Preparation method of elastic covering yarn

By pretreatment and post-treatment of core yarns and outsourcing fibers, the problems of insufficient elasticity and poor uniformity in traditional core yarn production are solved, the performance and production efficiency of elastic core yarns are improved, and better elasticity and uniformity are achieved sex.

CN118932575AInactive Publication Date: 2024-11-12XUZHOU YIXIANG TEXTILE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411318837.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-21
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The traditional core-encapsulated yarn production process has problems such as insufficient elasticity, poor uniformity and low production efficiency.

Method used

The core yarn and outsourcing fibers are used to remove impurities and improve processability. The core yarn is stretched and refined by a yarn machine, the outsourcing fibers are evenly coated with a core yarn and post-treatment such as shaping and heat treatment to improve elasticity and stability.

Benefits of technology

The elastic recovery rate, twist, strength and elongation of break of elastic core yarn are improved, the uniformity and production efficiency of the product are enhanced, and the consistency of the product is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932575A_ABST
    Figure CN118932575A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an elastic core-spun yarn, and relates to the technical field of spinning, and the preparation method comprises the following steps: preparing core-spun yarn raw materials which are a core yarn and an outer wrapping fiber; the core yarn and the outer wrapping fiber are pretreated, and third core yarn and third outer wrapping fiber are obtained; the third core yarn is stretched and refined through a spinning frame, and qualified core yarn is obtained; combining the qualified core yarn with the third wrapping fiber by adopting a core-spun machine to obtain an initial elastic core-spun yarn; post-processing the initial elastic covering yarn to obtain an intermediate elastic covering yarn; and detecting the quality of the middle elastic covering yarn, and screening to obtain the finished elastic covering yarn. According to the preparation method disclosed by the invention, the elasticity and the stability of the prepared intermediate elastic covering yarn are improved; therefore, the finished elastic core-spun yarn prepared by the preparation method is excellent in elasticity and good in uniformity, and the production efficiency and the consistency of the product are also improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of spinning, and in particular to a method for preparing an elastic core-spun yarn. Background Art

[0002] Core-spun yarn: Core-spun yarn is generally made of synthetic fiber filaments with good strength and elasticity as the core yarn, and short fibers such as cotton, wool, and viscose are twisted together to form yarn. Core-spun yarn has the excellent properties of filament core yarn and short fibers. It can make use of the excellent physical properties of core yarn chemical fiber filaments and the performance and surface characteristics of short fibers, give full play to the advantages of the two fibers and make up for their shortcomings. At present, ring-spun core-spun yarn is the mainstream in industrial production, and vortex-spun core-spun yarn and air-spun core-spun yarn also have a certain scale.

[0003] The traditional core-spun yarn production process has problems such as insufficient elasticity, poor uniformity, and low production efficiency. Therefore, an improved preparation method is needed to improve the performance and production efficiency of the elastic core-spun yarn. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing an elastic core-spun yarn, aiming to solve the above technical problems.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing an elastic core-spun yarn comprises the following steps:

[0007] Prepare the core-spun yarn raw material, wherein the core-spun yarn raw material comprises core yarn and outer covering fiber;

[0008] Pre-treating the core yarn and the outer covering fiber to remove impurities and improve the processability of the outer covering fiber, thereby obtaining a third core yarn and a third outer covering fiber;

[0009] The third core yarn is stretched and thinned by a spinning frame to achieve a predetermined fineness and strength, thereby obtaining a qualified core yarn;

[0010] The qualified core yarn is combined with the third outer covering fiber by using a core covering machine, and the third outer covering fiber is evenly covered on the qualified core yarn by adjusting the working parameters of the core covering machine to obtain the initial elastic core covering yarn;

[0011] Post-processing the initial elastic core-spun yarn to obtain an intermediate elastic core-spun yarn;

[0012] The intermediate elastic core-spun yarn is subjected to quality inspection and screened to obtain a finished elastic core-spun yarn.

[0013] Preferably, the core yarn is made of polyurethane elastic fiber, and the outer covering fiber is made of nylon fiber.

[0014] Preferably, the core yarn and the outer covering fiber are pretreated to remove impurities and improve the processability of the outer covering fiber, specifically comprising the following steps:

[0015] Using a cleaning liquid to clean the core yarn and the outer covering fiber to obtain a first core yarn and a first outer covering fiber;

[0016] Drying the first core yarn and the first outer covering fiber to obtain a second core yarn and a second outer covering fiber;

[0017] The second core yarn and the second sheath fiber are pre-stretched to obtain a third core yarn and a third sheath fiber.

[0018] Preferably, the core yarn and the outer fiber are cleaned to obtain a first core yarn and a first outer fiber, wherein the cleaning liquid is obtained by diluting water and a detergent according to a predetermined dilution ratio, and the pH value of the cleaning liquid is in the range of 6.5-7.5, the water temperature during the cleaning process is in the range of 30°C-50°C, and the cleaning time is in the range of 10min-30min.

[0019] Preferably, the first core yarn and the first outer covering fiber are dried to obtain the second core yarn and the second outer covering fiber, wherein the drying method is drying in a dryer, the drying temperature is 40°C to 80°C, the drying time is 30min-120min, and the relative humidity of the drying environment is kept below 20% during the drying process.

[0020] Preferably, a spinning frame is used to stretch and thin the third core yarn to achieve a predetermined fineness and strength, thereby obtaining a qualified core yarn, wherein the stretching ratio range of the third core yarn of the spinning frame is 1.2-3.0, the stretching temperature range is 60℃-150℃, the stretching speed range is 50m / min-300m / min, the fineness value of the qualified core yarn is 150D, and the strength value of the qualified core yarn is 4g / D.

[0021] Preferably, a core-wrapping machine is used to combine the qualified core yarn with the third outer covering fiber, and the third outer covering fiber is evenly coated on the qualified core yarn by adjusting the working parameters of the core-wrapping machine to obtain the initial elastic core-wrapped yarn, wherein the speed range of the core-wrapping machine is 20m / min-1000m / min, the tension range of the core-wrapping machine is 11CN-13CN, the coating ratio of the qualified core yarn to the third outer covering fiber is 2:1, and the coating angle range of the core-wrapping machine is 5° to 60°.

[0022] Preferably, the initial elastic core-spun yarn is post-processed to improve the elasticity and stability of the initial elastic core-spun yarn, thereby obtaining the intermediate elastic core-spun yarn, which specifically includes the following steps:

[0023] The initial elastic core-spun yarn is subjected to a setting treatment by using a setting machine, wherein the setting temperature range of the setting machine is 80° C.-180° C., and the setting time range is 5 min-20 min;

[0024] The initial elastic core-spun yarn after the setting treatment is heat treated, wherein the temperature range of the heat treatment is 60°C-150°C, and the time range of the heat treatment is 8min-16min;

[0025] The heat-treated initial elastic core-spun yarn is wound to obtain the intermediate elastic core-spun yarn.

[0026] Preferably, the intermediate elastic core-spun yarn is subjected to quality inspection to obtain the finished elastic core-spun yarn through screening, wherein the quality inspection items include inspecting the elasticity, uniformity, strength and elongation of the intermediate elastic core-spun yarn.

[0027] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0028] The elastic recovery rate, twist, strength and elongation at break of the elastic core-spun yarn prepared by the preparation method of the present invention are all superior to those of the elastic core-spun yarn prepared by the traditional method. At the same time, the core yarn and the outer sheath fiber are pretreated to remove impurities and improve the processability of the outer sheath fiber. At the same time, the elasticity and stability of the intermediate elastic core-spun yarn are improved by post-processing the initial elastic core-spun yarn. Therefore, the finished elastic core-spun yarn prepared by the preparation method of the present invention has excellent elasticity and good uniformity, and the production efficiency and consistency of the product are also improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0030] Figure 1 A flow chart of a method for preparing an elastic core-spun yarn is shown.

[0031] Figure 2 A flow chart for pre-treating the core yarn and sheath fibers is shown.

[0032] Figure 3 A flow chart for post-processing the initial elastic core-spun yarn is shown. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0035] Reference Figures 1 to 3 The preparation method of an elastic core-spun yarn of the present invention is further described in an embodiment.

[0036] Example 1, polyurethane elastic fiber is selected as the raw material of the core yarn and nylon fiber is selected as the raw material of the outer fiber, and then the polyurethane elastic fiber and the nylon fiber are cleaned with a cleaning solution with a pH value of 6.5 and a temperature of 30°C for 10 minutes to obtain the first core yarn and the first outer fiber, and then the drying temperature of the dryer is set to 40°C and the drying time is 30 minutes to dry the first core yarn and the first outer fiber, and keep the relative humidity of the drying environment below 20% to obtain the second core yarn and the second outer fiber, and then the second core yarn and the second outer fiber are pre-stretched to obtain the third core yarn and the third outer fiber, and then the stretching ratio of the spinning frame is set to 1.2, the stretching temperature is 60°C, and the stretching speed is 50m / min, and the third core yarn is stretched and thinned to obtain a fineness value of 150D and a strength value of 4g / D. Qualified core yarn; setting the speed of the core-wrapping machine to 20m / min, the tension of the core-wrapping machine to 11CN, and the covering angle range of the core-wrapping machine to 5°, combining the qualified core yarn with the third outer covering fiber, so that the third outer covering fiber is evenly covered on the qualified core yarn, wherein the covering ratio of the qualified core yarn to the third outer covering fiber is 2:1, so as to obtain the initial elastic core-wrapped yarn; setting the setting temperature range of the setting machine to 80°C and the setting time range to 5min, using the setting machine to set the initial elastic core-wrapped yarn, and then heat-treating the initial elastic core-wrapped yarn after the setting treatment, wherein the temperature range of the heat treatment is 60°C and the time range of the heat treatment is 8min; then winding the initial elastic core-wrapped yarn after the heat treatment to obtain the intermediate elastic core-wrapped yarn; testing the elasticity, uniformity, strength and elongation of the intermediate elastic core-wrapped yarn to obtain the finished elastic core-wrapped yarn.

[0037] In Example 2, polyurethane elastic fiber is selected as the raw material of the core yarn and nylon fiber is selected as the raw material of the outer fiber, and then the polyurethane elastic fiber and the nylon fiber are cleaned with a cleaning solution with a pH value of 7.5 and a temperature of 50°C for 30 minutes to obtain a first core yarn and a first outer fiber, and then the drying temperature of the dryer is set to 80°C and the drying time is 120 minutes to dry the first core yarn and the first outer fiber, and the relative humidity of the drying environment is kept below 20% to obtain a second core yarn and a second outer fiber, and then the second core yarn and the second outer fiber are pre-stretched to obtain a third core yarn and a third outer fiber, and then the stretching ratio of the spinning frame is set to 3.0, the stretching temperature is 150°C, and the stretching speed is 150m / min, and the third core yarn is stretched and thinned to obtain a composite yarn with a fineness value of 150D and a strength value of 4g / D. core yarn; setting the speed of the core-wrapping machine to 80m / min, the tension of the core-wrapping machine to 13CN, the covering angle range of the core-wrapping machine to 30°, combining the qualified core yarn with the third outer covering fiber, so that the third outer covering fiber is evenly covered on the qualified core yarn, wherein the covering ratio of the qualified core yarn to the third outer covering fiber is 2:1, so as to obtain the initial elastic core-wrapped yarn; setting the setting temperature range of the setting machine to 130°C, and the setting time range to 20min, using the setting machine to set the initial elastic core-wrapped yarn, and then heat-treating the initial elastic core-wrapped yarn after the setting treatment, wherein the temperature range of the heat treatment is 150°C, and the time range of the heat treatment is 16min; then winding the initial elastic core-wrapped yarn after the heat treatment to obtain the intermediate elastic core-wrapped yarn; testing the elasticity, uniformity, strength and elongation of the intermediate elastic core-wrapped yarn to obtain the finished elastic core-wrapped yarn.

[0038] Example 3, polyurethane elastic fiber is selected as the raw material of the core yarn and nylon fiber is selected as the raw material of the outer fiber, and then the polyurethane elastic fiber and the nylon fiber are cleaned with a cleaning solution with a pH value of 7 and a temperature of 40°C for 20 minutes to obtain a first core yarn and a first outer fiber, and then the drying temperature of the dryer is set to 60°C and the drying time is 80 minutes to dry the first core yarn and the first outer fiber, and the relative humidity of the drying environment is kept below 20% to obtain a second core yarn and a second outer fiber, and then the second core yarn and the second outer fiber are pre-stretched to obtain a third core yarn and a third outer fiber, and then the stretching ratio of the spinning frame is set to 2, the stretching temperature is 100°C, and the stretching speed is 100m / min, and the third core yarn is stretched and thinned to obtain a qualified core yarn with a fineness value of 150D and a strength value of 4g / D. Yarn; setting the speed of the core-wrapping machine to 50m / min, the tension of the core-wrapping machine to 12CN, and the covering angle range of the core-wrapping machine to 15°, combining the qualified core yarn with the third outer covering fiber, so that the third outer covering fiber is evenly covered on the qualified core yarn, wherein the covering ratio of the qualified core yarn to the third outer covering fiber is 2:1, so as to obtain the initial elastic core-wrapped yarn; setting the setting temperature range of the setting machine to 90°C and the setting time range to 15min, using the setting machine to set the initial elastic core-wrapped yarn, and then heat-treating the initial elastic core-wrapped yarn after the setting treatment, wherein the temperature range of the heat treatment is 80°C, and the time range of the heat treatment is 12min; then winding the initial elastic core-wrapped yarn after the heat treatment to obtain the intermediate elastic core-wrapped yarn; testing the elasticity, uniformity, strength and elongation of the intermediate elastic core-wrapped yarn to obtain the finished elastic core-wrapped yarn.

[0039] In a comparative example, a polyurethane elastic fiber with a diameter of 30 dtex is prepared as a core yarn; a polyester fiber with a fineness of 2.0 dtex is prepared as an outer fiber; the core yarn is chemically treated and impregnated with a surfactant to improve its adhesion with the outer fiber; the core yarn and the outer fiber are twisted together using a double twisting technology, first twisting in a clockwise direction for the first time and then twisting in a counterclockwise direction for the second time; the obtained core-spun yarn is heat-set to improve its elastic recovery performance, thereby obtaining a finished elastic core-spun yarn.

[0040] The quality inspection items of the intermediate elastic core-spun yarns prepared in Example 1, Example 2, and Example 3 and the finished elastic core-spun yarns prepared in the comparative example are as follows:

[0041] 50 cm lengths were cut from the intermediate elastic core-spun yarn prepared in Example 1, the intermediate elastic core-spun yarn prepared in Example 2, the intermediate elastic core-spun yarn prepared in Example 3, and the finished core-spun yarn in the comparative example, and they were named as Sample 1, Sample 2, Sample 3, and Sample 4, respectively;

[0042] Elasticity test: Use a dedicated tensile testing machine for testing. The steps of elasticity test are as follows:

[0043] Fix each sample on the fixture of the tensile testing machine and set the initial tension;

[0044] Stretch the sample at a constant rate to a specified elongation;

[0045] After holding for a certain period of time, release the tension and allow each sample to return to its original state;

[0046] Repeat the above steps several times, and record the elongation and recovery each time;

[0047] The elastic recovery rate of each sample was obtained by averaging the test results of each sample.

[0048] Uniformity test: Use a twist tester to test the twist of each sample, and take the average of the recorded results each time to get the twist of each sample;

[0049] Strength and elongation testing: Use a universal material testing machine to carry out strength and elongation testing.

[0050] Fix each sample on the fixture of the testing machine and set the appropriate tensile speed.

[0051] The samples were stretched until they broke, and the maximum load and elongation of each sample were recorded.

[0052] The test results of sample 1, sample 2, sample 3 and sample 4 are shown in the following table:

[0053] Sample 1 Sample 2 Sample 3 Sample 4 Elastic recovery rate / % 92 95 93 90 Twist / twist / m 95 100 94 91 Strength / cN / dtex 4 5 3 3 Elongation at break / % 286 300 282 230

[0054] It can be seen from the above table that the elastic recovery rate, twist, strength and elongation at break of the elastic core-spun yarn prepared by the preparation method of the present invention are superior to those of the elastic core-spun yarn prepared by the traditional method. At the same time, the core yarn and the outer fiber are pretreated to remove impurities and improve the processability of the outer fiber. At the same time, the elasticity and stability of the intermediate elastic core-spun yarn are improved by post-processing the initial elastic core-spun yarn. Therefore, the finished elastic core-spun yarn prepared by the preparation method of the present invention has excellent elasticity and good uniformity, and the production efficiency and consistency of the product are also improved.

[0055] The above description of the embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing an elastic core-spun yarn, characterized in that: The steps include: Prepare the core-spun yarn raw material, wherein the core-spun yarn raw material comprises core yarn and outer covering fiber; Pre-treating the core yarn and the outer covering fiber to remove impurities and improve the processability of the outer covering fiber, thereby obtaining a third core yarn and a third outer covering fiber; The third core yarn is stretched and thinned by a spinning frame to achieve a predetermined fineness and strength, thereby obtaining a qualified core yarn; The qualified core yarn is combined with the third outer covering fiber by using a core covering machine, and the third outer covering fiber is evenly covered on the qualified core yarn by adjusting the working parameters of the core covering machine to obtain the initial elastic core covering yarn; Post-processing the initial elastic core-spun yarn to obtain an intermediate elastic core-spun yarn; The intermediate elastic core-spun yarn is subjected to quality inspection and screened to obtain a finished elastic core-spun yarn.

2. The method for preparing an elastic core-spun yarn according to claim 1, characterized in that: The core yarn is made of polyurethane elastic fiber, and the outer covering fiber is made of nylon fiber.

3. The method for preparing an elastic core-spun yarn according to claim 2, characterized in that: The core yarn and the outer covering fiber are pretreated to remove impurities and improve the processability of the outer covering fiber, specifically comprising the following steps: Using a cleaning liquid to clean the core yarn and the outer covering fiber to obtain a first core yarn and a first outer covering fiber; Drying the first core yarn and the first outer covering fiber to obtain a second core yarn and a second outer covering fiber; The second core yarn and the second sheath fiber are pre-stretched to obtain a third core yarn and a third sheath fiber.

4. The method for preparing an elastic core-spun yarn according to claim 3, characterized in that: The core yarn and the outer fiber are cleaned to obtain a first core yarn and a first outer fiber, wherein the cleaning liquid is obtained by diluting water and a detergent according to a predetermined dilution ratio, and the pH value range of the cleaning liquid is 6.5-7.5, the water temperature range during the cleaning process is 30°C-50°C, and the cleaning time range is 10min-30min.

5. The method for preparing an elastic core-spun yarn according to claim 4, characterized in that: The first core yarn and the first outer fiber are dried to obtain a second core yarn and a second outer fiber, wherein the drying method is drying in a dryer, the drying temperature is 40°C to 80°C, the drying time is 30min-120min, and the relative humidity of the drying environment is kept below 20% during the drying process.

6. The method for preparing an elastic core-spun yarn according to claim 5, characterized in that: A spinning frame is used to stretch and thin the third core yarn to achieve a predetermined fineness and strength, thereby obtaining a qualified core yarn, wherein the stretching ratio range of the third core yarn of the spinning frame is 1.2-3.0, the stretching temperature range is 60℃-150℃, the stretching speed range is 50m / min-300m / min, the fineness value of the qualified core yarn is 150D, and the strength value of the qualified core yarn is 4g / D.

7. The method for preparing an elastic core-spun yarn according to claim 6, characterized in that: A core-wrapping machine is used to combine the qualified core yarn with the third outer covering fiber. By adjusting the working parameters of the core-wrapping machine, the third outer covering fiber is evenly coated on the qualified core yarn to obtain the initial elastic core-wrapped yarn. The speed range of the core-wrapping machine is 20m / min-1000m / min, the tension range of the core-wrapping machine is 11CN-13CN, the coating ratio of the qualified core yarn to the third outer covering fiber is 2:1, and the coating angle range of the core-wrapping machine is 5° to 60°.

8. The method for preparing an elastic core-spun yarn according to claim 7, characterized in that: The initial elastic core-spun yarn is post-processed to improve the elasticity and stability of the initial elastic core-spun yarn, thereby obtaining the intermediate elastic core-spun yarn, which specifically includes the following steps: The initial elastic core-spun yarn is subjected to a setting treatment by using a setting machine, wherein the setting temperature range of the setting machine is 80° C.-180° C., and the setting time range is 5 min-20 min; The initial elastic core-spun yarn after the setting treatment is heat treated, wherein the temperature range of the heat treatment is 60°C-150°C, and the time range of the heat treatment is 8min-16min; The heat-treated initial elastic core-spun yarn is wound to obtain the intermediate elastic core-spun yarn.

9. The method for preparing an elastic core-spun yarn according to claim 8, characterized in that: The intermediate elastic core-spun yarn is subjected to quality inspection to obtain finished elastic core-spun yarn through screening, wherein the quality inspection items include inspecting the elasticity, uniformity, strength and elongation of the intermediate elastic core-spun yarn.