Preparation method of quartz crucible
By designing quartz sand particle size distribution and silicone mixing at different levels in quartz crucibles, the problem of crystallization layer falling off during high-temperature operation of quartz crucibles is solved, and the uniformity of heat source radiation and service life are improved.
Patent Information
- Application Number
- CN202310515475.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
In the traditional quartz crucible preparation process, due to the uneven particle size of the quartz sand, the crystallization layer is prone to fall off during high temperature operation, which affects the crystal growth rate and service life.
Different levels of quartz sand particle size distribution are used, the inner layer uses 80-120μm uniform quartz sand, the outer layer contains small and large-size quartz sand, and silicone is added, and the arc melting and vacuum treatment is carried out to ensure each The layer of quartz sand is evenly stirred and dense.
It effectively reduces the risk of crystallization layer falling off, ensures the uniformity of heat source radiation, reduces corrosion reactions on the inner and outer surfaces, and extends the service life of the quartz crucible.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of quartz crucible preparation, and in particular, relates to a method for preparing a quartz crucible. Background Art
[0002] In the important method of producing single crystal silicon - CZ, quartz crucible is an important auxiliary material, mainly playing the role of carrying high-temperature silicon melt. Its quality not only affects the crystallization rate of crystal growth, but also affects the service life. Quartz crucibles tend to turn into silicon dioxide crystals (cristobalite) at high temperatures. This process is called recrystallization, also known as "devitrification", and is also commonly called "crystallization". The traditional preparation process is to directly load high-purity quartz sand into the mold. The purity of quartz sand used to make quartz crucibles is 99.9980%. The particle size distribution of quartz sand is generally: 40-460μm, the particle size of quartz sand is uneven, the particle size difference is 11 times, and the surface area difference is 130 times; different particle sizes have different specific surface areas, different adsorption capacities, and different crystallization rates, which will have a greater impact on the crystallization of quartz crucibles. Summary of the invention
[0003] The present application provides a method for preparing a quartz crucible, which particularly solves the technical problem in the prior art that the crystallization layer of the quartz crucible is easily detached due to the impurity gaps between the quartz sand particles during long-term high-temperature operation.
[0004] In order to solve at least one of the above technical problems, the technical solution adopted in this application is:
[0005] A method for preparing a quartz crucible. When preparing the quartz crucible, the particle size distribution of the quartz sand used in the inner layer of the quartz crucible is different from that of the quartz sand used in the outer layer thereof; quartz sand with a cross-distributed and uniform particle size in the range of 80-120 μm is selected from the materials required for preparing the inner layer of the quartz crucible.
[0006] Furthermore, the quartz sand used in the inner layer of the quartz crucible has a uniform particle size distribution, and its particle size range is smaller than the particle size range of part of the quartz sand used in the outer layer of the quartz crucible.
[0007] Furthermore, the components used for the outer layer of the quartz crucible include small-size quartz sand and large-size quartz sand, wherein the amount of the small-size quartz sand is less than the amount of the large-size quartz sand.
[0008] Furthermore, the components used for the outer layer of the quartz crucible also include organic silicon, wherein the mass ratio of organic silicon, small-particle quartz sand and large-particle quartz sand is 0.5-1:1-1.5:10-12.
[0009] Furthermore, the mass ratio of silicone, small-particle quartz sand and large-particle quartz sand is 0.8:1:11.
[0010] Furthermore, the particle size range of the small-size quartz sand is 40-120 μm; the particle size range of the large-size quartz sand is 120-400 μm.
[0011] Furthermore, when preparing the quartz sand used for the outer layer of the quartz crucible, all the materials of the components are first prepared based on the configuration mass ratio, and then the silicone, small-particle quartz sand and large-particle quartz sand are placed together in a sand mixing device for mixing and stirring.
[0012] Furthermore, the mixing and stirring time is 4-12 hours.
[0013] Furthermore, during melting, the outer layer and the inner layer of the quartz crucible are laid in the mold of the quartz crucible from the outside to the inside based on the thickness of the quartz crucible; then the quartz sand after laying is arc-melted and vacuumed simultaneously, and the direction of vacuuming is from the inside to the outside along the thickness of the quartz crucible.
[0014] Furthermore, the vacuum value during vacuuming is -0.085MP to -0.09MP, and the pumping speed is 300-600L / s.
[0015] A preparation method for a quartz crucible designed by the present application is adopted, different quartz sand particle sizes are designed based on the positions of different layers, and the quartz sands of different particle sizes are mixed evenly by adjusting their configuration ratio and stirring steps, and then the quartz crucible is prepared; the technical problem that the crystallization layer of the quartz crucible is easy to fall off due to the impurity gap between the quartz sand particle sizes during long-term high-temperature operation of the quartz crucible is solved, and the heat source radiation of the quartz crucible is ensured to be uniform during crystal pulling, the probability of corrosion reaction on the inner and outer surfaces of the quartz crucible is reduced, the thickness of the crystallization layer in the outer layer is effectively reduced, and the service life of the quartz crucible is increased. DETAILED DESCRIPTION
[0016] The present application is described in detail below with reference to specific embodiments.
[0017] This embodiment provides a method for preparing a quartz crucible. When preparing the quartz crucible, the particle size of the quartz sand used to prepare the inner layer of the quartz crucible is different from the particle size of the quartz sand used to prepare the outer layer of the quartz crucible, and at least two quartz sands with different particle sizes are included in the materials required for preparing the inner layer of the quartz crucible. At the same time, quartz sands with cross-distributed and uniform particle sizes in the range of 80-120 μm are selected from the materials required for preparing the inner layer of the quartz crucible. The quartz sand required for the outer layer of the quartz crucible includes two different particle sizes, the purpose of which is to reduce the gap between the quartz sand particles on the outer wall of the quartz crucible, so as to reduce the content of gas impurities in the outer wall of the quartz crucible, thereby improving the purity of the quartz crucible.
[0018] Specifically, the quartz sand used to prepare the inner layer of the quartz crucible has a consistent particle size distribution, and the purity is 99.9999% quartz sand, and the particle size range is 80-120 μm. Since the quartz sand used in the inner layer of the quartz crucible is in direct contact with the silicon material used to pull the single crystal, it is required to have density and high purity.
[0019] Furthermore, the particle size of the quartz sand used to prepare the inner layer of the quartz crucible is smaller than the particle size range of part of the quartz sand used to prepare the outer layer of the quartz crucible, that is, the particle size range of the quartz sand used to prepare the inner layer of the quartz crucible is between the particle size range of the quartz sand used to prepare the outer layer of the quartz crucible. Considering the production cost and based on the contact degree between the outer layer and the silicon material used for crystal pulling, the particle size distribution of the quartz sand used to prepare the outer layer of the quartz crucible is generally more dispersed, while the particle size of the quartz sand used for the inner layer is more concentrated. Because when preparing the outer layer of the quartz crucible, the particle size distribution of the quartz sand particles is too dispersed, which will lead to larger gaps between the particles, and gas impurities are easily introduced, which will affect the purity of the quartz crucible. When preparing the outer layer of the quartz crucible, while using quartz sand with large particle size for preparing the outer layer of the quartz crucible, quartz sand particles smaller than the quartz sand particles used for the inner layer are cross-mixed to fill the gaps between the larger quartz sand particles with smaller particles, thereby reducing the air rate in the gaps between the main quartz sand particles used in the preparation of the outer layer, and reducing the air impurities entering the gaps, thereby improving the overall strength and purity of the outer layer of the quartz crucible, and further reducing the probability of crystallization.
[0020] The quartz sand components used to prepare the outer layer of the quartz crucible include small-grained quartz sand and large-grained quartz sand, wherein the amount of small-grained quartz sand is less than that of large-grained quartz sand. This is because when preparing the outer layer of the quartz crucible, large-grained quartz sand is the main component, and small-grained quartz sand is used as auxiliary quartz sand to fill the gaps between large-grained quartz sands to improve the density between adjacent large-grained quartz sands, thereby reducing air impurities in the gaps between large-grained quartz sands.
[0021] Furthermore, since both large-particle quartz sand and small-particle quartz sand are granular dry particles, organic matter is also required for bonding and mixing when preparing the outer layer of the quartz crucible so that the large-particle quartz sand and the small-particle quartz sand can be fully mixed and bonded together. Furthermore, the components used to prepare the outer layer of the quartz crucible also include silicone, wherein the mass ratio of silicone, small-particle quartz sand and large-particle quartz sand is 0.5-1:1-1.5:10-12. That is, among the materials used to prepare the outer layer of the quartz crucible, silicone has the smallest mass proportion, large-particle quartz sand has the largest mass proportion, and small-particle quartz sand has a mass proportion between silicone and large-particle quartz sand; moreover, the total mass proportion of silicone and small-particle quartz sand is also much smaller than the mass proportion of large-particle quartz sand.
[0022] Preferably, the mass ratio of silicone, small-particle quartz sand and large-particle quartz sand is 0.8:1:11. When configured in this ratio, a quartz crucible with uniform density and high purity can be manufactured, and crystallization of the quartz crucible can be suppressed to the greatest extent.
[0023] Specifically, the quartz sand required for preparing the outer layer of the quartz crucible has a particle size range of 40-120 μm for small-particle quartz sand and a particle size range of 120-400 μm for large-particle quartz sand. The particle size range used for the inner layer of the quartz crucible is 80-120 μm, which is between large-particle quartz sand and small-particle quartz sand, and is more inclined to small-particle quartz sand.
[0024] When preparing the quartz sand for the outer layer of the quartz crucible, it is necessary to first select the configuration material based on the configuration mass ratio requirements, and separate the quartz sand through sieves of different particle size ranges in advance to sort out the quartz sand particles of the desired particle size range.
[0025] Mix and prepare the materials used for the outer layer of the quartz crucible, place the organic silicon, small-sized quartz sand and large-sized quartz sand in the sand mixing equipment for mixing and stirring, and the mixing and stirring time is 4-12 hours. Since the quartz sand particles are granular materials, they do not adhere to each other, and the small-sized quartz sand and the large-sized quartz sand can be organically bonded by organic silicon. All particles are added to the mixing container for stirring and mixing, so that all quartz sand can be fully mixed, so that all small-sized quartz sand can be completely filled in the gaps between the large-sized quartz sand.
[0026] Further, after the mixing is completed, melting begins. First, the outer layer and the inner layer of the quartz crucible are laid in the mold of the quartz crucible from the outside to the inside based on the thickness of the quartz crucible, that is, a mixture of large-grained quartz sand and small-grained quartz sand is laid first, and the size and shape of the quartz crucible mold are given for spraying to complete the laying of the outer quartz crucible; then the inner layer of quartz sand with a particle size range of 80-120μm is sprayed to complete the laying of the inner quartz crucible.
[0027] After the material is laid, the quartz sand behind the material is arc-melted and vacuumed simultaneously. The direction of vacuuming is from the inside to the outside along the thickness of the quartz crucible to ensure the vacuum degree of the inner layer of the quartz crucible. Since small-particle quartz sand is added to the outer layer material, the gap space in the material in the outer layer is small, so it is necessary to extend the vacuuming time to ensure the purity of the quartz crucible. Preferably, the vacuum value during vacuuming is -0.085MP to -0.09MP, the pumping speed is 300-600L / s, and the vacuuming time is 1.5-2 times the normal vacuuming time of the existing same type and size.
[0028] The quartz crucible prepared by this method reduces the surface area difference between the outer layer and the inner layer of the quartz crucible, and the volume and number of bubbles in the outer layer become smaller, so that the thickness of the outer layer is denser, which can effectively reduce the thickness of the outer crystallization layer and thus increase the operating time.
[0029] During the crystal pulling process, the reaction rate will be reduced to 1-2 times of the original rate for every 10℃ increase in temperature. It can also alleviate the technical problem of uneven heating of the quartz crucible due to high temperature, minimize the impact of the thermal field temperature during crystal pulling, ensure the relative stability of the thermal field temperature, and alleviate the crystallization problem of the quartz crucible.
[0030] It can not only solve the technical problem of the crystallization layer falling off due to the long-term high-temperature operation of the quartz crucible, but also ensure that the technical problem of uneven heat source radiation caused by the thickening of the crystallization layer during the crystal pulling operation of the quartz crucible is solved. At the same time, it can also reduce the probability of corrosion reaction on the inner and outer surfaces of the quartz crucible due to long-term crystal pulling operation, delay the time for the crystallization layer to form after the reaction between the two, and increase the service life of the quartz crucible.
[0031] The quartz crucible prepared by the preparation method of the present application and the quartz crucible prepared by the prior art, that is, the outer layer of the quartz crucible prepared by the conventional quartz sand with a particle size range of 40-460 μm, for quartz crucibles of different diameters, respectively, 28-inch quartz crucible, 30-inch quartz crucible, 32-inch quartz crucible and 36-inch quartz crucible, respectively, the comparison of their service time results is shown in Table 1. It can be seen from Table 1 that for quartz crucibles of the same size, when other conditions remain unchanged, the service life of the quartz crucible obtained by the preparation method of the present application is longer than that of the quartz crucible prepared by the prior art.
[0032] Table 1 Comparison of service life of quartz crucibles prepared by the preparation method of the present application and by the prior art
[0033]
[0034] A preparation method for a quartz crucible designed by the present application is adopted, different quartz sand particle sizes are designed based on the positions of different layers, and the quartz sands of different particle sizes are mixed evenly by adjusting their configuration ratio and stirring steps, and then the quartz crucible is prepared; the technical problem that the crystallization layer of the quartz crucible is easy to fall off due to the impurity gap between the quartz sand particle sizes during long-term high-temperature operation of the quartz crucible is solved, and the heat source radiation of the quartz crucible is ensured to be uniform during crystal pulling, the probability of corrosion reaction on the inner and outer surfaces of the quartz crucible is reduced, the thickness of the crystallization layer in the outer layer is effectively reduced, and the service life of the quartz crucible is increased.
[0035] The above detailed description of the embodiments of the present application is only a preferred embodiment of the present application and cannot be considered to limit the scope of implementation of the present application. All equivalent changes and improvements made within the scope of the present application should still fall within the scope of the patent coverage of the present application.
Claims
1. A method for preparing a quartz crucible, characterized in that: When preparing the quartz crucible, the particle size distribution of the quartz sand used in the inner layer of the quartz crucible is different from that of the quartz sand used in the outer layer; quartz sand with a cross-distributed and uniform particle size in the range of 80-120 μm is selected from the materials required for preparing the inner layer of the quartz crucible.
2. The method for preparing a quartz crucible according to claim 1, characterized in that: The quartz sand used in the inner layer of the quartz crucible has a uniform particle size distribution, and its particle size range is smaller than that of part of the quartz sand used in the outer layer of the quartz crucible.
3. The method for preparing a quartz crucible according to claim 1 or 2, characterized in that: The components used for the outer layer of the quartz crucible include small-grained quartz sand and large-grained quartz sand, wherein the amount of the small-grained quartz sand is less than the amount of the large-grained quartz sand.
4. The method for preparing a quartz crucible according to claim 3, characterized in that: The components used for the outer layer of the quartz crucible also include organic silicon, wherein the mass ratio of organic silicon, small-grained quartz sand and large-grained quartz sand is 0.5-1:1-1.5:10-12.
5. The method for preparing a quartz crucible according to claim 4, characterized in that: The mass ratio of silicone, small-particle quartz sand and large-particle quartz sand is 0.8:1:
11.
6. The method for preparing a quartz crucible according to claim 4 or 5, characterized in that: The particle size range of small-size quartz sand is 40-120μm; the particle size range of large-size quartz sand is 120-400μm.
7. The method for preparing a quartz crucible according to claim 6, characterized in that: When preparing the quartz sand used for the outer layer of the quartz crucible, firstly prepare all the materials of the components based on the configuration mass ratio, and then place the silicone, small-particle quartz sand and large-particle quartz sand together in a sand mixing device for mixing and stirring.
8. The method for preparing a quartz crucible according to claim 7, characterized in that: The mixing time is 4-12h.
9. A method for preparing a quartz crucible according to any one of claims 1-2, 4-5, 7-8, characterized in that: During melting, the outer layer and the inner layer of the quartz crucible are laid in the mold of the quartz crucible from the outside to the inside based on the thickness of the quartz crucible; then the quartz sand after laying is arc-melted and vacuumed simultaneously, and the direction of vacuuming is from the inside to the outside along the thickness of the quartz crucible.
10. The method for preparing a quartz crucible according to claim 9, characterized in that: The vacuum value during vacuuming is -0.085MP to -0.09MP, and the pumping speed is 300-600L / s.
Citation Information
Patent Citations
Preparation method of high performance fused silica crucible for polycrystalline silicon ingot casting
CN110922175A
Quartz glass crucible and method for the production thereof
CN1662680A
Silica glass crucible and method for manufacturing the same
TW201109484A
Method of producing a quartz glass crucible
US20090320521A1
Quartz Glass Crucible for Pulling Silicon Single Crystal and Method of Manufacturing Quartz Glass Crucible for Pulling Silicon Single Crystal
US20100139549A1