High-thermal-conductivity carbon fiber as well as preparation method and application thereof
By stretching and carbonizing ultra-high molecular weight polyethylene and carbonizing with strong oxidizing agents, combined with heat treatment, carbon fibers with high thermal conductivity were prepared, which solved the problem of insufficient performance of existing thermal conductivity carbon fibers and achieved significant improvement in thermal conductivity.
Patent Information
- Application Number
- CN202411292747.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-12
AI Technical Summary
Existing thermal carbon fibers are still not sufficient to meet the demand in some applications where thermal conductivity is demanded, resulting in the need to adopt more costly other thermally conductive materials, such as graphene materials.
By stretching the ultra-high molecular weight polyethylene, the crystallinity is controlled, and the reaction carbonization is carried out with strong oxidizing agent, the crystallization state of the polymer raw silk is fixed, and the carbonized fibers are finally graphitized through heat treatment to obtain anisotropic High thermal conductivity carbon fiber.
The thermal conductivity of carbon fibers is significantly enhanced, and the thermal conductivity in the axial direction of the fibers is significantly improved, and the thermal conductivity coefficient can reach 500-1800W/(m.K), far exceeding that of general thermally conductive carbon fibers.
Smart Images

Figure CN118932552A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of inorganic carbon materials, and in particular to a high thermal conductivity carbon fiber and a preparation method and application thereof. Background Art
[0002] Carbon fiber refers to high-strength and high-modulus fiber with a carbon content of more than 90%. It has the best high-temperature resistance among all chemical fibers. Traditional carbon fiber is made of high-molecular fibers such as acrylic and viscose fibers, which are oxidized and carbonized at high temperatures. It is an excellent material for manufacturing high-tech equipment such as aerospace.
[0003] Among carbon fibers, there is a special type of thermally conductive carbon fiber, which is a high thermal conductivity carbon fiber material developed for thermal engineering design. The thermal conductivity of this carbon fiber in the fiber direction can exceed that of copper, reaching up to 700W / mk. It also has good mechanical properties, electrical conductivity, and excellent thermal conductivity and radiation heat dissipation capabilities. The fibrous high thermal conductivity carbon powder made of this carbon fiber is fibrous in shape and can be designed with a thermal orientation. This is the biggest difference and advantage from previous carbon powders and other thermally conductive materials. It can be used to fill polymer composites, develop heat dissipation materials for electronic appliances, and solve heat dissipation problems of high-density integrated electronic components and LEDs.
[0004] However, in some application fields with higher thermal conductivity requirements, the thermal conductivity of thermal conductive carbon fiber is still not enough to meet the needs, and technicians have to use other more expensive thermal conductive materials, such as graphene materials. Therefore, it is necessary to develop carbon fiber materials with better thermal conductivity to meet industry needs. Summary of the invention
[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a high thermal conductivity carbon fiber and a preparation method and application thereof.
[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes: In a first aspect, the present invention provides a method for preparing a high thermal conductivity carbon fiber, comprising: Performing a stretching treatment on ultra-high molecular weight polyethylene to obtain polymer precursor, wherein the ultra-high molecular weight polyethylene has a selected molecular weight, and the stretching treatment has a selected elongation and a selected stretching rate, so that the crystallinity of the polymer precursor is above 80%; Using a strong oxidant to perform a reaction carbonization treatment on the polymer precursor to obtain carbonized fibers, wherein the reaction carbonization treatment removes non-carbon elements in the polymer precursor and sets the crystal state of the polymer precursor; The carbonized fibers are subjected to heat treatment to finally graphitize the carbonized fibers to obtain high thermal conductivity carbon fibers.
[0007] In a second aspect, the present invention further provides a high thermal conductivity carbon fiber obtained by the above preparation method, wherein the high thermal conductivity carbon fiber has an anisotropic degree of graphitization, and the degree of graphitization along the radial direction is higher than the degree of graphitization along the axial direction.
[0008] In a third aspect, the present invention also provides the use of the above-mentioned high thermal conductivity fiber in the preparation of a heat transfer component.
[0009] Based on the above technical solution, compared with the prior art, the beneficial effects of the present invention at least include: The preparation method provided by the present invention regulates the crystallinity of the polymer precursor and retains the property of the crystallization state of the precursor when carbonizing the polymer precursor with a strong oxidant, so that the crystal morphology of the polymer precursor is transferred to the carbonized fiber, and finally through subsequent heat treatment, the prepared carbon fiber has an anisotropic degree of graphitization, thereby significantly enhancing the thermal conductivity in the axial direction of the fiber, and achieving a significant improvement in thermal conductivity compared to the thermally conductive carbon fiber prepared by the prior art.
[0010] The above description is only an overview of the technical solution of the present invention. In order to enable those skilled in the art to more clearly understand the technical means of the present application and implement them according to the contents of the specification, the following is a description of the preferred embodiments of the present invention in conjunction with detailed drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 is a schematic diagram of the cross-sectional morphology of a carbonized fiber provided in a typical embodiment of the present invention; Figure 2 This is a transmission electron microscope electron diffraction pattern provided by a typical implementation case of the present invention, in which obvious graphitization orientation can be seen. DETAILED DESCRIPTION
[0012] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.
[0013] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0014] A first aspect of an embodiment of the present invention provides a method for preparing a high thermal conductivity carbon fiber, which comprises the following steps: Performing a stretching treatment on ultra-high molecular weight polyethylene to obtain polymer precursor, wherein the ultra-high molecular weight polyethylene has a selected molecular weight, and the stretching treatment has a selected elongation and a selected stretching rate, so that the crystallinity of the polymer precursor is above 80%; Using a strong oxidant to perform a reaction carbonization treatment on the polymer precursor to obtain carbonized fibers, wherein the reaction carbonization treatment removes non-carbon elements in the polymer precursor and sets the crystal state of the polymer precursor; The carbonized fibers are subjected to heat treatment to finally graphitize the carbonized fibers to obtain high thermal conductivity carbon fibers.
[0015] Regarding how to regulate the crystallinity of polymer precursors, in some exemplary embodiments, the selected molecular weight is 100,000-10,000,000, the selected elongation is 200-700%, and the selected stretching rate is 10-300 m / min. Within the above parameter range, it can be ensured that the crystallinity of the polymer precursor meets the requirements, but it does not mean that the feasible scope of the present invention is limited to this. The above parameters are only exemplary, and those skilled in the art can make appropriate adjustments for different brands and raw materials provided by manufacturers, and the final result is still subject to the regulation result of the crystallinity.
[0016] In the present invention, the crystallinity of the polymer precursor is adjusted by regulating the molecular weight and stretching conditions, and the crystal state in the polymer precursor is "fixed" by carbonization with a strong oxidant so that it is finally "inherited" to the carbon fiber. This is the key to achieving high thermal conductivity. The formed carbon fiber has an axial and radial anisotropic degree of graphitization, and the thermal conductivity in the direction where heat conduction is required is significantly enhanced, thereby obtaining a thermal conductivity coefficient far exceeding that of general thermally conductive carbon fibers.
[0017] For the details of the specific strong oxidant carbonization treatment, reference may be made to the previous research of the inventor of the present invention, "Method for preparing carbon powder from organic polymer materials and method for detecting the crystalline form in organic polymer materials". However, it should be noted that this previous research was based on the preparation of powdered carbon materials, or the use of the detection of the morphology of carbon materials to indirectly reflect the crystalline state in the polymer, rather than the preparation of carbon fibers. Although the basic principles used are similar, the purposes of the two are different.
[0018] In addition, there are some existing technologies, such as the Chinese invention patent with publication number CN114959950A, which mentions a technical solution of using chlorosulfonic acid and other oxidizing acids to treat the polymer after drawing, and then carbonizing and graphitizing it. However, although the strong oxidant is also used to treat the polymer precursor, the purpose of the treatment is different. Its main purpose is sulfonation, which is generally used to increase the number of surface groups and improve the interface binding ability. The range of chemical reaction is generally limited to the vicinity of the surface; while the present invention uses a strong oxidant to perform carbonization. The reaction range of carbonization is comprehensive inside and outside, and non-carbon elements will also be removed inside the fiber. Otherwise, only surface carbonization can be achieved and the internal crystalline state cannot be fixed. In terms of purpose, the above-mentioned prior art does not need to fix the crystalline state, so it is not necessary to deliberately control the crystallinity of the polymer precursor, and the present invention is obviously different from this.
[0019] However, due to the essential difference in purpose, the technical solution proposed in the present invention also has significantly different reaction conditions from the above-mentioned prior art when using a strong oxidant for treatment, as shown in the following part for details.
[0020] In some embodiments, the temperature of the reaction carbonization treatment is 30-120° C. and is lower than the crystallization temperature of the polymer precursor.
[0021] In some embodiments, the strong oxidant includes any one of chlorosulfonic acid, concentrated sulfuric acid, and fluorosulfonic acid, or a combination of two or more thereof.
[0022] The temperature conditions for the reaction carbonization treatment mentioned above are general, but they need to be differentiated for different strong oxidants. For example, for chlorosulfonic acid, an oxidant, its oxidation and dehydration ability is strong. Therefore, for the purpose of fixing the crystal form in the polymer precursor and achieving complete carbonization, the temperature of the reaction carbonization treatment needs to be controlled relatively gently, generally between 30-65°C. When it is lower than 30°C, generally only sulfonation reaction will occur without obvious carbonization; when it is higher than 65°C, it is easy to cause the carbonization rate to be too fast, which will cause microscopic looseness, and it is difficult to fix the crystal form in the polymer precursor, making it difficult to achieve the purpose of high thermal conductivity. For other commonly used strong oxidants, such as concentrated sulfuric acid, due to the differences in oxidizability and dehydration ability, the suitable temperature window varies, usually 80-120°C.
[0023] In general, in the prior art, the temperature for treating polymer precursors with a strong oxidizing sulfonating agent, such as chlorosulfonic acid, is relatively high, generally 70-95°C, and the preferred range is generally around 80-85°C. This is determined by its purpose, which is to graft sulfonic acid groups on the surface rather than to use the crystal form of the polymer precursor to achieve anisotropic graphitization of the carbon fiber. The present invention is different from its purpose. Based on previous studies, the carbonization reaction can shape the crystalline state in the ultra-high molecular weight polyethylene fiber. Using this principle, the present invention creatively adopts corresponding technical means to ultimately retain the crystalline state in the polymer precursor in the carbon fiber, thereby achieving a great improvement in thermal conductivity.
[0024] If the temperature conditions are not properly controlled during the reaction carbonization treatment of the polymer precursor according to the instructions of this type of prior art, it is very easy to cause the problem of being unable to fix the crystal form in the polymer precursor. In addition, in the inventor's previous research, a strong oxidant was used to fix the crystal form in the polymer, and the reaction carbonization temperature used in the process of preparing nano-scale carbon materials was also higher, even reaching 140°C. This is because the purpose itself is to form a nano-scale dispersed material, rather than a complete fiber material. Therefore, it only needs to fix some crystal particles (such as onion-shaped crystal balls or nano-scale fiber crystals) at the microscopic level. These crystal particles do not need to form continuous fibers at the macroscopic level, so there is no need to consider the damage to the fiber structure caused by an excessively fast carbonization rate.
[0025] In some embodiments, the reaction carbonization treatment time is 1-48h.
[0026] In addition, regarding the subsequent heat treatment process, in some embodiments, the heat treatment includes a thermal carbonization treatment and a graphitization treatment in sequence, and the temperature of the graphitization treatment is higher than that of the thermal carbonization treatment.
[0027] In some embodiments, the temperature of the thermal carbonization treatment is 300-1500° C., and the time is 1-48 h; the temperature of the graphitization treatment is 2000-3200° C., and the time is 8-72 h.
[0028] As some typical examples of the above technical solutions, the specific process flow of the preparation method provided by the present invention is as follows: Using ultra-high molecular weight polyethylene as raw material, the crystallinity of ultra-high molecular weight polyethylene is adjusted by adjusting the molecular weight and stretching speed, and the crystallinity is controlled at 80-99%; The obtained tow is carbonized by a strong oxidant, such as concentrated sulfuric acid, chlorosulfonic acid, etc., to achieve reaction carbonization; The carbonized product is carbonized in a carbonization furnace, and the carbonization temperature is, for example, 300-1500°C; Then, graphitization treatment is performed, and the graphitization temperature is, for example, 2000-3200°C.
[0029] In the above steps, after the reaction carbonization, the product has a high degree of graphitization, and after subsequent thermal carbonization and graphitization, the radial graphitization degree of the fiber will be significantly higher than that in other directions, ultimately making the thermal conductivity of the fiber reach 500-1800W / (mK).
[0030] Correspondingly, another aspect of an embodiment of the present invention further provides a high thermal conductivity carbon fiber obtained by the above preparation method, wherein the high thermal conductivity carbon fiber has an anisotropic degree of graphitization, and the degree of graphitization along the radial direction is higher than the degree of graphitization along the axial direction.
[0031] In some embodiments, the thermal conductivity of the high thermal conductivity carbon fiber is 700-1800 W / (mK).
[0032] At the same time, the embodiment of the present invention also provides the application of the above-mentioned high thermal conductivity carbon fiber in the preparation of heat transfer components. The application includes but is not limited to: using the carbon fiber to prepare thermal conductive and structural integrated materials to achieve lightweight structural and thermal conductive dual applications, or using the carbon fiber as an additive, such as adding it to resin or concrete after being chopped, etc.
[0033] The technical solution of the present invention is further described in detail below through several embodiments and in conjunction with the accompanying drawings. However, the selected embodiments are only used to illustrate the present invention, and do not limit the scope of the present invention.
[0034] Example 1 This embodiment illustrates a preparation process of a high thermal conductivity carbon fiber, which is specifically as follows: 1. Purchase ultra-high molecular weight polyethylene (Hunan Zhongtai, ZTXS series, molecular weight 2-3 million), control the elongation rate to 500%, the elongation rate to 150m / min, and draw the raw yarn. The crystallinity of the raw yarn is measured to be 95%.
[0035] 2. The raw silk was immersed in chlorosulfonic acid, the temperature was controlled at 60°C, and the reaction carbonization treatment was carried out for 5 hours.
[0036] 3. Take out the reaction carbonized silk thread, clean it and then perform heat treatment carbonization. The carbonization temperature is 900℃ and the time is 10h.
[0037] 4. Send the heat-treated carbonized wire into a graphitization furnace, set the graphitization temperature to 2800°C, and the time to 24 hours to finally obtain high thermal conductivity carbon fiber.
[0038] Figure 1The cross-sectional morphology of the product obtained in step 2 is shown. It can be seen that after the oxidation and carbonization treatment, the internal crystalline state is fixed and retained, which also lays the foundation for the formation of anisotropic graphitization degree in the subsequent process; Figure 2 The transmission electron microscope electron diffraction pattern of the product is shown, and obvious graphitization orientation can be seen.
[0039] In addition, the thermal conductivity of the carbon fiber obtained in this embodiment was measured, and the final test result was 961 W / (mK), which is significantly higher than that of traditional thermal conductive carbon fiber.
[0040] Comparative Example 1 This comparative example is substantially the same as Example 1, except that: The drawing conditions in step 1 were changed to 5 m / min, and the crystallinity of the final raw wire was 75%.
[0041] The remaining steps are the same as those in Example 1.
[0042] The carbon fiber finally obtained does not have an obvious anisotropic graphitization degree, and its thermal conductivity is 321 W / (mK), which is significantly lower than that of Example 1.
[0043] Comparative Example 2 This comparative example is substantially the same as Example 1, except that: The temperature in step 2 is set to 25° C., at which time only the sulfonation reaction occurs, and the carbonization reaction of the entire fiber body cannot occur.
[0044] The remaining steps are the same as those in Example 1.
[0045] Finally, no carbon fiber is obtained and the residual carbon rate is less than 10%.
[0046] Comparative Example 3 This comparative example is substantially the same as Example 1, except that: The temperature in step 2 is set to 85°C. Although the polymer precursor with a high degree of crystallinity can still be carbonized at this time, the carbonization process directly destroys the crystal morphology in the fiber, making it impossible to fix the crystal form inside.
[0047] The carbon fiber finally obtained is similar to that of Comparative Example 1, and continuous graphitized fibers are obtained in the fibers, and the thermal conductivity is also significantly lower, which is 21 W / (mK).
[0048] Example 2 This embodiment is substantially the same as Embodiment 1, and the main difference is that: In step 2, the strong oxidant is replaced with concentrated sulfuric acid, the treatment temperature is 80°C, and the treatment time is 24h.
[0049] The remaining steps are the same as those in Example 1.
[0050] The carbon fiber obtained in this embodiment still has the same anisotropic graphitization degree as that in Embodiment 1, and the thermal conductivity is as high as 783 W / (mK).
[0051] Example 3 This embodiment is substantially the same as Embodiment 1, and the main difference is that: In step 3, the carbonization temperature is 300°C and the time is 5 hours; in step 4, the graphitization temperature is set to 2000°C and the time is 24 hours.
[0052] The remaining steps are the same as those in Example 1.
[0053] The carbon fiber obtained in this embodiment still has the same anisotropic graphitization degree as that in Embodiment 1, and the thermal conductivity is as high as 655 W / (mK).
[0054] Example 4 This embodiment is substantially the same as Embodiment 1, and the main difference is that: In step 3, the carbonization temperature is 1500° C. and the time is 12 h; in step 4, the graphitization temperature is set to 3200° C. and the time is 72 h.
[0055] The remaining steps are the same as those in Example 1.
[0056] The carbon fiber obtained in this embodiment still has the same anisotropic graphitization degree as that in Embodiment 1, and the thermal conductivity is as high as 1320 W / (mK).
[0057] Based on the above embodiments and comparative examples, it can be clearly seen that the preparation method provided in the embodiments of the present invention can retain the crystalline state of the polymer precursor by regulating the crystallinity of the polymer precursor and using a strong oxidant to carbonize the polymer precursor, so that the crystalline morphology of the polymer precursor is transferred to the carbonized fiber, and finally through subsequent heat treatment, the prepared carbon fiber has an anisotropic degree of graphitization, thereby significantly enhancing the thermal conductivity in the axial direction of the fiber, and achieving a significant improvement in thermal conductivity compared to the thermally conductive carbon fiber prepared by the prior art.
[0058] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing high thermal conductivity carbon fiber, characterized in that: include: Performing a stretching treatment on ultra-high molecular weight polyethylene or high-density polyethylene to obtain polymer precursors, wherein the ultra-high molecular weight polyethylene or high-density polyethylene has a selected molecular weight, and the stretching treatment has a selected elongation and a selected stretching rate, so that the crystallinity of the polymer precursor is above 80%; Using a strong oxidant to perform a reaction carbonization treatment on the polymer precursor to obtain carbonized fibers, wherein the reaction carbonization treatment removes non-carbon elements in the polymer precursor and sets the crystal state of the polymer precursor; The carbonized fibers are subjected to heat treatment to finally graphitize the carbonized fibers to obtain high thermal conductivity carbon fibers.
2. The preparation method according to claim 1, characterized in that: The selected molecular weight is 100000-10000000, the selected elongation is 200-700%, and the selected stretching rate is 10-300 m / min.
3. The preparation method according to claim 1, characterized in that: The temperature of the reaction carbonization treatment is 30-120° C., and is lower than the crystallization temperature of the polymer precursor.
4. The preparation method according to claim 1 or 3, characterized in that: The strong oxidant includes any one of chlorosulfonic acid, concentrated sulfuric acid, and fluorosulfonic acid, or a combination of two or more thereof.
5. The preparation method according to claim 3, characterized in that: The reaction carbonization treatment time is 1-48h; And / or, the polymer filament has a diameter of 1-20 μm.
6. The preparation method according to claim 1, characterized in that: The heat treatment includes a thermal carbonization treatment and a graphitization treatment in sequence, and the temperature of the graphitization treatment is higher than that of the thermal carbonization treatment.
7. The preparation method according to claim 6, characterized in that: The temperature of the thermal carbonization treatment is 300-1500°C and the time is 1-48h; The temperature of the graphitization treatment is 2000-3200° C., and the time is 8-72 hours.
8. The high thermal conductivity carbon fiber obtained by the preparation method according to any one of claims 1 to 7, characterized in that: The high thermal conductivity carbon fiber has an anisotropic graphitization degree, and the graphitization degree in the radial direction is higher than that in the axial direction.
9. The high thermal conductivity carbon fiber according to claim 8, characterized in that: The thermal conductivity of the high thermal conductivity carbon fiber is 500-1800 W / (mK).
10. Use of the high thermal conductivity carbon fiber according to claim 8 or 9 in preparing a heat transfer component.