Preparation method and application of two-dimensional ErOCl thin film material
By preparing two-dimensional erbium oxychloride (ErOCl) film materials, using their high dielectric constant characteristics, the problem of lack of high K gate dielectrics in two-dimensional electronic devices is solved, and efficient ErOCl film synthesis is achieved for field effect transistors , significantly improves device performance and stability and alleviates the short channel effect.
Patent Information
- Application Number
- CN202410992457.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the preparation of two-dimensional electronic device materials lacks a suitable high dielectric constant (K) gate dielectric, resulting in a short channel effect after the transistor size is reduced, affecting device performance, and the amorphous structure and hanging bonds of traditional materials. Causes charge transfer problems.
By designing chemical formulas and process conditions, a two-dimensional erbium oxychloride (ErOCl) film material was prepared, and using its high K characteristics as gate dielectric, it achieved efficient ErOCl film synthesis, used for the preparation of field effect transistors, providing an atom Level pure interface to reduce interface capture state and substrate scattering effects.
It realizes the efficient preparation of ErOCl film materials, has good chemical stability and mechanical strength, and is suitable for large-scale production, which significantly improves the electrical performance of field effect transistors, including low leakage current and good switching characteristics, alleviates short channels. effect.
Smart Images

Figure CN118932483A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor materials and devices, and in particular relates to a preparation method of a two-dimensional ErOCl thin film material and application thereof. Background Art
[0002] In order to meet the ever-evolving technological needs and improve the performance of electronic devices (including speed, power consumption and computing power), the size of traditional silicon-based field-effect transistors (FETs) is being reduced. However, this size reduction has also caused the so-called short channel effect, which is an undesirable phenomenon. It is reported that the size of transistors can be effectively reduced by using ultra-thin channel materials and dielectric layers with high dielectric constants (K). Integrating high-mobility two-dimensional (2D) semiconductor channels with ultra-thin high-K gate dielectrics in transistors is expected to alleviate the above effects. However, the subsequent manufacturing is hindered by the lack of suitable 2D high-K gate dielectrics.
[0003] In the field of insulators, silicon dioxide, aluminum oxide, and hafnium dioxide are commonly used. Although these materials are widely used for their excellent electrical insulation properties, their amorphous structural characteristics and the presence of dangling bonds lead to several problems in the charge transport process. Specifically, the amorphous structure of these materials may act as charge scattering centers, while dangling bonds may cause charge trapping phenomena, both of which have an adverse effect on device performance. The electronic properties of 2D FETs often rely on their intrinsic defects, surface adsorption, or interface perturbations. Defects are located at the interface (such as oxide dangling bonds) and in the channel, exhibiting fast charge exchange and affecting the subthreshold swing (SS), while scattering at these defects reduces mobility. Boundary traps can also lead to various instabilities in the device threshold voltage, including flicker noise, hysteresis, and long-term drifts known as bias temperature instability in silicon technology. Therefore, new high-K van der Waals (VDW) dielectrics, which have no dangling bonds on the surface, exhibit atomic smoothness, and have low defect density and high breakdown field (EBD), are more suitable for 2D electronics. By using this high KVDW dielectric, we can construct an atomically pure interface between the semiconductor channel and the dielectric layer, which almost eliminates the existence of interface trapping states and effectively avoids unnecessary substrate scattering effects. The optimization of this interface directly improves the accuracy and response speed of gate control, while significantly reducing the hysteresis caused by charge storage. Therefore, the introduction of high KVDW dielectrics has important practical significance and application potential for improving the performance of 2D electronic devices, especially in terms of gate regulation efficiency and stability. Ultrathin VDW erbium oxychloride (ErOCl) has the characteristics of wide bandgap, high dielectric constant, suitable band offset, small stripping energy, air stability and insolubility in water, and is considered to be a promising gate dielectric material. In recent years, reports have pointed out the application potential of LaOCl in next-generation electronic devices. Given the structural similarity between ErOCl and LaOCl, we have reason to believe that ErOCl also has the potential to become a high-performance gate dielectric material. It also has certain potential for application in next-generation electronic devices. Therefore, the preparation of large-area erbium oxychloride is expected to promote the development of field-effect transistors. Summary of the invention
[0004] The present invention aims to solve the limitations of the prior art in the preparation of two-dimensional electronic device materials, and provides a preparation method and application of a two-dimensional erbium oxychloride (ErOCl) thin film material. The method realizes the efficient synthesis of ErOCl thin film materials through the designed chemical formula and process conditions: ErOCl powder is mixed with a specific flux in an optimized ratio to form a uniform precursor mixture. Subsequently, large-area growth of ErOCl thin film is achieved by precisely controlling the heating temperature, the holding time and the reaction atmosphere. The obtained thin film material has good chemical stability and a certain mechanical strength, while maintaining the characteristics of non-toxicity and environmental protection. The two-dimensional ErOCl thin film material prepared by this method not only has a simple preparation process, but also has high cost-effectiveness and is suitable for large-scale production. In addition, the field effect transistor prepared based on this material exhibits good electrical properties, including low leakage current and good switching characteristics.
[0005] The method for preparing the two-dimensional ErOCl thin film material of the present invention comprises the following steps:
[0006] The ErOCl powder and flux in a mass ratio of 1:1 to 3:1 are mixed to obtain a precursor; the precursor is kept warm for 5-30 minutes at a temperature of 500-900°C in an inert gas atmosphere, and then naturally cooled to room temperature to obtain a two-dimensional ErOCl thin film material.
[0007] The specific operation steps are as follows: first, grind the ErCl3·6H2O powder into fine powder, and place it in a muffle furnace for heating at a temperature range of 500°C to 900°C, and keep it at this temperature for 12 to 24 hours to calcine to obtain ErOCl powder; next, mix the obtained ErOCl powder with a flux in a preset ratio, place it in a quartz test tube as a precursor, place the quartz test tube containing the precursor in the central temperature zone of a horizontal tube furnace, and place the substrate near the precursor powder, then introduce inert gas into the tube furnace, heat the precursor to 500-900°C, keep the temperature for 5-30 minutes, and then naturally cool it to room temperature, thereby obtaining a two-dimensional ErOCl thin film material.
[0008] The flux is a chloride salt selected from one or more of sodium chloride, ammonium chloride and potassium chloride, and is used to reduce the melting point of ErOCl powder.
[0009] The substrate is any one of a doped silicon wafer with an oxide layer, a mica wafer, and a sapphire.
[0010] The thickness of the two-dimensional ErOCl thin film material is 5-400nm, and the area of the film is at the centimeter level.
[0011] The inert gas is argon, and the flow rate is controlled to be 30-200 sccm.
[0012] During the preparation process, the distance between the source and the substrate is controlled at 0-5 mm.
[0013] Application of the two-dimensional ErOCl thin film material of the present invention in preparing field effect transistors.
[0014] The field effect transistor includes a substrate and the two-dimensional ErOCl thin film material placed on the substrate. The multilayer or single layer of molybdenum disulfide obtained by mechanical peeling acts as a semiconductor and a pair of electrodes are deposited on the MoS2 layer. An appropriate distance must be maintained between the electrodes to ensure an effective current transmission path while avoiding short circuit.
[0015] Furthermore, the substrate is any one of a doped silicon wafer with an oxide layer, a mica wafer, and a sapphire; the electrode is any one or more of indium gold, silver, tin, and copper electrodes; and the thickness of the electrode is 50 to 100 nm.
[0016] During the specific preparation, the grown two-dimensional ErOCl thin film material is transferred to the surface of the substrate, and then the multilayer or single layer of molybdenum disulfide obtained by mechanical peeling is transferred onto the two-dimensional ErOCl thin film material, and then the electrode pattern is engraved on the surface of the molybdenum disulfide material. Finally, according to the engraved electrode pattern, two electrodes are deposited on the surface of the molybdenum disulfide layer respectively.
[0017] Furthermore, before depositing the electrode, an adhesion layer is first evaporated, and the adhesion layer is indium metal with a thickness of 10-15 nm.
[0018] Nanosheet growth can be understood as single crystal growth. The particles inside the crystal are regularly and periodically arranged in three-dimensional space. The arrangement of particles in the entire crystal in space is long-range ordered, and the lattice is continuous. Two-dimensional nanosheets focus on growth in the two-dimensional direction. They grow according to certain rules in the two-dimensional direction, and the growth in thickness is relatively small compared to the other two directions. Thin film preparation focuses more on growth in the two-dimensional direction. Ideal thin film growth is best achieved by the growth of single crystals of materials. However, due to the self-limitation of single crystal materials, they generally grow in three directions at the same time. Therefore, the increase in the size in the two-dimensional direction will also increase the thickness and thus fail to meet the two-dimensional requirements. Therefore, most general thin films are polycrystalline growth. The present invention prepares a polycrystalline thin film. The difficulty is to regulate the growth conditions so that the polycrystalline is connected into a thin film. At present, there is little research on rare earth oxyhalides, and there is basically no research on ErOCl thin films.
[0019] The atomic number of rare earth elements is relatively large, and most stable rare earth compounds have relatively high melting points. Currently, the main methods for preparing rare earth oxyhalides are solution reaction method and CVD preparation method; the solution method mainly prepares nanosheets, and the solution is heated at low temperature and compounds are added to react, and the generated nanosheets are relatively small in size; when using CVD or PVD methods to prepare rare earth oxyhalide compounds, the reaction source is evaporated from powder into gas at a relatively high temperature, and then the gaseous source reacts on a specific substrate, and the crystal nucleus grows into nanosheets according to a certain rule. In this process, the content of the source, the distance between the source and the substrate, the temperature of the furnace, and the insulation time are all very important influencing factors. The present invention prepares nanosheets on a substrate by regulating the above factors, and then obtains ErOCl thin films.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0021] 1. The present invention designs characteristic parameters for preparing ErOCl thin film materials, especially the mass ratio of ErOCl powder and flux, so that the method of the present invention is simple to implement, has a high success rate, and has high sample quality. It is also compatible with existing PVD processes and is suitable for the growth and large-scale application of large-size samples.
[0022] 2. The ErOCl thin film material prepared by the present invention can be used as a gate insulating material for field effect transistors, and has the advantages of high environmental stability and non-toxicity, and is expected to alleviate the short channel effect currently caused by the continuous reduction in the size of field effect transistors.
[0023] 3. The present invention uses a two-dimensional micro-nano device as the gate of a field effect transistor, which has the advantages of easy integration and process compatibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the structure of the ErOCl crystal prepared in Example 1 of the present invention.
[0025] Figure 2 This is an optical microscope top view of the two-dimensional ErOCl thin film material prepared in Example 3 of the present invention.
[0026] Figure 3 This is an optical microscope top view of the two-dimensional ErOCl thin film material prepared in Example 3 of the present invention.
[0027] Figure 4 This is an atomic force microscope image of the two-dimensional ErOCl thin film material prepared in Example 3 of the present invention.
[0028] Figure 5 This is a picture of a mica sheet grown on a two-dimensional ErOCl thin film material prepared in Example 3 of the present invention.
[0029] Figure 6This is an X-ray diffraction pattern of the two-dimensional ErOCl thin film material prepared in Example 3 of the present invention.
[0030] Figure 7 This is a transmission electron microscope characterization image of the two-dimensional ErOCl thin film material prepared in Example 3 of the present invention.
[0031] Figure 8 This is an elemental composition analysis diagram of the two-dimensional ErOCl thin film material prepared in Example 3 of the present invention.
[0032] Fig. 9 It is a schematic diagram of the structure of the field effect transistor prepared in Example 7 of the present invention.
[0033] Fig.10 This is an optical microscope top view of the field effect transistor prepared in Example 7 of the present invention.
[0034] Fig.11 It is a current-voltage diagram of the output curve of the field effect transistor prepared in Example 7 of the present invention.
[0035] Fig.12 3 is a current-voltage diagram of the transfer curve of the field effect transistor prepared in Example 7 of the present invention.
[0036] Fig.13 It is an optical microscope top view of the two-dimensional ErOCl thin film material prepared in Examples 1, 2, 3, and 4 of the present invention.
[0037] Fig.14 It is an optical microscope top view of the two-dimensional ErOCl thin film material prepared in Examples 2 and 5 of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0039] The present invention provides a simple two-dimensional ErOCl thin film material and a preparation method thereof. The material can be used as an insulating material for field effect transistors and has high stability and is non-toxic and harmless. On the other hand, the present invention provides an application of the two-dimensional ErOCl thin film material in preparing field effect transistors. The specific implementation steps are as follows:
[0040] Step 1: Grind ErCl3·6H2O powder into fine powder, heat it in a muffle furnace to 500-900°C, and keep it at this temperature for 12-24 hours to calcine and obtain ErOCl powder.
[0041] Step 2: The obtained ErOCl powder is mixed with a flux in a preset ratio and placed in a quartz test tube as a precursor. The quartz test tube containing the precursor is placed in the central temperature zone of a horizontal tube furnace, and the substrate is placed near the precursor powder.
[0042] Step 3: Introduce inert gas into a tube furnace, heat the precursor to 500-900°C, maintain the temperature for 5-30 minutes, and then cool naturally to room temperature to obtain a two-dimensional ErOCl thin film material.
[0043] In another aspect, the present invention uses the prepared two-dimensional ErOCl thin film material to prepare a field effect transistor, comprising the following steps:
[0044] Step 1: Take a substrate and transfer the two-dimensional ErOCl thin film material to the surface of the substrate. The substrate can be any one of a doped silicon wafer with an oxide layer, a mica wafer, and a sapphire.
[0045] Step 2: Transfer the mechanically exfoliated multilayer or monolayer MoS2 onto the top of the 2D ErOCl thin film material
[0046] Step 3: Design the electrode pattern using CAD software, and use UV exposure and electron beam exposure to etch the pattern on the multilayer or single layer of molybdenum disulfide;
[0047] Step 4: Prepare metal electrodes by using electron beam deposition. First, evaporate 10-15nm of indium metal, and then evaporate 50-100nm of gold electrode on the indium metal. The indium metal serves as a transition layer to increase the adhesion of the gold electrode.
[0048] Embodiment 1:
[0049] According to the method for preparing two-dimensional ErOCl thin film material provided by the present invention, a horizontal tube furnace is used, 50 mg of ErOCl powder, 50 mg of chloride salt (such as NH4Cl), a mica substrate, a distance between the substrate and the source of 5 mm, a central temperature zone of 600°C, and a holding time of 30 minutes. Before the reaction, pre-vacuum is performed, and then Ar gas is filled to one atmosphere, and a gas flow rate of 700sccm is maintained for 5 minutes of gas washing. During the reaction, 100sccm of Ar gas is introduced and the pressure is maintained at one atmosphere. After the reaction is completed, the carrier gas remains unchanged, and the product is cooled to room temperature with the furnace. The product is collected on a mica substrate to obtain a two-dimensional ErOCl thin film material with a small film size.
[0050] Embodiment 2:
[0051] According to the method for preparing a two-dimensional ErOCl thin film material provided by the present invention, a horizontal tube furnace is used, ErOCl powder 50mg, chloride salt (such as NH4Cl) 50mg, a mica substrate, a distance between the substrate and the source of 5mm, a central temperature zone of 700℃, and a holding time of 30min. Pre-vacuuming is performed before the reaction, and then Ar gas is filled to one atmosphere, and a gas flow rate of 700sccm is maintained for 5min. During the reaction, 100sccm of Ar gas is introduced and the pressure is maintained at one atmosphere. After the reaction is completed, the carrier gas remains unchanged, the product is cooled to room temperature with the furnace, and the mica substrate collects the product to obtain a two-dimensional ErOCl thin film material, and a large piece of uniform film is obtained.
[0052] Embodiment 3:
[0053] According to the method for preparing a two-dimensional ErOCl thin film material provided by the present invention, a horizontal tube furnace is used, ErOCl powder 50mg, chloride salt (such as NH4Cl) 50mg, the substrate is a mica sheet, the distance between the substrate and the source is 5mm, the central temperature zone is 800℃, and the holding time is 30min. Pre-vacuum is first performed before the reaction, and then Ar gas is filled to one atmosphere, and the gas flow rate of 700sccm is maintained for 5min. During the reaction, 100sccm of Ar gas is passed and the pressure is maintained at one atmosphere. After the reaction is completed, the carrier gas remains unchanged, the product is cooled to room temperature with the furnace, and the mica sheet substrate collects the product to obtain a two-dimensional ErOCl thin film material, which almost covers the entire mica sheet.
[0054] Embodiment 4:
[0055] According to the method for preparing a two-dimensional ErOCl thin film material provided by the present invention, a horizontal tube furnace is used, ErOCl powder 50mg, chloride salt (such as NH4Cl) 50mg, the substrate is a mica sheet, the distance between the substrate and the source is 5mm, the central temperature zone is 900℃, and the holding time is 30min. Pre-vacuum is first performed before the reaction, and then Ar gas is filled to one atmosphere, and the gas flow rate of 700sccm is maintained for 5min. During the reaction, 100sccm of Ar gas is passed and the pressure is maintained at one atmosphere. After the reaction is completed, the carrier gas remains unchanged, the product is cooled to room temperature with the furnace, and the mica sheet substrate collects the product to obtain a two-dimensional ErOCl thin film material, which is almost covered with mica sheets, and the film thickness increases and shows unevenness.
[0056] Embodiment 5:
[0057] According to the method for preparing a two-dimensional ErOCl thin film material provided by the present invention, a horizontal tube furnace is used, ErOCl powder 50mg, chloride salt (such as NH4Cl) 50mg, the substrate is a mica sheet, the distance between the substrate and the source is 0mm, the central temperature zone is 700℃, and the holding time is 30min. Pre-vacuum is performed before the reaction, and then Ar gas is filled to one atmosphere, and the gas flow rate of 700sccm is maintained for 5min. During the reaction, 100sccm of Ar gas is passed and the pressure is maintained at one atmosphere. After the reaction is completed, the carrier gas remains unchanged, the product is cooled to room temperature with the furnace, and the mica sheet substrate collects the product to obtain a two-dimensional ErOCl thin film material. Compared with Example 2, the obtained thin film material has a larger size.
[0058] Embodiment 6:
[0059] According to the method for preparing a two-dimensional ErOCl thin film material provided by the present invention, a horizontal tube furnace is used, 30 mg of ErOCl powder, 120 mg of chloride salt, a mica sheet substrate, a distance between the substrate and the source of 5 mm, a central temperature zone of 800 ° C, and a holding time of 15 min. Before the reaction, pre-vacuum is first performed, and then Ar gas is filled to one atmosphere, and a gas flow rate of 700 sccm is maintained for 5 minutes. During the reaction, 60 sccm of Ar gas is passed and the pressure is maintained at one atmosphere. After the reaction is completed, the carrier gas remains unchanged, the product is cooled to room temperature with the furnace, and the mica sheet substrate collects the product to obtain a two-dimensional ErOCl thin film material, which is almost covered with mica sheets.
[0060] Embodiment 7:
[0061] According to the application of a two-dimensional ErOCl thin film material provided by the present invention, FET is prepared, the two-dimensional ErOCl thin film material prepared in Example 1 is transferred to a silicon wafer with an oxide layer, the mechanically peeled multilayer molybdenum disulfide is transferred to the two-dimensional ErOCl thin film material, electrodes are designed, 10nm of indium metal and 50nm of gold are deposited as electrodes by electron beam evaporation, and the current and voltage performance of the FET device is tested using a K4200 source meter.
[0062] Figure 1 It is a schematic diagram of the structure of the two-dimensional ErOCl thin film material prepared in Example 1. The crystal layers of the two-dimensional ErOCl thin film material are connected by van der Waals forces.
[0063] Figure 2 This is an optical microscope top view of the two-dimensional ErOCl thin film material prepared in Example 3. The two-dimensional ErOCl thin film material is composed of regular triangles stacked together.
[0064] Figure 3This is an optical microscope top view of the two-dimensional ErOCl thin film material prepared in Example 3. The two-dimensional ErOCl thin film material is a large-area film with a relatively clean surface.
[0065] Figure 4 This is an atomic force microscope image of the two-dimensional ErOCl thin film material prepared in Example 3 transferred to a silicon wafer with an oxide layer, showing that the thickness of the two-dimensional ErOCl thin film material is about 40 nm.
[0066] Figure 5 This is a picture of a mica sheet grown with the two-dimensional ErOCl thin film material prepared in Example 3. The mica sheet has been ultrasonically cleaned, showing that the two-dimensional ErOCl thin film material basically covers the entire mica sheet, and the prepared film is at the centimeter level.
[0067] Figure 6 This is the X-ray diffraction pattern of the two-dimensional ErOCl thin film material prepared in Example 3. The two-dimensional ErOCl thin film material prepared on mica is transferred to quartz glass by a wet method for X-ray diffraction, and four obvious characteristic peaks appear, corresponding to the (003), (006), (009) and (0012) crystal planes of the two-dimensional ErOCl thin film material.
[0068] Figure 7 This is a transmission electron microscope characterization image of the two-dimensional ErOCl thin film material prepared in Example 3. The lattice fringes can be seen relatively clearly, and after Fourier transformation, it can be seen that it is a hexagonal crystal system, which is consistent with the crystal system of ErOCl in the literature.
[0069] Figure 8 This is the element map of the two-dimensional ErOCl thin film material prepared in Example 3. It can be clearly seen that the three elements Er, O, and Cl are evenly distributed.
[0070] Fig. 9 This is a schematic diagram of the structure of the field effect transistor prepared in Example 7
[0071] Fig.10 This is an optical microscope top view of the field effect transistor prepared in Example 7
[0072] Fig.11 This is the current-voltage diagram of the output curve of the field effect transistor prepared in Example 7. It can be seen that ErOCl has a certain regulation ability and can withstand a voltage of up to 40V without obvious breakdown changes.
[0073] Fig.12 This is a current-voltage diagram of the transfer curve of the field effect transistor prepared in Example 7. It can be seen that the device has a certain switching ratio and a good subthreshold.
[0074] Fig.13This is an optical microscope top view of the two-dimensional ErOCl thin film material prepared in Examples 1, 2, 3, and 4. It can be clearly seen that with the increase of the heating temperature, when other conditions remain unchanged, the higher the temperature, the larger the range of thin film formation. However, the higher the temperature is not necessarily better. Too high a temperature will also cause the film to become thicker.
[0075] Fig.14 This is an optical microscope top view of the two-dimensional ErOCl thin film material prepared in Examples 2 and 5. It can be seen that the closer the distance between the substrate and the source, the larger the film area can be formed, but at the same time the thickness of the thin film material will also increase.
[0076] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a two-dimensional ErOCl thin film material, characterized in that The steps include: ErOCl powder and flux are mixed to obtain a precursor; the precursor is kept warm for 5-30 minutes at a temperature of 500-900° C. in an inert gas atmosphere, and then naturally cooled to room temperature to obtain a two-dimensional ErOCl thin film material.
2. The preparation method according to claim 1, characterized in that: The mass ratio of ErOCl powder to flux is 1:1 to 3:
1.
3. The preparation method according to claim 1, characterized in that: The flux is a chloride salt, selected from one or more of sodium chloride, ammonium chloride and potassium chloride.
4. The preparation method according to claim 1, characterized in that: The thickness of the two-dimensional ErOCl thin film material is 5-400nm, and the area of the film is at the centimeter level.
5. The preparation method according to claim 1, characterized in that: The inert gas is argon, and the flow rate is controlled to be 30-200 sccm.
6. Use of the two-dimensional ErOCl thin film material prepared by any one of the methods of claims 1-5 in the preparation of field effect transistors.
7. The use according to claim 6, characterized in that: The field effect transistor includes, from bottom to top, a substrate, a two-dimensional ErOCl thin film layer, a MoS2 layer, and a counter electrode.
8. The use according to claim 7, characterized in that: The substrate is any one of a doped silicon wafer with an oxide layer, a mica wafer, and a sapphire.
9. The use according to claim 7, characterized in that: The electrode is any one or more of indium gold, silver, tin, and copper electrodes; the thickness of the electrode is 50 to 100 nm.
10. The use according to claim 7, characterized in that: An adhesion layer is also provided between the MoS2 layer and the counter electrode to increase the adhesion of the electrode, and the adhesion layer is indium metal with a thickness of 10-15 nm.
Citation Information
Cited By
Preparation method of two-dimensional single crystal rare earth compound nanosheet
CN119640395A
Preparation Method of Two-Dimensional Single-Crystalline Rare Earth Compound Nanosheets
CN119640395B
Preparation method of two-dimensional TbOCl single crystal material and application of two-dimensional TbOCl single crystal material in field effect transistor
CN121381144A