Fiber material with antibacterial function and preparation method thereof
By mixing raw materials such as titanium source under high temperature and high pressure to form nano-flower-like TiO2, antibacterial fiber materials can be directly prepared, which solves the problem of complicated preparation process in the existing technology and realizes the preparation of fiber materials with strong antibacterial properties, good air permeability and low cost.
Patent Information
- Application Number
- CN202411224059.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The existing antibacterial materials are complicated to prepare, time-consuming and labor-intensive, and the textile materials themselves do not have bactericidal and antiviral properties.
Titanium source, alkyl alcohol solvent, chemical reactants, co-solvent and polymer particles are mixed and reacted under high temperature and high pressure to form nano-flower-like TiO2, which directly prepares antibacterial fiber materials. This combines multiple steps into one, realizing in-situ synthesis of antibacterial agents and polymer dissolution.
The prepared fiber material has strong antibacterial and long-lasting effects, good breathability, and is suitable for protective clothing and masks. It can effectively inhibit bacteria and viruses, simplify the production process, and reduce costs.
Smart Images

Figure CN118932522A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of antibacterial materials, and in particular to a fiber material with antibacterial function and a preparation method thereof. Background Art
[0002] In the field of antibacterial materials, protective materials such as masks and protective clothing intercept carriers containing bacteria or viruses outside the body through physical isolation to avoid physical damage caused by subsequent infection. Protective equipment is currently mainly made of microfiber textile materials, which do not have bactericidal and antiviral properties. Combining antibacterial agents with protective materials is the key to realizing the transformation of protective materials from physical protection to active antibacterial and bactericidal protection. The metal oxide titanium dioxide has the characteristics of stability, low cost, strong heat resistance and semiconductor properties. Under solar radiation, photoelectrons with energy greater than the band gap are captured, generating redox photogenerated electrons and hole pairs, which migrate to the surface of the metal oxide and undergo oxidation or reduction reactions with external water molecules or oxygen to generate active substances, which further react with the bacterial cell wall to kill the bacteria.
[0003] The conventional idea and method for combining antimicrobial agents with textile materials is to first prepare the antimicrobial agents, and then prepare them into antimicrobial nonwoven materials through physical blending, surface coating or plasma treatment, or after textile processing. The preparation process is divided into multiple discontinuous steps, which is time-consuming, labor-intensive, and occupies multiple sets of equipment. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a fiber material with antibacterial function and a preparation method thereof. The present invention combines multiple steps into one, greatly saving production and labor costs, and the prepared fiber material has the advantages of strong antibacterial properties and long-lasting antibacterial properties.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a fiber material with antibacterial function, comprising the following steps:
[0007] A titanium source, an alkyl alcohol solvent, a chemical reactant, a cosolvent and polymer particles are mixed, and the resulting mixture is heated to 170-200° C. and reacted for 5-10 hours under a closed and first stirring condition, wherein the titanium source and the alkyl alcohol solvent form a titanium alcohol complex, which is then dehydrated to form TiO2 under the action of the chemical reactant; the chemical reactant includes at least one of N,N-dimethylformamide and N,N-dimethylacetamide;
[0008] The obtained reaction system is pressurized to 7-15 MPa, and the stirring rate is increased. The second stirring is performed for 1-1.5 hours. The polymer particles become fluid and impact TiO2 together with the alkyl alcohol solvent to form nanoflower-like TiO2 to obtain a spinning solution. The spinning solution is then ejected through the spinneret hole after releasing the pressure. The solvent evaporates to form polymer fibers, thereby obtaining a fiber material with antibacterial function.
[0009] Preferably, the titanium source is one or more of tetrabutyl titanate, titanium tetrachloride and titanium sulfate.
[0010] Preferably, the alkyl alcohol solvent has no more than 5 carbon atoms.
[0011] Preferably, the polymer particles include one or more of polyethylene particles, polypropylene particles, polyester particles and polyamide particles.
[0012] Preferably, the co-solvent includes at least one of ethylene dichloride and methylene dichloride.
[0013] Preferably, based on 100% of the raw material mass, the titanium source accounts for 5-8%, the chemical reactant accounts for 25-35%, the alkyl alcohol solvent accounts for 30-37%, the cosolvent accounts for 10-15%, and the polymer particles account for 5-30%.
[0014] Preferably, the first stirring rate is 20-40 r / min; the second stirring rate is 100-200 r / min.
[0015] Preferably, the gas used for pressurization is one or more of argon, nitrogen and carbon dioxide.
[0016] Preferably, after the polymer fibers are formed, the process further comprises air-opening the polymer fibers and collecting the opened fibers with a conveyor belt.
[0017] The present invention provides a fiber material with antibacterial function prepared by the preparation method described in the above scheme, which is composed of polymer fibers, and nano-flower-shaped TiO2 is distributed on the surface of the polymer fibers.
[0018] The invention provides a method for preparing a fiber material with antibacterial function, comprising the following steps: mixing a titanium source, an alkyl alcohol solvent, a chemical reactant, a cosolvent and polymer particles, heating the obtained mixture to 170-200°C for reaction for 5-10 hours under a closed and first stirring condition, wherein the titanium source and the alkyl alcohol solvent form a titanium alcohol complex, and then dehydrate to form TiO2 under the action of the chemical reactant; the chemical reactant comprises at least one of N,N-dimethylformamide and N,N-dimethylacetamide; pressurizing the obtained reaction system to 7-15MPa, increasing the stirring rate, and performing a second stirring for 1-1.5 hours, wherein the polymer particles become a fluid state, and impact TiO2 together with the alkyl alcohol solvent to form nano-flower-shaped TiO2, thereby obtaining a spinning solution, and then releasing the pressure through a spinneret to eject the spinning solution, wherein the solvent evaporates to form polymer fibers, thereby obtaining a fiber material with antibacterial function.
[0019] The present invention mixes various raw materials and heats them to 170-200°C. The titanium source is evenly dispersed in the solvent to form a titanium alcohol complex with the solvent. Then, under the action of a chemical reactant, a dehydration reaction occurs to generate TiO2. Under a critical state, the polymer particles become fluid. Due to the viscosity difference with the solvent, titanium dioxide is repeatedly and irregularly impacted by the solvent and the polymer fluid, forming flow marks on the surface of the TiO2 particles, which are similar to the surface of shellfish in a tidal area (sand and seawater are washed together). At the same time, it is ensured that there will be no serious collision with other titanium dioxide particles, and its morphology is finally manifested as a nano-flower shape.
[0020] The present invention combines multiple processes such as antimicrobial agent synthesis, polymer dissolution, and uniform dispersion of the antimicrobial agent in the polymer into one in the entire preparation process, which can be completed in the same reactor. The same solvent is used to cleverly realize in-situ preparation of the antimicrobial agent and polymer dissolution, which has the advantages of saving time and labor.
[0021] The antibacterial agent titanium dioxide loaded on the fiber material prepared by the present invention has a nano-flower morphology and has the characteristics of a large specific surface area. First, it can fully contact and absorb natural light to produce active oxygen (hydroxyl free radicals, superoxide free radicals and photogenerated holes) substances to destroy the activity of bacteria, thereby inhibiting bacteria and killing bacteria; second, the irregular surface shape makes it easy for the antibacterial agent to be embedded in the polymer surface, has a strong interface bonding force with the polymer, and is not easy to fall off, thereby achieving a long-lasting antibacterial effect of the fiber material.
[0022] The fiber material prepared by the present invention can be in the form of individual fibers, or in the form of nonwoven materials after fiber opening and collection.
[0023] After the polymer fibers are formed, the present invention further opens the fibers by air flow, and the spinning solution is subjected to tension to form microfibers, so that the obtained nonwoven material has good air permeability while maintaining good antibacterial properties, and is comfortable to wear. The protective clothing prepared with the nonwoven material can be used for a long time in the prevention of hospital bacterial infections, special medical accident treatment and other scenarios.
[0024] The fiber material of the present invention has a short preparation process, a simple preparation method, is easy to implement, has strong applicability, can be quickly and mass-produced, and can be used as a raw material for protective clothing, masks or other protective devices to cope with sudden health and safety accidents.
[0025] The results of the examples show that the nonwoven material prepared by the present invention has an air permeability of 200-400 mm / s, a longitudinal breaking strength of >200 N, and a transverse breaking strength of >150 N. It has excellent antibacterial effect, and the antibacterial rates against Escherichia coli, Staphylococcus aureus and Helicobacter pylori are all greater than 99.8%; the antiviral activity rate against RNA virus H1N1 reaches 98.24%. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the device used for preparing the antibacterial nonwoven material in the embodiments and comparative examples of the present invention, wherein 1 is a stirring device, 2 is a feeding hole, 3 is a stirring device, 4 is a spinneret hole, 5 is an air fiber opening device, 6 is a collecting device, and 7 is a nonwoven material;
[0027] Figure 2 is a morphology diagram of the nonwoven material of Example 1, wherein a is the surface morphology of the nonwoven material, and b is the microfiber morphology;
[0028] Figure 3 The morphology of the antimicrobial agent in Example 2, wherein a is the aggregation state of the antimicrobial agent and b is the surface morphology of the antimicrobial agent;
[0029] Figure 4 The morphology of the antibacterial nonwoven material of Example 2, wherein a is the surface morphology of the antibacterial nonwoven material, the embedded image is the enlarged image of the area, and b is the microfiber morphology;
[0030] Figure 5 The mechanical properties of the nonwoven materials of Examples 1 to 2 and Comparative Example 1, a is Example 1, b is Example 2, and c is Comparative Example 1;
[0031] Figure 6 The electron paramagnetic resonance spectra of the nonwoven material in comparative example 1 and the antibacterial nonwoven material in example 2 under light irradiation, the spin trapping agents are ·OH(a), h + (b) and O2 - (c);
[0032] Figure 7This is the antibacterial performance diagram of the antibacterial nonwoven material of Example 2, wherein a is a blank control sample, and b to d are diagrams showing the inhibition effect on Escherichia coli colonies at different concentrations. Specifically, b is 0.075 mg / mL, c is 0.1 mg / mL, d is 0.125 mg / mL, e is 0.15 mg / mL, and f is 0.175 mg / mL. DETAILED DESCRIPTION
[0033] The present invention provides a method for preparing a fiber material with antibacterial function, comprising the following steps:
[0034] A titanium source, an alkyl alcohol solvent, a chemical reactant, a cosolvent and polymer particles are mixed, and the resulting mixture is heated to 170-200° C. and reacted for 5-10 hours under a closed and first stirring condition, wherein the titanium source and the alkyl alcohol solvent form a titanium alcohol complex, which is then dehydrated to form TiO2 under the action of the chemical reactant; the chemical reactant includes at least one of N,N-dimethylformamide and N,N-dimethylacetamide;
[0035] The obtained reaction system is pressurized to 7-15 MPa, and the stirring rate is increased. The second stirring is performed for 1-1.5 hours. The polymer particles become fluid and impact TiO2 together with the alkyl alcohol solvent to form nanoflower-like TiO2 to obtain a spinning solution. The spinning solution is then ejected through the spinneret hole after releasing the pressure. The solvent evaporates to form polymer fibers, thereby obtaining a fiber material with antibacterial function.
[0036] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0037] The present invention mixes a titanium source, an alkyl alcohol solvent, a chemical reactant, a co-solvent and polymer particles.
[0038] In the present invention, the titanium source is preferably one or more of tetrabutyl titanate, titanium tetrachloride and titanium sulfate; the number of carbon atoms of the alkyl alcohol solvent is preferably not more than 5, and is more preferably isopropanol, ethylene glycol, n-propanol or a mixture thereof; in the present invention, the alkyl alcohol solvent has two functions: one is to form a titanium alcohol complex with the titanium source, and the other is to reduce the interfacial tension of the polymer in the solvent under high temperature and high pressure.
[0039] In the present invention, the chemical reactant includes at least one of N,N-dimethylformamide and N,N-dimethylacetamide; the cosolvent preferably includes at least one of dichloroethane and dichloromethane; the cosolvent functions to increase the cloud point pressure of the spinning solution. In the present invention, the polymer particles preferably include one or more of polyethylene particles, polypropylene particles, polyester particles and polyamide particles; the polymer viscosity is preferably 1000-45000 mPa·s (using GB / T1632.1-2008 to test the viscosity of the polymer dilute solution, normal pressure 25°C, using a capillary viscometer).
[0040] In the present invention, based on 100% raw material mass, the titanium source is preferably 5-8%, more preferably 6-7%; the chemical reactant is preferably 25-35%, more preferably 28-32%; the alkyl alcohol solvent is preferably 30-37%, more preferably 32-35%; the co-solvent is preferably 10-15%, more preferably 12-14%; the polymer particles are preferably 5-30%, more preferably 10-25%, and further preferably 15-20%.
[0041] In the present invention, the polymer particles are preferably dried first and then mixed. The present invention has no special requirements on the drying temperature, and any drying temperature known in the art can be used. In the embodiment of the present invention, it is 60°C.
[0042] In the present invention, the mixing preferably includes: firstly adding the titanium source, the alkyl alcohol solvent, the chemical reactants and the co-solvent into a reaction kettle, stirring evenly, and then adding the polymer particles.
[0043] After the mixing is completed, the present invention heats the obtained mixture to 170-200° C., preferably 180-190° C., under closed and first stirring conditions, and reacts for 5-10 hours, preferably 6-8 hours.
[0044] In the present invention, the first stirring rate is preferably 20-40 r / min. In the reaction process of the present invention, the titanium source and the alkyl alcohol solvent form a titanium alcohol complex, which is then dehydrated to form TiO2 under the action of chemical reactants, and the polymer is partially dissolved.
[0045] After the reaction is completed, the present invention pressurizes the obtained reaction system to 7-15MPa, increases the stirring rate, and stirs for a second time for 1-1.5h, the polymer particles become fluid, and impact TiO2 with the alkyl alcohol solvent to form nano-flower-shaped TiO2, to obtain a spinning solution, and then releases the pressure through the spinneret to spray the spinning solution, the solvent evaporates, and polymer fibers are formed, and a fiber material with antibacterial function is obtained. In the critical state, there is a viscosity difference between the polymer and the solvent, and then under the impact of the fluid, flow marks are formed on the surface of the TiO2 particles, and its morphology finally appears as a nano-flower-shaped
[0046] In the present invention, the gas used for pressurization is preferably one or more of argon, nitrogen and carbon dioxide; the pressure is increased to 7-15MPa, preferably 9-13MPa; the second stirring rate is preferably 100-200r / min, more preferably 120-180r / min.
[0047] The present invention promotes the polymer to become a fluid state through high temperature and high pressure. Due to the viscosity difference with the solvent, titanium dioxide is repeatedly subjected to irregular impacts of the solvent and the polymer fluid, forming flow marks on the surface of TiO2 particles, similar to the surface of shellfish in a tidal area (sand and seawater are washed together), and its morphology finally appears as a nanoflower. After the second stirring is completed, a spinning solution is obtained.
[0048] The present invention releases the pressure instantaneously to eject the spinning solution. In the present invention, the diameter of the spinneret hole is preferably 10 to 50 cm.
[0049] After the polymer fibers are formed, the present invention preferably further comprises air-opening the polymer fibers, collecting the opened fibers with a conveyor belt, and obtaining a fiber material with antibacterial function. In this case, the fiber material is an antibacterial nonwoven material.
[0050] In the present invention, the speed of the fiber opening is preferably 20 to 200 m / s, more preferably 50 to 150 m / s. In the present invention, the spinning solution is subjected to tension to form fine fibers through airflow fiber opening, so that the obtained nonwoven material has good air permeability while maintaining good antibacterial properties. In the present invention, the diameter of the polymer fiber after airflow fiber opening is preferably 0.5 to 2 μm.
[0051] The present invention provides a fiber material with antibacterial function prepared by the preparation method described in the above scheme, which is composed of polymer fibers, and nano-flower-shaped TiO2 is distributed on the surface of the polymer fibers.
[0052] Nanoflower-like TiO2 has the characteristics of large specific surface area. First, it can fully contact and absorb natural light to produce active oxygen (hydroxyl radicals, superoxide radicals and photogenerated holes) substances, destroying the activity of bacteria, thereby inhibiting bacteria and killing bacteria; second, the irregular surface shape makes it easy for the antibacterial agent to be embedded in the polymer surface, has a strong interfacial bonding force with the polymer, and is not easy to fall off, thereby achieving a long-lasting antibacterial effect of the fiber material.
[0053] In the present invention, when the fiber material is an antibacterial nonwoven material, the antibacterial nonwoven material is composed of polymer fibers, the diameter of the polymer fibers is preferably 0.5-2 μm, the polymer fibers are densely arranged, the longitudinal breaking strength is greater than 200N, the transverse breaking strength is greater than 150N, and the air permeability is 200-400mm / s.
[0054] The fiber material with antibacterial function and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0055] Example 1
[0056] Use Figure 1 The antibacterial non-woven material was prepared by an experimental device. The reactor capacity was 10L, tetrabutyl titanate was used as the titanium source, N,N-dimethylformamide was used as the chemical reactant, isopropanol was used as the solvent, dichloroethane was used as the co-solvent, polyethylene particles were used as the polymer particles, and nitrogen was used as the protective gas.
[0057] 1500g polyethylene particles were dried in an oven at 60°C, and 250g tetrabutyl titanate, 1250g N,N-dimethylformamide, 1500g isopropanol and 500g ethylene dichloride were added to the reactor through the reactor feed port in turn, and mechanically stirred for 5min at a stirring speed of 20r / min. The dried polymer particles were added to the reactor, heated to 180°C, and stirred for 8h. Carbon dioxide gas was injected into the reactor, the pressure in the reactor was increased to 7MPa, and the stirring speed was slowly increased to 100r / min. After stirring for 1h, the pressure was released, the solvent in the polymer solution evaporated, and a microfiber bundle was formed. The fiber was opened by air flow through an air fiber opening device, and the opening air flow speed was 150m / s. Finally, the antibacterial nonwoven material was collected by a conveyor belt.
[0058] Through testing and analysis, the average fiber diameter is 1.2μm, the fiber transverse breaking strength is 160N, the longitudinal breaking strength is 209N, and the air permeability is 291mm / s (refer to the national standard GB / T15453-1997, analyzed using a differential pressure flowmeter, the same below). When the concentration of the non-woven material is 0.15mg / mL, the antibacterial rate against Escherichia coli is 99.8%, and the antiviral activity rate against RNA virus H1N1 reaches 98.35%.
[0059] Figure 2 The morphology of the nonwoven material of Example 1, wherein a is the surface morphology of the nonwoven material, and b is the microfiber morphology. Figure 2 It can be seen that nonwoven materials are composed of polymer microfibers with a diameter of 0.5 to 2 μm. The fibers are stacked on each other, leaving pores and have good air permeability.
[0060] Example 2
[0061] Use Figure 1The antibacterial non-woven material was prepared by an experimental device. The reactor capacity was 10L, tetrabutyl titanate was used as the titanium source, N,N-dimethylformamide was used as the chemical reactant, ethylene glycol was used as the solvent, chloroform was used as the cosolvent, polyester particles were used as the polymer particles, and argon was used as the protective gas.
[0062] 1500g polyester particles were dried in an oven at 80°C, and 250g tetrabutyl titanate, 1250g N,N-dimethylformamide, 1500g ethylenedipropylene glycol and 500g chloroform were added to the reactor through the reactor feed port in sequence, and mechanically stirred for 5min at a stirring speed of 20r / min. The dried polymer particles were added to the reactor, heated to 180°C, and stirred for 8h. Argon was injected into the reactor, the pressure in the reactor was increased to 8MPa, and the stirring speed was slowly increased to 100r / min. After stirring for 1h, the pressure was released, the solvent in the polymer solution evaporated, and a microfiber bundle was formed. The fiber was opened by air flow through an air fiber opening device, and the opening air flow speed was 200m / s. Finally, the antibacterial nonwoven material was collected by a conveyor belt.
[0063] Through testing and analysis, the average fiber diameter is 1.0μm, the fiber transverse breaking strength is 163N, the longitudinal breaking strength is 211N, the air permeability is 298mm / s, and the antibacterial rate against Escherichia coli is 99.8% when the concentration of the non-woven material is 0.15mg / mL, and the antiviral activity rate against RNA virus H1N1 reaches 98.57%.
[0064] Figure 3 is the morphology of the antibacterial agent in Example 2, wherein a is the aggregation state of the antibacterial agent and b is the surface morphology of the antibacterial agent. Figure 3 It can be seen that the antibacterial agent particles are uniform in size, at the micro-nano level, and the surface is similar to the shape of petals.
[0065] Figure 4 The morphology of the antibacterial nonwoven material of Example 2, wherein a is the surface morphology of the antibacterial nonwoven material, the embedded image is the enlarged image of the region, and b is the microfiber morphology. Figure 4 It can be seen that the antimicrobial agent is evenly dispersed on the nonwoven material and the fiber surface, and the surface petal-like morphology is embedded on the fiber surface, which improves the antimicrobial durability of the fiber.
[0066] Figure 7 The antibacterial performance diagram of the antibacterial nonwoven material of Example 2 was tested by the oscillation method, where a is a blank control sample, and b to d are the inhibition effects of different nonwoven material concentrations on Escherichia coli colonies. Specifically, b is 0.075 mg / mL, c is 0.1 mg / mL, d is 0.125 mg / mL, e is 0.15 mg / mL, and f is 0.175 mg / mL. Figure 7 It can be seen that the antibacterial nonwoven material of Example 2 exhibits a good antibacterial effect on Escherichia coli.
[0067] Comparative Example 1
[0068] Use Figure 1 The antibacterial non-woven material was prepared by an experimental device. The reactor capacity was 10L, N,N-dimethylformamide was used as the chemical reactant, isopropanol was used as the solvent, dichloroethane was used as the co-solvent, polyethylene particles were used as the polymer particles, and nitrogen was used as the protective gas.
[0069] 1500g polyethylene particles were dried in an oven at 60°C, and 1250g N,N-dimethylformamide, 1500g isopropanol and 500g ethylene dichloride were added to the reactor through the reactor feed port in turn, and mechanically stirred for 5 minutes at a stirring speed of 20r / min. The dried polymer particles were added to the reactor, heated to 180°C, and stirred for 8 hours. Nitrogen was injected into the reactor, the pressure in the reactor was increased to 15MPa, and the stirring speed was slowly increased to 100r / min. After stirring for 1 hour, the pressure was released, the solvent in the polymer solution evaporated, and a microfiber bundle was formed. The fiber was opened by air flow through an air fiber opening device, and the opening air flow speed was 150m / s. Finally, it was collected by a conveyor belt to form an antibacterial nonwoven material.
[0070] Through testing and analysis, the average fiber diameter is 0.9μm, the fiber transverse breaking strength is 157N, the longitudinal breaking strength is 201N, the air permeability is 292mm / s, and the antibacterial rate against Escherichia coli is 0.12% when the concentration of non-woven material is 0.15mg / mL; the antiviral activity rate against RNA virus H1N1 reaches 5.24%.
[0071] Figure 5 The mechanical properties of the nonwoven materials of Examples 1 to 2 and Comparative Example 1, a is Example 1, b is Example 2, and c is Comparative Example 1. Figure 5 It can be seen that the longitudinal breaking strength of the nonwoven fabrics prepared in Examples 1 to 2 and Comparative Example 1 is greater than 200N, and the transverse breaking strength is greater than 150N.
[0072] Figure 6 For the nonwoven material in Comparative Example 1 (i.e. Figure 6 The nonwoven fabric in Example 2 (i.e. Figure 6 Electron paramagnetic resonance spectra of the antibacterial nonwoven fabric under light irradiation. The spin trapping agents are ·OH(a), h + (b) and O2 - (c) By Figure 6 It can be seen that the nonwoven material of the present invention can generate active oxygen (hydroxyl free radicals, superoxide free radicals and photogenerated holes) substances under light conditions, has strong oxidizing properties, and can be used to oxidatively kill bacteria.
[0073] Based on Examples 1 to 2 and Comparative Example 1, the following conclusions can be drawn: (1) The antibacterial nonwoven material is simplifies the manufacturing process by using in-situ synthesis of antibacterial agents and instantaneous pressure release method. Compared with the traditional preparation process, the production cost and production time are reduced and shortened; (2) It can be seen from the results of Examples 1 to 2 that the antibacterial nonwoven material prepared by the present invention has the characteristics of good antibacterial property, high breaking strength and strong air permeability; (3) It can be seen from Examples 1 to 2 and Comparative Example 1 that in the absence of a titanium source, a nonwoven material composed of fine fibers can still be prepared. The titanium source is a precursor of the main antibacterial agent and is a key component that gives the nonwoven material antibacterial function.
[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a fiber material with antibacterial function, It is characterized in that The following steps are involved: The titanium source, alkyl alcohol solvent, chemical reactant, cosolvent and polymer particles are mixed, and the obtained mixture is heated to 170-200°C for reaction for 5-10 hours under the condition of sealing and first stirring. The titanium source and the alkyl alcohol solvent form a titanium alcohol complex, which is then dehydrated under the action of the chemical reactant to form TiO 2 ; The chemical reactant includes at least one of N,N-dimethylformamide and N,N-dimethylacetamide; The obtained reaction system is pressurized to 7-15 MPa, the stirring rate is increased, and the second stirring is performed for 1-1.5 hours. The polymer particles become fluid and impact the TiO2 with the alkyl alcohol solvent. 2 Formation of nanoflower-like TiO 2 , a spinning solution is obtained, and then the spinning solution is ejected through the spinneret by releasing the pressure, the solvent evaporates, and polymer fibers are formed to obtain a fiber material with antibacterial function.
2. The preparation method according to claim 1, It is characterized in that The titanium source is one or more of tetrabutyl titanate, titanium tetrachloride and titanium sulfate.
3. The preparation method according to claim 1, It is characterized in that The alkyl alcohol solvent has no more than 5 carbon atoms.
4. The preparation method according to claim 1, It is characterized in that The polymer particles include one or more of polyethylene particles, polypropylene particles, polyester particles and polyamide particles.
5. The preparation method according to claim 1, It is characterized in that The co-solvent includes at least one of ethylene dichloride and methylene dichloride.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that The mass of the raw materials is 100%, the titanium source is 5-8%, the chemical reactant is 25-35%, the alkyl alcohol solvent is 30-37%, the auxiliary solvent is 10-15%, and the polymer particles are 5-30%.
7. The preparation method according to claim 1, It is characterized in that The first stirring rate is 20-40 r / min; the second stirring rate is 100-200 r / min.
8. The preparation method according to claim 1, It is characterized in that The gas used for pressurization is one or more of argon, nitrogen and carbon dioxide.
9. The preparation method according to claim 1, It is characterized in that After the polymer fibers are formed, the method further includes air-opening the polymer fibers and collecting the opened fibers with a conveyor belt.
10. The fiber material with antibacterial function prepared by the preparation method according to any one of claims 1 to 9 is composed of polymer fibers, and the surface of the polymer fibers is distributed with nano-flower-like TiO 2 .
Citation Information
Patent Citations
Novel titanium dioxide particle material, preparation method thereof, application thereof in environment protection field
CN108147453A
Silver phosphate / silver / titanium dioxide nanoflower composite and preparation method and application thereof
CN108579775A
Nano-filtration fiber with antibacterial function and preparation method thereof
CN111455491A
Stretch-resistant cellulose-TiO2 grafted polyvinyl alcohol antibacterial plastic film and preparation method thereof
CN113773537A
Photocatalytic antibacterial fiber and preparation method thereof
CN115216853A