Sports socks and production process of anti-skid yarns thereof

The anti-slip yarn made of polyester slices solves the problem of reduced friction under sweat by precrystallization, spinning, stripping, bleaching, fiber opening and drafting twisting processes. Achieve greater friction and better comfort protection during exercise.

CN118932578APending Publication Date: 2024-11-12HAINING CHUANGYUAN KNITTING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411270034.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The friction of existing sports socks reduces after being soaked in sweat, resulting in reduced comfort and may cause foot wear. The existing high-strength yarn is harder and not suitable for long-term wear.

Method used

Polyester slices are used as raw material, and anti-slip yarn is made through precrystallization, spinning, stripping, bleaching, fiber opening and drafting twisting, ensuring that the yarn is soft and durable while ensuring high friction. sex.

Benefits of technology

The made non-slip yarn provides greater friction and better comfort during exercise, reducing the risk of socks falling off and providing professional protection during high-intensity exercise.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses sports socks and a production process of anti-slip yarns thereof, and belongs to the technical field of yarn preparation, polyester chips are selected as raw materials, and the production process of the anti-slip yarns is completed through the steps of raw material processing, spinning, drawing, bleaching, splitting, drafting and twisting and the like. The sports socks are woven by the anti-skid yarns; polyester chips are spun, drawn slivers obtained after three times of drawing are conducted on the polyester chips are high in strength, the drawn slivers are softer after splitting, the hand feeling of the drawn slivers is improved, fibers of the split drawn slivers crack into mutually-connected filaments, the friction area between the fibers and a contact object is increased so as to increase friction force, and a finished product is formed after drafting and twisting. The strength of the anti-skid yarn is further improved, gaps among the filaments are smaller, the friction area is further enlarged, the friction force is increased, the anti-skid yarn is softer, and the woven sports socks have various characteristics of the anti-skid yarn and can be protected more comprehensively during sports.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of yarn preparation, in particular to a production process of anti-slip yarn for sports socks. Background Art

[0002] When doing sports, people usually wear professional sportswear to make their limbs more comfortable during exercise. Compared with ordinary socks, sports socks generally have greater friction. During exercise, they can better fit the feet and the inside of the shoes, reducing the probability of injury due to socks falling off during exercise.

[0003] Existing sports socks generally use high-friction yarn weaving or glue-dotting technology on the bottom to improve friction. After the socks with glue-dotting on the bottom are soaked with sweat, the friction will be reduced, making them lose their function. High-friction yarn is generally harder, which reduces the wearing comfort. During high-intensity exercise, it will cause foot abrasions. The defects are relatively obvious. Therefore, a production process of sports socks and anti-slip yarns thereof is proposed to solve the above problems. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the present invention provides a production process of sports socks and anti-slip yarns thereof. When the socks are worn, the friction between the socks and the soles of the feet and the soles of the shoes is large during exercise, while taking into account the comfort of wearing, thereby achieving a professional protective effect.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a production process of anti-slip yarn, selecting polyester chips as raw materials, and completing the production process of anti-slip yarn through raw material processing, spinning, drawing, bleaching, fiber opening, drafting and twisting, etc. The specific steps are as follows:

[0006] S1. Raw material processing: After pre-crystallization, drying and solid phase polymerization, the polyester chips are added to the screw extruder;

[0007] S2, spinning: The screw extruder melts the raw materials, filters them, removes impurities, and then stretches and cools them to obtain polyester filament fibers;

[0008] S3, drawing: feeding multiple polyester filament fibers into a drawing frame and combining them to make drawn slivers;

[0009] S4, bleaching: soaking the cooked noodles prepared in step S3 in a bleaching agent for bleaching;

[0010] S5, fiber opening: soaking the bleached sliver in step S4 in a strong alkali to open the sliver;

[0011] S6, drawing and twisting: the sliver after opening in step S5 is drawn and twisted on a roving frame, and then further drawn, twisted and wound on a spinning frame, and finally combined to form an anti-slip yarn.

[0012] Preferably, the raw material processing technology in step S1 is as follows: the pre-crystallization temperature of the polyester chips is 170° C., the crystallization time is 1h-2h, the drying temperature of the polyester chips after pre-crystallization is 160° C.-170° C., and the drying time is 4h-6h.

[0013] Preferably, the spinning process in step S2 is as follows: spinning temperature 260°C-270°C, spinning speed 2200m / min, cooling temperature 20°C-25°C, cooling wind speed 0.1m / s-0.3m / s.

[0014] Preferably, the drawing process in step S3 is specifically as follows: the drawing process is completed through first drawing, second drawing and third drawing, the first drawing is six strands drawn together, and the stretching multiple after drawing is 2 times, the second drawing is eight strands drawn together, and the stretching multiple after drawing is 7 times, and the third drawing is four strands drawn together, and the stretching multiple after drawing is 11 times.

[0015] Preferably, the bleaching process in step S4 is specifically as follows: a mixed solvent of sodium hypochlorite and hydrogen peroxide is selected as the bleaching agent, the bleaching time is 30 min-40 min, and the bleaching temperature is 100° C.-130° C.

[0016] Preferably, the fiber opening process in step S5 is specifically as follows: a sodium hydroxide solution with a concentration of 40 g / L-60 g / L is selected as the strong alkaline solution, the fiber opening time is 60 min-80 min, and the fiber opening temperature is 90° C.-110° C.

[0017] Preferably, the number of strands of the cooked noodles in step S3 is 192F, and the denier thereof is 600D.

[0018] The present invention also provides a pair of sports socks, which are made by weaving the above-mentioned anti-skid yarn.

[0019] Compared with the prior art, the present invention can achieve the following beneficial effects:

[0020] The polyester chips are spun and the strength of the sliver after three-pass drawing is high. After bleaching and fiber opening, the state of the sliver is changed to make it soft to the touch. The opened sliver fibers are longitudinally cracked into interconnected filaments, which have an anti-slip effect. After stretching and twisting, the finished product is formed, which further improves the strength of the anti-slip yarn, makes the gaps between the filaments smaller, increases the friction and becomes softer, and is used to weave sports socks. The socks have various characteristics of anti-slip yarn and can provide more comprehensive protection during exercise. DETAILED DESCRIPTION

[0021] The technical solution of the present invention is described below through specific embodiments.

[0022] The production process of the anti-slip yarn provided by the present invention selects polyester chips as raw materials, and completes the production process of the anti-slip yarn through the steps of raw material processing, spinning, drawing, bleaching, fiber opening, drafting and twisting. The specific steps are as follows:

[0023] Embodiment 1:

[0024] S1. Raw material processing: After pre-crystallization, drying and solid phase polymerization, the polyester chips are added to the screw extruder; the pre-crystallization temperature of the polyester chips is 170°C, the crystallization time is 2h, and the drying temperature of the polyester chips after pre-crystallization is 160°C, and the drying time is 6h.

[0025] S2. Spinning: The screw extruder melts the raw materials, filters them to remove impurities, and then stretches and cools them to obtain polyester filament fibers; the spinning temperature is 260°C, the spinning speed is 2200m / min, the cooling temperature is 25°C, and the cooling wind speed is 0.1m / s.

[0026] S3. Drawing: Feed multiple polyester filament fibers into a drawing frame and combine them to make drawn slivers; the drawing process is completed through first, second and third drawing. The first drawing is six strands, and the drafting multiple after drawing is 2 times; the second drawing is eight strands, and the drafting multiple after drawing is 7 times; the third drawing is four strands, and the drafting multiple after drawing is 11 times. The number of strands in the drawn sliver is 192F, and its denier is 600D.

[0027] S4, bleaching: soaking the cooked strips prepared in step S3 in a bleaching agent for bleaching; a mixed solvent of sodium hypochlorite and hydrogen peroxide is selected as the bleaching agent, the bleaching time is 40 minutes, and the bleaching temperature is 100°C.

[0028] S5, fiber opening: soak the bleached sliver in step S4 in a strong alkali for fiber opening; a sodium hydroxide solution with a concentration of 40 g / L is selected as the strong alkali solution, the fiber opening time is 80 min, and the fiber opening temperature is 90°C.

[0029] S6, drawing and twisting: the sliver after opening in step S5 is drawn and twisted on a roving frame, and then further drawn, twisted and wound on a spinning frame, and finally combined to form an anti-slip yarn.

[0030] Anti-slip yarn is woven into sports socks.

[0031] Embodiment 2:

[0032] S1. Raw material processing: After pre-crystallization, drying and solid phase polymerization, the polyester chips are added to the screw extruder; the pre-crystallization temperature of the polyester chips is 170°C, the crystallization time is 2h, and the drying temperature of the polyester chips after pre-crystallization is 160°C, and the drying time is 6h.

[0033] S2. Spinning: The screw extruder melts the raw materials, filters them to remove impurities, and then stretches and cools them to obtain polyester filament fibers; the spinning temperature is 270°C, the spinning speed is 2200m / min, the cooling temperature is 25°C, and the cooling wind speed is 0.3m / s.

[0034] S3. Drawing: Feed multiple polyester filament fibers into a drawing frame and combine them to make drawn slivers; the drawing process is completed through first, second and third drawing. The first drawing is six strands, and the drafting multiple after drawing is 2 times; the second drawing is eight strands, and the drafting multiple after drawing is 7 times; the third drawing is four strands, and the drafting multiple after drawing is 11 times. The number of strands in the drawn sliver is 192F, and its denier is 600D.

[0035] S4, bleaching: soaking the cooked strips prepared in step S3 in a bleaching agent for bleaching; a mixed solvent of sodium hypochlorite and hydrogen peroxide is selected as the bleaching agent, the bleaching time is 30 minutes, and the bleaching temperature is 130°C.

[0036] S5, fiber opening: soak the bleached sliver in step S4 in a strong alkali for fiber opening; select a sodium hydroxide solution with a concentration of 60g / L as the strong alkali solution, the fiber opening time is 60min, and the fiber opening temperature is 110°C.

[0037] S6, drawing and twisting: the sliver after opening in step S5 is drawn and twisted on a roving frame, and then further drawn, twisted and wound on a spinning frame, and finally combined to form an anti-slip yarn.

[0038] Anti-slip yarn is woven into sports socks.

[0039] Embodiment 3:

[0040] S1. Raw material processing: After pre-crystallization, drying and solid phase polymerization, the polyester chips are added into the screw extruder; the pre-crystallization temperature of the polyester chips is 170°C, the crystallization time is 1h, and the drying temperature of the polyester chips after pre-crystallization is 160°C, and the drying time is 5h.

[0041] S2. Spinning: The screw extruder melts the raw materials, filters them to remove impurities, and then stretches and cools them to obtain polyester filament fibers; the spinning temperature is 270°C, the spinning speed is 2200m / min, the cooling temperature is 25°C, and the cooling wind speed is 0.1m / s.

[0042] S3. Drawing: Feed multiple polyester filament fibers into a drawing frame and combine them to make drawn slivers; the drawing process is completed through first, second and third drawing. The first drawing is six strands, and the drafting multiple after drawing is 2 times; the second drawing is eight strands, and the drafting multiple after drawing is 7 times; the third drawing is four strands, and the drafting multiple after drawing is 11 times. The number of strands in the drawn sliver is 192F, and its denier is 600D.

[0043] S4, bleaching: soaking the cooked strips prepared in step S3 in a bleaching agent for bleaching; a mixed solvent of sodium hypochlorite and hydrogen peroxide is selected as the bleaching agent, the bleaching time is 40 minutes, and the bleaching temperature is 120°C.

[0044] S5, fiber opening: soak the bleached sliver in step S4 in a strong alkali for fiber opening; a sodium hydroxide solution with a concentration of 40 g / L is selected as the strong alkali solution, the fiber opening time is 80 min, and the fiber opening temperature is 110°C.

[0045] S6, drawing and twisting: the sliver after opening in step S5 is drawn and twisted on a roving frame, and then further drawn, twisted and wound on a spinning frame, and finally combined to form an anti-slip yarn.

[0046] Anti-slip yarn is woven into sports socks.

[0047] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. The production process of anti-slip yarn, Features: Select polyester chips as raw materials, and go through raw material processing, spinning, drawing, bleaching, fiber opening, drafting and twisting to complete the production process of anti-slip yarn. The specific steps are as follows: S1. Raw material processing: After pre-crystallization, drying and solid phase polymerization, the polyester chips are added to the screw extruder; S2, spinning: The screw extruder melts the raw materials, filters them, removes impurities, and then stretches and cools them to obtain polyester filament fibers; S3, drawing: feeding multiple polyester filament fibers into a drawing frame and combining them to make drawn slivers; S4, bleaching: soaking the cooked noodles prepared in step S3 in a bleaching agent for bleaching; S5, fiber opening: soaking the bleached sliver in step S4 in a strong alkali to open the sliver; S6, drawing and twisting: the sliver after opening in step S5 is drawn and twisted on a roving frame, and then further drawn, twisted and wound on a spinning frame, and finally combined to form an anti-slip yarn.

2. The production process of the anti-slip yarn according to claim 1, Features: The raw material processing technology in step S1 is specifically as follows: the pre-crystallization temperature of the polyester chips is 170° C., the crystallization time is 1h-2h, the drying temperature of the polyester chips after pre-crystallization is 160° C.-170° C., and the drying time is 4h-6h.

3. The production process of the anti-slip yarn according to claim 1, Features: The spinning process in step S2 is specifically as follows: spinning temperature is 260°C-270°C, spinning speed is 2200m / min, cooling temperature is 20°C-25°C, cooling wind speed is 0.1m / s-0.3m / s.

4. The production process of the anti-slip yarn according to claim 1, Features: The drawing process in step S3 is specifically as follows: the drawing process is completed through first drawing, second drawing and third drawing, the first drawing is six strands, and the drafting multiple after drawing is 2 times, the second drawing is eight strands, and the drafting multiple after drawing is 7 times, and the third drawing is four strands, and the drafting multiple after drawing is 11 times.

5. The production process of the anti-slip yarn according to claim 1, Features: The bleaching process in step S4 is specifically as follows: a mixed solvent of sodium hypochlorite and hydrogen peroxide is selected as the bleaching agent, the bleaching time is 30 min-40 min, and the bleaching temperature is 100° C.-130° C.

6. The production process of the anti-slip yarn according to claim 1, Features: The fiber opening process in step S5 is specifically as follows: a sodium hydroxide solution with a concentration of 40 g / L-60 g / L is selected as a strong alkaline solution, the fiber opening time is 60 min-80 min, and the fiber opening temperature is 90° C.-110° C.

7. The production process of the anti-slip yarn according to claim 4, Features: The number of strands of the cooked yarn in step S3 is 192F, and the denier thereof is 600D.

8. A pair of sports socks, Features: The anti-slip yarn according to any one of claims 1 to 7 is used for weaving.

Citation Information

Patent Citations

  • Socks and preparing method thereof

    CN103564663A

  • Fabric and applications thereof

    CN105506848A

  • Preparation method of colorful weak-twisted composite yarn

    CN107780012A

  • Preparation method of linen and fine-denier polyester socks

    CN108442139A

  • Composite long / short spun yarn,its manufacturing method, grey cloth and fabric using the same, and fabric opening apparatus for making the same

    CN1521291A