stage hot pressing temperature is 700°C, the heating time is 180min, the vacuum degree is less than 5Pa, the pressure is 800N, and the hot pressing time is 180min;
[0080] 8) After the hot pressing is completed, the temperature is slowly cooled to room temperature, and the cooling time is 180 minutes to complete the seed crystal bonding process;
[0081] 9) Select a graphite ring with an outer diameter of 158 mm, an inner diameter of 152 mm, and a height of 39 mm, and match it with the SiC seed crystal bonding sheet. The gap between the back of the assembly and the crucible cover is 1 mm;
[0082] 10) Performing SiC crystal growth experiments by PVT method using the above seed crystal bonding and fixing scheme;
[0083] 11) After the crystal growth is completed, the graphite material on the back of the ingot is scraped off with a scraper, and the back of the ingot is sublimated without back. Figure 7 shown.
[0084] Comparative Example 1
[0085] 1) Prepare bonding glue, the adhesive is epoxy resin, the solvent is acetone, and the mass ratio of the adhesive to the solvent is 1:3;
[0086] 2) Take a 6-inch 4H silicon carbide seed crystal with a thickness of 350 μm and a diameter of 153 mm;
[0087] 3) Select graphite paper with a thickness of 0.5 mm and a diameter of 160 mm;
[0088] 4) Spin-coat the adhesive glue on the Si surface of the silicon carbide seed crystal and the first surface of the graphite paper, first at 500 rpm for 10 seconds, then at 1200 rpm for 40 seconds, and then bake at 120°C for 20 minutes;
[0089] 5) placing the seed crystal coated surface and the first coated surface of the graphite paper face to face for the first vacuum hot pressing treatment, the first vacuum hot pressing treatment temperature is 170° C., the heating time is 90 min, the vacuum degree is less than 5 Pa, the pressure is 1200 N, and the hot pressing time is 90 min;
[0090] 6) Select a crucible cover, wherein the diameter of the crucible cover contacting the seed crystal surface is 180 mm, and the thickness of the crucible cover is 20 mm;
[0091] 7) After the hot pressing is completed, the seed crystal is taken out, and the bonding glue is spin-coated on the second side of the graphite paper. The bonding is firstly spread at a speed of 500 rpm for 10 seconds, and then at a speed of 1200 rpm for 40 seconds. Then, the bonding is baked at 120°C for 20 minutes, and the bonding glue is sprayed on the surface of the crucible cover that is attached to the seed crystal. The thickness of the sprayed glue is 3 μm;
[0092] 8) The glue-coated surface of the graphite paper and the glue-sprayed surface of the crucible cover are placed face to face for a second vacuum hot pressing treatment. The second vacuum hot pressing treatment is carried out in two stages. The hot pressing temperature in the first stage is 170° C., the heating time is 90 min, the vacuum degree is less than 5 Pa, the pressure is 1200 N, and the hot pressing time is 90 min; the hot pressing temperature in the second stage is 650° C., the heating time is 150 min, the vacuum degree is less than 5 Pa, the pressure is 1200 N, and the hot pressing time is 150 min;
[0093] 9) After the hot pressing is completed, the temperature is slowly cooled to room temperature, and the cooling time is 180 minutes to complete the seed crystal bonding process;
[0094] 10) Using the above seed crystal bonding and fixing scheme, a SiC crystal growth experiment was carried out using the PVT method;
[0095] 11) After the crystal growth is completed, the graphite material on the back of the ingot is scraped off with a scraper. A large number of back sublimation areas appear on the back of the ingot. Figure 8 shown.
Claims
1. A seed crystal bonding process to inhibit SiC back sublimation, Features The following steps are involved: (1) applying adhesive glue on the back side of the seed crystal and the first side of the graphene film by spin coating, and then drying the adhesive film; (2) placing the back side of the seed crystal and the first side of the graphene film dried film face to face, and performing a first vacuum hot pressing treatment; (3) applying adhesive glue on the wafer-type seed crystal holder and the second surface of the graphene film by spin coating, and then drying the adhesive film; (4) placing the wafer-type seed crystal holder and the adhesive film dried on the second side of the graphene film face to face, and performing a second vacuum hot pressing process to form a carbonized film / graphene film / carbonized film multilayer composite material between the seed crystal and the seed crystal holder to obtain a SiC seed crystal bonding sheet; (5) The SiC seed crystal bonding sheet is encapsulated using a graphite ring of matching size to complete the bonding process.
2. The seed crystal bonding process for suppressing SiC back sublimation as claimed in claim 1, Features The viscosity of the adhesive in step 1 and step 3 is 10-1000 mPa·s, the spin coating speed is 500-4000 rpm, the spin coating time is 20-60 s, the drying temperature is 50-120°C, the drying time is 2-20 min, the thickness of the obtained adhesive film after drying is 0.5-50 μm, and the uniformity of the film thickness is ±5%.
3. The seed crystal bonding process for suppressing SiC back sublimation as claimed in claim 1, Features In step 2, the temperature of the first vacuum hot pressing treatment is 150-260° C., the heating time is 30-120 min, the vacuum degree is less than 5 Pa, the pressure is 600-1500 N, and the hot pressing time is 30-120 min.
4. The seed crystal bonding process for suppressing SiC back sublimation as claimed in claim 1, Features The second vacuum hot pressing treatment in step 4 is carried out in two stages; the hot pressing temperature in the first stage is 150-260°C, the heating time is 30-120min, the vacuum degree is less than 5Pa, the pressure is 600-1500N, and the hot pressing time is 30-120min; the hot pressing temperature in the second stage is 500-800°C, the heating time is 60-240min, the vacuum degree is less than 5Pa, the pressure is 600-1500N, and the hot pressing time is 60-240min.
5. The seed crystal bonding process for suppressing SiC back sublimation as claimed in claim 1, Features The bonding glue is an organic solution of an adhesive; the adhesive is one or more of epoxy resin, polyimide, polyamic acid, phenolic resin, and polymethyl methacrylate; the organic solvent is one or more of propylene glycol methyl ether acetate, N,N-dimethylacetamide, N-methylpyrrolidone, methanol, ethanol, acetone, and chloroform; the mass percentage concentration of the adhesive is 20-50%.
6. The seed crystal bonding process for suppressing SiC back sublimation as claimed in claim 1, Features The graphene film has a thickness of 50 to 500 μm and a density of 2.00 to 2.15 g / cm 3 , porosity is less than 10%; wherein the size of the graphene microscopic sheet is greater than 50nm, the angle between the graphene microscopic sheet and the surface of the graphene film is less than 20°, and the roughness Ra of both sides of the graphene film is less than 3.2μm.
7. The seed crystal bonding process for suppressing SiC back sublimation as claimed in claim 1, Features The wafer-type seed crystal holder adopts graphite paper or graphene thick film.
8. The seed crystal bonding process for suppressing SiC back sublimation as claimed in claim 1, Features The diameter D2 of the graphene film is greater than or equal to the diameter D1 of the seed crystal, and the diameter D3 of the disc-type seed crystal holder is greater than or equal to the diameter D2 of the graphene film, satisfying the numerical relationship: D2-D1=0~40mm, D3-D2=0~40mm; the inner diameter D4 and outer diameter D5 of the graphite ring satisfy the numerical relationship: D4-D2=-10~10mm, D5-D3=-10~10mm; the end face of the graphite ring that cooperates with the SiC seed crystal bonding sheet is provided with 1~3 steps.
9. The seed crystal bonding process for suppressing SiC back sublimation as claimed in claim 1, Features The gap between the SiC seed crystal bonding sheet and the crucible cover is 0.1-30 mm.
10. The seed crystal bonding process for suppressing SiC back sublimation as claimed in claim 1, Features The SiC crystal growth method applicable to the seed crystal bonding process is PVT, HTCVD or TSSG; the crystal structure of the seed crystal is one of 3C, 4H, 6H, and 15R, which is a single crystal phase.
Citation Information
Cited By
Seed crystal bonding method for inhibiting back sublimation of SiC
CN121110173A
High-residual-carbon low-pore anti-reverse-sublimation silicon carbide seed crystal composite bonding process
CN122833704A