Method for preparing silicon-coated soft / hard carbon composite carbon nanotube film through coaxial static spinning and application of silicon-coated soft / hard carbon composite carbon nanotube film
The soft/hard carbon composite carbon nanotube film synthesized by coaxial static spinning method and high-temperature carbonization process solves the problem of silicon volume expansion and poor conductivity of the negative electrode material of lithium-ion batteries, and realizes a battery with high discharge specific capacity and long cycle life performance.
Patent Information
- Application Number
- CN202410952858.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-12
AI Technical Summary
The negative electrode material of lithium-ion battery has problems such as volume expansion, resulting in electrode powderization, poor conductivity and low cycling performance. The prior art silicon-carbon composite materials have complex processes and high costs.
Using coaxial static spinning method and high-temperature carbonization process, the soft/hard carbon composite carbon nanotube film with yolk shell structure is synthesized by mesophase as soft carbon precursor and polyacrylonitrile as hard carbon precursor, and the internal cavity is used. Combining carbon shell with the outer layer relieves the volume expansion of silicon and speeds up the electrode reaction rate.
It achieves high discharge specific capacity and long cycle life, simplifies the process, reduces costs, and improves the electrochemical performance of the battery.
Smart Images

Figure CN118932604A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrochemical energy storage, and specifically relates to a method for preparing a silicon-coated soft / hard carbon composite carbon nanotube film by coaxial static spinning and application of the film in a negative electrode of a lithium ion battery. Background Art
[0002] The rapid development of society has driven all walks of life to move forward in leaps and bounds. The level of science and technology and living standards are getting higher and higher. People's requirements for daily necessities and scientific and technological products are getting higher and higher, and the use of energy is also increasing day by day. As energy consumption continues to increase, people have begun to vigorously develop clean energy, such as hydropower, wind power and solar energy. However, these clean energy sources are difficult to be used directly, and it is necessary to find suitable energy storage and conversion equipment. Secondary batteries are considered to be excellent energy storage devices. They can reversibly convert electrical energy and chemical energy through internal reversible chemical reactions. Lithium-ion batteries are currently the most widely used secondary batteries. They have the advantages of high energy density and long cycle life, and are widely studied. At present, graphite materials are commonly used as the negative electrode of lithium-ion batteries in business, which have the advantages of good cycle stability and high safety performance. However, the theoretical specific capacity is only 372mAh g -1 , gradually unable to meet people's needs, it is necessary to find new negative electrode materials for further development. Silicon negative electrode is considered to be a new negative electrode material that is expected to replace graphite. This is because the discharge capacity of silicon is as high as 4200mAhg when fully discharged. -1 , which is 11 times that of graphite negative electrode, and has the advantages of abundant reserves and low discharge platform. However, silicon negative electrode also has some problems:
[0003] 1. The lithium insertion process of silicon is an alloying reaction. Huge volume changes will occur during the lithium insertion and removal process. The volume expansion rate is as high as 300%, which is prone to electrode pulverization and active material falling off from the current collector.
[0004] 2. Silicon is a semiconductor material with poor conductivity;
[0005] 3. During the cycle, repeated volume changes of the material will cause the SEI film on the electrode interface to rupture, and SEI will continue to be generated, consuming lithium ions in the solution, resulting in low coulombic efficiency of the battery and poor cycle performance.
[0006] In response to the above problems, the current solutions are mainly: silicon nano-crystallization, silicon-oxygen anode, silicon-metal composite and silicon-carbon composite. 1. Silicon nano-crystallization is to reduce the size of silicon particles and avoid the crushing of silicon particles to reduce the impact of volume expansion. However, there are still problems such as poor conductivity and poor cycle stability; 2. Silicon-oxygen anode is that when silicon oxide reacts with lithium during the first lithiation, it will generate irreversible inert components such as lithium silicate and lithium oxide, thereby alleviating the volume change of silicon. However, the degree of oxidation of silicon-oxygen anode has a great influence on the performance of the electrode, the degree of oxidation is not easy to control, and it has the disadvantages of complex production process, high production cost and low first-cycle coulomb efficiency; 3. Silicon-metal composite anode is to improve the conductivity of the electrode by adding highly conductive metals, so as to improve the discharge specific capacity of the electrode. However, it has the disadvantages of high cost and poor cycle performance; 4. Silicon-carbon composite is to improve the conductivity of the electrode by introducing carbon materials, and synthesize carbon materials with different structures at the same time to alleviate the volume expansion of silicon, thereby improving the electrochemical performance of the electrode. Silicon-carbon composites have mature processes and have advantages such as high first-cycle coulombic efficiency and high specific capacity, which are more advantageous than other strategies. At present, the preparation methods of silicon-carbon composite materials include: magnesium thermal reduction method, chemical vapor deposition, mechanical grinding method, sol-gel method and electrospinning method. Among them, electrospinning method has the advantages of simple synthesis process, green and pollution-free, and large-scale production, and is widely used in the field of batteries. Moreover, electrospinning method can be combined with other methods to design silicon carbon fibers with different structures. For example, Zeng et al. encapsulated silicon in zeolite imidazole framework material (ZIF-8), and then spun it with polyacrylonitrile to obtain N-doped porous silicon carbon nanofibers. The porous structure can reduce the impact of volume change, and carbon fiber can improve the conductivity of the material, synergistically improving the electrochemical performance of the battery (Journal of Energy Chemistry, 2021, 54: 727-735). Pei et al. synthesized composite silicon-carbon nanofibers with core-shell structure by coaxial spinning, with Si and polyvinyl alcohol (PVA) as the core layer and polyacrylonitrile as the shell layer. The polyacrylonitrile shell provides structural protection for silicon, the internal PVA thin layer improves the conductivity of silicon, and together with the external polyacrylonitrile, it forms a three-dimensional conductive network to promote charge transfer during the charge and discharge process (Carbon, 2023, 203: 436-444). The core-shell structure can alleviate the volume expansion of silicon to a certain extent, but its structure may be destroyed as the cycle proceeds, and the cycle performance will drop significantly; while the porous structure has more pores, the electrolyte infiltration is serious, the side reactions between the electrode and the electrolyte increase, and the coulomb efficiency is low. In addition, a suitable carbon source is also particularly important for improving the performance of silicon-carbon composite materials. For example, Li et al. coated a layer of phenolic resin carbon (RF) on the surface of nano-silicon particles by hydrothermal method, and made silicon and carbon layer in close contact by hot pressing; then coated a layer of coal tar (CTP) by solution evaporation method, and hot pressed again to make the particles dense, and finally carbonized at high temperature to obtain D-Si@RF-CTP nanoparticles with core-shell structure.The compact outer layer can reduce the side reaction of silicon with the electrolyte, the porous interior can accommodate the volume change, and the mechanical and chemical synergistic effect between the two structurally different carbon layers can endow the resulting particles with high densification and excellent resistance to particle fracture at 500 mA g. --1 After 60 cycles under the same conditions, the capacity retention rate was 89.4%, which has excellent cycle stability (Energy Storage Materials, 2023, 56: 40-49.). However, its synthesis process is complicated, and hot pressing is required during the synthesis process to increase the compaction density of the material.
[0007] In summary, the present invention aims at the deficiencies of the prior art and designs a soft / hard carbon composite carbon nanotube film coated with silicon nanoparticles having a yolk shell structure, and improves the electrochemical performance of the material through the synergistic effect of a reasonable structure and a suitable carbon source. Summary of the invention
[0008] The purpose of the present invention is to overcome the shortcomings of the prior art, and to synthesize a silicon-coated soft / hard carbon composite carbon nanotube (Si@SHC-CNT) film with a yolk shell structure by coaxial static spinning and carbonization process using mesophase pitch as a soft carbon precursor and polyacrylonitrile as a hard carbon precursor. The internal cavity and the outer composite carbon shell are used to alleviate the volume expansion of silicon, and the characteristics of hard carbon and soft carbon are used to synergistically accelerate the electrode reaction rate, so that the Si@SHC-CNT film exhibits excellent electrochemical performance when used as the negative electrode of a lithium-ion battery.
[0009] The present invention is achieved through the following technical solutions.
[0010] A method for preparing a silicon-coated soft / hard carbon composite carbon nanotube film by coaxial static spinning comprises the following steps:
[0011] (1) adding polyacrylonitrile (PAN) and mesophase pitch (MP) to a mixed solution of N,N-dimethylformamide and tetrahydrofuran, and stirring to form a shell layer precursor spinning solution; adding silicon nanoparticles and styrene-acrylonitrile copolymer (SAN) to N,N-dimethylformamide, and stirring to form a core layer precursor spinning solution;
[0012] (2) The two precursor spinning solutions in step (1) are subjected to a coaxial electrospinning method to obtain a fiber membrane precursor, specifically:
[0013] The two precursor spinning solutions are added into two syringes respectively. The syringe containing the core layer precursor spinning solution is directly connected to the inner cavity of the coaxial spinning needle. The syringe containing the shell layer precursor spinning solution is connected to the side chamber of the coaxial spinning needle via an adapter and a rubber hose. The two precursor spinning solutions are ejected simultaneously and converge at the front end of the coaxial spinning needle to form a fiber membrane precursor on the collector.
[0014] (3) The fiber membrane precursor obtained in step (2) is pre-oxidized in an air atmosphere, and the obtained pre-oxidation product is further heat-treated in an inert atmosphere to obtain a silicon-coated soft / hard carbon composite carbon nanotube film.
[0015] Preferably, in step (1), the average molecular weight of polyacrylonitrile is 85,000-150,000, and the average molecular weight of styrene-acrylonitrile copolymer is 165,000-185,000.
[0016] Preferably, in step (1), the concentration of polyacrylonitrile in the shell precursor spinning solution is 10-12wt%; the concentration of mesophase pitch is 1-3wt%; and the mass ratio of N,N-dimethylformamide to tetrahydrofuran is equal to the mass ratio of polyacrylonitrile to mesophase pitch.
[0017] Preferably, in step (1), the content of silicon nanoparticles in the core layer precursor spinning solution is 3-6 wt %; and the concentration of styrene-acrylonitrile copolymer is 20-24 wt %.
[0018] Preferably, in step (2), the coaxial electrospinning conditions are: the flow rate ratio of the core layer precursor spinning solution to the shell layer precursor spinning solution is 1:(1.5-3), the spinning distance is maintained at 10-20 cm, the spinning voltage is 10-20 kV, the spinning temperature is 40-50°C, and the humidity is 40-50%.
[0019] Preferably, in step (3), the pre-oxidation temperature is 250-280°C, the heating rate is 1-5°C / min, and the holding time is 2-3h.
[0020] Preferably, in step (3), the inert atmosphere is argon, and the gas flow rate is 30-60 ml / min.
[0021] Preferably, in step (3), the heat treatment is a high-temperature carbonization process, the temperature is 700-900°C, the heating rate is 2-5°C / min, and the insulation time is 1-3h.
[0022] The silicon-coated soft / hard carbon composite carbon nanotube film prepared by the above-mentioned preparation method has a yolk shell structure, the internal cavity can alleviate the volume expansion of silicon, and the outer carbon shell coats the silicon, reducing the occurrence of side reactions between silicon and the electrolyte; at the same time, the outer carbon shell improves the electron and ion transmission rate of the material, so that when the silicon-coated soft / hard carbon composite carbon nanotube film is used as a negative electrode material for a lithium-ion battery, the battery exhibits a high discharge specific capacity and a long cycle life.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] (1) The preparation process of the present invention is simple, environmentally friendly, safe and controllable. The prepared film is flexible and can be directly used as the negative electrode of a lithium-ion battery after cutting, without the need for a binder and a current collector, thereby improving the energy density of the battery.
[0025] (2) The Si@SHC-CNT film with yolk shell structure prepared by the present invention is a three-dimensional conductive network formed by staggered stacking of carbon nanotubes of uniform size, which is conducive to the transmission of electrons. In addition, the hard carbon produced by the decomposition of polyacrylonitrile has a larger interlayer spacing, which is conducive to the transmission of lithium ions; at the same time, the soft carbon produced by the decomposition of the intermediate phase asphalt introduces more carbon layers with small interlayer spacing. These carbon layers are relatively more orderly, which can reduce the electron transmission resistance and accelerate the electron transmission rate; the synergistic effect of the soft / hard carbon composite carbon shell is conducive to accelerating the electrode reaction rate and improving the electrode electrochemical performance. The soft / hard carbon composite carbon shell can alleviate the volume expansion of silicon to a certain extent and maintain the stability of the carbon nanotube structure; and the internal cavity formed by the complete decomposition of SAN can also effectively alleviate the huge volume change of silicon particles during the cycle, which is conducive to improving the electrode cycle stability.
[0026] In short, the present invention combines coaxial electrospinning and high-temperature carbonization processes to synthesize a soft / hard carbon composite carbon nanotube film with silicon as the core, a soft / hard carbon composite carbon layer as the shell, and an ovoid shell structure with a cavity inside. The synthesis process of the present invention is simple, and the process is safe and controllable. The volume expansion of silicon is alleviated by designing the internal cavity, and the outer carbon shell better wraps the silicon particles, which can reduce the occurrence of side reactions. At the same time, the outer soft / hard carbon composite carbon shell can accelerate the transmission of electrons and ions. When the silicon-coated soft / hard carbon composite carbon nanotube film prepared by the present invention is used as the negative electrode of a lithium-ion battery, the battery exhibits a high discharge specific capacity and a long cycle life, which effectively solves the problems of poor cycle performance and low electrode capacity of the current flexible material silicon-carbon electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 a and Figure 1 b in the figure are scanning electron microscope photographs of the fiber membrane precursor prepared in Example 1 of the present invention at different magnifications.
[0028] Figure 2 a and Figure 2 b in the figure are scanning electron microscope photos of Si@SHC15%-CNT prepared in Example 1 of the present invention at different magnifications.
[0029] Figure 3 This is a transmission electron microscope photograph of Si@SHC15%-CNT prepared in Example 1 of the present invention.
[0030] Figure 4 a and Figure 4b in the figure are scanning electron microscope photos of Si@SHC30%-CNT prepared in comparative example 3 of the present invention at different magnifications.
[0031] Figure 5 This is the XRD pattern of Si@SHC15%-CNT prepared in Example 1 of the present invention.
[0032] Figure 6 The graph shows the cycle performance of Si@HC-CNT prepared in Comparative Example 2 of the present invention, Si@SHC15%-CNT prepared in Example 1, and Si@SHC30%-CNT films prepared in Comparative Example 3 as negative electrode materials for lithium-ion batteries. DETAILED DESCRIPTION
[0033] In order to better understand the present invention, the specific implementation of the present invention is further described in detail below in combination with embodiments, comparative examples and drawings, but the implementation mode of the present invention is not limited thereto.
[0034] Example 1
[0035] 1) 0.70 g of polyacrylonitrile and 0.14 g of mesophase pitch were dissolved in a mixed solution of 1.02 g of tetrahydrofuran and 5.10 g of N,N-dimethylformamide, and stirred to form a shell layer precursor spinning solution, wherein the concentration of the mesophase pitch was 2 wt %; 0.18 g of silicon nanoparticles and 0.72 g of styrene-acrylonitrile copolymer were dissolved in 2.1 g of N,N-dimethylformamide, and stirred to form a core layer precursor spinning solution.
[0036] 2) Coaxial electrospinning: The two precursor spinning solutions prepared in step 1) are respectively loaded into the syringe, the shell layer precursor spinning solution is connected to the side chamber of the coaxial static spinning needle through an adapter, a rubber hose and a catheter, and the core layer precursor spinning solution is directly connected to the inner cavity of the coaxial static spinning needle. The distance between the spinning needle and the collector is 16cm, and the spinning voltage is 17kV. Under the conditions of temperature of 50°C and humidity of 50%, the flow rate of the shell layer spinning solution is 1.8ml / h, and the flow rate of the core layer spinning solution is 0.9ml / h for coaxial static spinning, forming a fiber membrane precursor on the collector.
[0037] 3) The fiber film precursor was pre-oxidized in air, heated to 250°C at 1°C / min, and kept at 250°C for 2h; the pre-oxidized product was placed in a sealed tube, heated to 800°C at 2°C / min under Ar gas protection, and kept at 800°C for 2h. After natural cooling, a soft / hard carbon composite carbon nanotube (Si@SHC15%-CNT, 15% refers to the soft carbon mass ratio) film coated with silicon nanoparticles was obtained.
[0038] Figure 1 a and Figure 1b in the figure are scanning electron microscope photos of the fiber membrane precursor prepared in this example at different magnifications. It can be seen that the obtained fiber membrane precursor is composed of one-dimensional fibers of uniform size arranged in a staggered manner. Figure 2 a and Figure 2 b in the figure are scanning electron microscope photos of Si@SHC15%-CNT prepared in this example at different magnifications. It can be seen that after high-temperature annealing, SAN is completely decomposed and voids are formed inside the fiber, which is beneficial to alleviate the volume expansion of silicon during the cycle. Figure 3 This is the TEM photo of Si@SHC15%-CNT prepared in this embodiment. It can be seen that the prepared fiber has a yolk-shell structure, with silicon particles inside and an outer layer of a composite carbon layer formed by the decomposition of PAN and MP. The size of the internal silicon particles is about 100nm, and the thickness of the shell carbon layer is about 100-150nm; the outer carbon layer completely wraps the silicon particles and has a cavity inside, thus forming a silicon-carbon composite nanotube with a yolk-shell structure. Figure 5 This is the XRD pattern of Si@SHC15%-CNT prepared in this example. After comparing it with the standard PDF card, it is confirmed that the silicon particles are successfully loaded therein.
[0039] Example 2
[0040] A method for preparing a silicon-coated soft / hard carbon composite carbon nanotube film by coaxial static spinning is basically the same as Example 1, except that: 0.77g of polyacrylonitrile and 0.07g of mesophase asphalt are dissolved in a mixed solution of 0.51g of tetrahydrofuran and 5.61g of N,N-dimethylformamide, and stirred evenly to form a shell precursor spinning solution, and the concentration of the mesophase asphalt is 1wt%.
[0041] Example 3
[0042] A method for preparing a silicon-coated soft / hard carbon composite carbon nanotube film by coaxial static spinning is basically the same as Example 1, except that: 0.63g of polyacrylonitrile and 0.21g of mesophase asphalt are dissolved in a mixed solution of 1.54g of tetrahydrofuran and 4.62g of N,N-dimethylformamide, and stirred evenly to form a shell precursor spinning solution, and the concentration of the mesophase asphalt is 3wt%.
[0043] Comparative Example 1
[0044] 1) 0.5 g of polyacrylonitrile was dissolved in 4.5 g of N, N-dimethylformamide and stirred to form a shell layer precursor spinning solution; 0.48 g of styrene-acrylonitrile copolymer was dissolved in 1.52 g of N, N-dimethylformamide and stirred to form a core layer precursor spinning solution.
[0045] 2) Coaxial electrospinning: The two precursor spinning solutions prepared in step 1) are respectively loaded into the syringe, the shell layer precursor spinning solution is connected to the side chamber of the coaxial static spinning needle through an adapter, a rubber hose and a catheter, and the core layer precursor spinning solution is directly connected to the inner cavity of the coaxial static spinning needle. The distance between the spinning needle and the collector is 16cm, and the spinning voltage is 18kV. Under the conditions of temperature of 50°C and humidity of 50%, the flow rate of the shell layer spinning solution is 1.8ml / h, and the flow rate of the core layer spinning solution is 0.9ml / h for coaxial static spinning, forming a fiber membrane precursor on the collector.
[0046] 3) Pre-oxidize the fiber film precursor in air, heat it up to 250°C at 1°C / min, and keep it at 250°C for 2h; place the pre-oxidized product in a sealed tube, heat it up to 800°C at 2°C / min under Ar gas protection, and keep it at 800°C for 2h. After completion, cool it naturally to obtain a hard carbon nanotube (HC-CNT) film.
[0047] Comparative Example 2
[0048] 1) 0.84 g of polyacrylonitrile was dissolved in 6.16 g of N,N-dimethylformamide and stirred to form a shell layer precursor spinning solution; 0.18 g of silicon nanoparticles and 0.72 g of styrene-acrylonitrile copolymer were dissolved in 2.1 g of N,N-dimethylformamide and stirred to form a core layer precursor spinning solution.
[0049] 2) Coaxial electrospinning: The two precursor spinning solutions prepared in step 1) are respectively loaded into the syringe, the shell layer precursor spinning solution is connected to the side chamber of the coaxial static spinning needle through an adapter, a rubber hose and a catheter, and the core layer precursor spinning solution is directly connected to the inner cavity of the coaxial static spinning needle. The distance between the spinning needle and the collector is 16cm, and the spinning voltage is 17kV. Under the conditions of temperature of 50°C and humidity of 50%, the flow rate of the shell layer spinning solution is 1.8ml / h, and the flow rate of the core layer spinning solution is 0.9ml / h for coaxial static spinning, forming a fiber membrane precursor on the collector.
[0050] 3) Pre-oxidize the fiber film precursor in air, heat it up to 250°C at 1°C / min, and keep it at 250°C for 2h; place the pre-oxidized product in a sealed tube, heat it up to 800°C at 2°C / min under Ar gas protection, and keep it at 800°C for 2h. After cooling naturally, a silicon-coated hard carbon nanotube (Si@HC-CNT) film can be obtained.
[0051] Comparative Example 3
[0052] 1) 0.56 g of polyacrylonitrile and 0.28 g of mesophase pitch were dissolved in a mixed solution of 2.05 g of tetrahydrofuran and 4.10 g of N,N-dimethylformamide, and stirred to form a shell layer precursor spinning solution, wherein the concentration of the mesophase pitch was 4 wt %; 0.18 g of silicon nanoparticles and 0.72 g of styrene-acrylonitrile copolymer were dissolved in 2.1 g of N,N-dimethylformamide, and stirred to form a core layer precursor spinning solution.
[0053] 2) Coaxial electrospinning: The two precursor spinning solutions prepared in step 1) are respectively loaded into the syringe, the shell layer precursor spinning solution is connected to the side chamber of the coaxial static spinning needle through an adapter, a rubber hose and a catheter, and the core layer precursor spinning solution is directly connected to the inner cavity of the coaxial static spinning needle. The distance between the spinning needle and the collector is 16cm, and the spinning voltage is 17kV. Under the conditions of temperature of 50°C and humidity of 50%, the flow rate of the shell layer spinning solution is 1.8ml / h, and the flow rate of the core layer spinning solution is 0.9ml / h for coaxial static spinning, forming a fiber membrane precursor on the collector.
[0054] 3) Pre-oxidize the fiber film precursor in air, heat it up to 250°C at 1°C / min, and keep it at 250°C for 2h; place the pre-oxidized product in a sealed tube, heat it up to 800°C at 2°C / min under Ar gas protection, and keep it at 800°C for 2h. After cooling naturally, a silicon-coated soft / hard carbon composite carbon nanotube (Si@SHC30%-CNT, 30% refers to the soft carbon mass ratio) film can be obtained.
[0055] Figure 4 a and Figure 4 Figures b in the figure are scanning electron microscope photos of Si@SHC30%-CNT prepared in this comparative example at different magnifications. It can be seen that after high-temperature annealing, the asphalt and silicon agglomerate, the fiber structure is destroyed, more gaps appear, and more silicon is exposed on the surface, thereby increasing the side reactions between the electrode and the electrolyte and significantly reducing the electrode cycle performance.
[0056] Application Example 1
[0057] The Si@HC-CNT film obtained in Comparative Example 2 was applied to the negative electrode of a lithium-ion battery. Metal lithium was used as the counter electrode, Si@HC-CNT film was used as the negative electrode, and 1M LiPF 6 EC:DEC:DMC=1:1:1 Vol%+5% FEC solution was used as the electrolyte, and Celgard 2500 was used as the separator. The battery was assembled in a glove box filled with Ar gas.
[0058] The above assembled battery was subjected to constant current charge and discharge test on the Xinwei electrochemical workstation. The test voltage range was 0.01-1.6V, and the constant current charge and discharge test current density was 0.4A g-1 , the active substances are calculated based on the total mass of the film.
[0059] Application Example 2
[0060] The Si@SHC15%-CNT film obtained in Example 1 was applied to the negative electrode of a lithium-ion battery. Metal lithium was used as the counter electrode, Si@SHC15%-CNT film was used as the negative electrode, and 1M LiPF 6 EC:DEC:DMC=1:1:1 Vol%+5% FEC solution was used as the electrolyte, and Celgard 2500 was used as the separator. The battery was assembled in a glove box filled with Ar gas.
[0061] The assembled battery was subjected to constant current charge and discharge test on a Xinwei electrochemical workstation. The test voltage range was 0.01-1.6V and the constant current charge and discharge test current density was 0.4A g -1 , the active substances are calculated based on the total mass of the film.
[0062] Application Example 3
[0063] The Si@SHC30%-CNT film obtained in Comparative Example 3 was applied to the negative electrode of a lithium-ion battery. Metal lithium was used as the counter electrode, Si@SHC30%-CNT film was used as the negative electrode, and 1M LiPF 6 EC:DEC:DMC=1:1:1 Vol%+5% FEC solution was used as the electrolyte, and Celgard 2500 was used as the separator. The battery was assembled in a glove box filled with Ar gas.
[0064] The assembled battery was subjected to constant current charge and discharge test on a Xinwei electrochemical workstation. The test voltage range was 0.01-1.6V and the constant current charge and discharge test current density was 0.4A g -1 , the active substances are calculated based on the total mass of the film.
[0065] Figure 6 The following is a comparison of the cycling performance of Si@HC-CNT in Application Example 1, Si@SHC15%-CNT in Application Example 2, and Si@SHC30%-CNT in Application Example 3 as negative electrode materials for lithium-ion batteries. As can be seen from the figure, at 0.4A g -1 At a current density of 1.34 W, the first cycle discharge capacity of Si@SHC15%-CNT electrode is 1331 mAh g -1 , Coulomb efficiency is 73%; the discharge capacity is higher than that of Si@HC-CNT electrode, because the addition of mesophase pitch introduces more ordered carbon layers, accelerates the transmission of electrons, makes the active substances fully react, and has a higher discharge capacity. After 80 cycles, Si@SHC15%-CNT electrode still has 964mAh g-1 The high discharge specific capacity, except for the first cycle, the capacity retention rate is as high as 87.6%. This is because SAN is completely decomposed, and a cavity is formed inside the fiber, which can effectively alleviate the volume expansion of silicon. The soft / hard carbon composite carbon layer formed by the outer layer PAN and the intermediate phase asphalt has a certain structural stability, which makes the electrode material have good cycle stability. Although the Si@SHC30%-CNT electrode has a higher initial discharge specific capacity, due to excessive addition of asphalt, the asphalt softens and agglomerates with silicon during the carbonization process, the yolk shell structure of the fiber is destroyed, part of the silicon particles are exposed, and the side reaction between silicon and the electrolyte increases, resulting in a significant decrease in the electrode cycle stability. Therefore, the method of improving the electrochemical properties of the material by the synergistic effect of reasonable structural design and suitable carbon source in the present invention is effective, and the Si@SHC15%-CNT electrode has the best cycle performance.
[0066] The above embodiments are used to illustrate the present invention, and the implementation methods of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a silicon-coated soft / hard carbon composite carbon nanotube film by coaxial static spinning, characterized in that: The following steps are involved: (1) adding polyacrylonitrile and mesophase pitch to a mixed solution of N,N-dimethylformamide and tetrahydrofuran, and stirring to form a shell layer precursor spinning solution; adding silicon nanoparticles and styrene-acrylonitrile copolymer to N,N-dimethylformamide, and stirring to form a core layer precursor spinning solution; (2) The two precursor spinning solutions in step (1) are subjected to a coaxial electrospinning method to obtain a fiber membrane precursor, specifically: The two precursor spinning solutions are added into two syringes respectively. The syringe containing the core layer precursor spinning solution is directly connected to the inner cavity of the coaxial spinning needle. The syringe containing the shell layer precursor spinning solution is connected to the side chamber of the coaxial spinning needle via an adapter and a rubber hose. The two precursor spinning solutions are ejected simultaneously and converge at the front end of the coaxial spinning needle to form a fiber membrane precursor on the collector. (3) The fiber membrane precursor obtained in step (2) is pre-oxidized in an air atmosphere, and the obtained pre-oxidation product is further heat-treated in an inert atmosphere to obtain a silicon-coated soft / hard carbon composite carbon nanotube film.
2. The method according to claim 1, characterized in that In the step (1), the average molecular weight of polyacrylonitrile is 85,000-150,000, and the average molecular weight of styrene-acrylonitrile copolymer is 165,000-185,000.
3. The method according to claim 1, characterized in that In the step (1), the concentration of polyacrylonitrile in the shell precursor spinning solution is 10-12wt%, and the concentration of mesophase pitch is 1-3wt%; the mass ratio of N,N-dimethylformamide to tetrahydrofuran is equal to the mass ratio of polyacrylonitrile to mesophase pitch.
4. The method according to claim 1, characterized in that: In the step (1), the content of silicon nanoparticles in the core layer precursor spinning solution is 3-6wt%, and the concentration of styrene-acrylonitrile copolymer is 20-24wt%.
5. The method according to claim 1, characterized in that In the step (2), the coaxial electrospinning conditions are: the flow rate ratio of the core layer precursor spinning solution to the shell layer precursor spinning solution is 1:(1.5-3), the spinning distance is maintained at 10-20 cm, the spinning voltage is 10-20 kV, the spinning temperature is 40-50° C., and the humidity is 40-50%.
6. The method according to claim 1, characterized in that In the step (3), the pre-oxidation temperature is 250-280° C., the heating rate is 1-5° C. / min, and the holding time is 2-3 h.
7. The method according to claim 1, characterized in that In the step (3), the inert atmosphere is argon gas, and the gas flow rate is 30-60 ml / min.
8. The method according to claim 1, characterized in that In the step (3), the heat treatment is a high-temperature carbonization process, the temperature is 700-900°C, the heating rate is 2-5°C / min, and the insulation time is 1-3h.
9. A silicon-coated soft / hard carbon composite carbon nanotube film prepared by the method according to any one of claims 1 to 8, characterized in that: The membrane has a yolk-shell structure.
10. Use of the silicon-coated soft / hard carbon composite carbon nanotube film according to claim 9 in the negative electrode of a lithium-ion battery.
Citation Information
Patent Citations
Core-shell structure silicon / carbon fiber flexible composite electrode material and preparation method thereof, and application of core-shell structure silicon / carbon fiber flexible composite electrode material
CN110112405A
Lithium ion self-supporting silicon-carbon composite nanofiber negative electrode material and preparation method and application thereof
CN116516522A
Silicon carbon fiber material, preparation method and application thereof, and battery
CN117758394A
Tied Arch Wale Structure With Increased Horizontal Resistance
KR1020250154698A
Manufacturing method of lithium-ion battery negative-electrode material effectively buffering volume change effect of silicon
WO2018032975A1
Cited By
High-performance porous soft and hard carbon fiber negative electrode material for lithium ion battery and preparation method of high-performance porous soft and hard carbon fiber negative electrode material