Dipping solution for fiber skeleton material
By using phenolic bonding resin and sulfur-containing and active proton compounds in the impregnation solution of fiber skeleton materials to form hydrogen bonds and chemical bonds, the problem of insufficient adhesion between fiber skeleton materials and rubber in the prior art is solved, and high efficiency is achieved Increased adhesion and reduced energy consumption.
Patent Information
- Application Number
- CN202310515311.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
The existing RFL impregnation system has shortcomings in improving the adhesion between fiber skeleton materials and rubber, especially the problem of decreasing adhesion after long-term use and heat-absorbing. In addition, the traditional two-bath impregnation method has high energy consumption, so seeking a one-bath Method impregnating formula to reduce energy consumption and improve adhesion.
Using a dipping solution including phenolic binder resin, latex and sulfur-containing and active proton compounds, react with phenolic resin and rubber through hydrogen bonds and chemical bonds to improve the working strength of the dipping layer and rubber, and in a bath or two It is used in bath immersion method to reduce energy consumption.
The effect strength between the impregnated adhesive resin and latex and rubber is improved, the overall adhesion is enhanced, the synthesis process is simplified, the stability and production efficiency are improved, the production cost is reduced, and the use of toxic substances is avoided.
Smart Images

Figure BDA0004218875330000031 
Figure BDA0004218875330000032 
Figure BDA0004218875330000033
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of dipping solutions, and in particular relates to a dipping solution for a fiber skeleton material. Background Art
[0002] Fiber skeleton materials are mainly used in rubber products to carry loads and maintain the dimensional stability of products. Their adhesion to rubber plays a decisive role in the performance and service life of rubber products. Its most common application scenarios include conveyor belts, tires, hoses, etc. Common skeleton materials include metal, cellulose, nylon and polyester.
[0003] For polymer skeleton materials such as polyester / nylon, it is necessary to make a dipping layer through dipping treatment to improve the adhesion with rubber. The existing mainstream dipping is mostly RFL dipping system, in which R is resorcinol, F is formaldehyde, and L is latex, that is, a composite dipping emulsion of latex wrapped in phenolic resin formed by condensation of resorcinol and formaldehyde. The RFL system is mainly combined with the fiber through the intermolecular force of RF, and cross-linked with the rubber through the co-vulcanization of latex. In recent years, with the development of skeleton material technology and the advancement of tire technology, the fine denier / lightweight of skeleton materials has become a trend. Fine denier fibers bear the same mechanical force as the original coarse denier fibers, so it brings higher requirements for the adhesion of the dipping layer. During the use of tires, the adhesion, especially the adhesion after heat aging during long-term use, has also put forward higher and higher requirements. On the other hand, the existing polyester dipping usually adopts two-bath dipping, and the first bath containing blocked isocyanate and epoxy components plays a role in enhancing the adhesion between polyethylene glycol terephthalate (PET) and RFL. However, this method has the disadvantage of relatively high energy consumption. The industry has been trying to find a one-bath dipping formula for polyester. If you want to add an additive to the RFL dipping solution that helps to bond with PET, you must enhance the adhesion of the original RFL component to the rubber to ensure that the addition of new additives does not have a negative impact on the adhesion of the RFL-rubber interface.
[0004] Patents under application numbers CN 2022111567246 and CN20221156741X mention the use of some disulfides containing active functional groups, reacting with disulfides containing epoxy / siloxane groups and other groups with the dipping adhesive resin (RF or non-RF) system, and co-vulcanizing with rubber and latex to form additional chemical bonds at the dipping-rubber interface, thereby increasing the adhesion. However, the stability of the active compounds in this application is relatively low, and hydrolysis / polymerization and other reactions are prone to occur during long-term storage, causing adverse interference to subsequent applications. This has affected the implementation of the technology to a certain extent. The patent with application number CN 2022111567180 mentions the use of disulfides containing functional groups such as hydroxyl groups to enhance the adhesion of non-RF dipping systems, but the overall physical properties of this type of formula are still somewhat different from those of the RFL dipping system, and it will take some time to promote its application.
[0005] Therefore, it is urgent to find a method that can effectively improve the adhesion of the RFL dipping system. Summary of the invention
[0006] In view of the above-mentioned shortcomings or deficiencies of the prior art, the technical problem to be solved by the present application is to provide a dipping solution for a fiber skeleton material.
[0007] To solve the above technical problems, this application is implemented through the following technical solutions:
[0008] The present application proposes a dipping solution for a fiber skeleton material, comprising: a first-bath dipping solution suitable for a one-bath dipping method or a second dipping solution suitable for a two-bath dipping method; the first-bath dipping solution has a solid content of 8% to 45%, and its dry weight includes: 15% to 70% of a phenolic adhesive resin, 20 to 70% of a latex, and 3% to 20% of a sulfur-containing and active proton compound; the second dipping solution has a solid content of 8% to 45%, and its dry weight includes: 10% to 60% of a phenolic adhesive resin, 30 to 85% of a latex, and 3% to 20% of a sulfur-containing and active proton compound.
[0009] Furthermore, the solid content of the one-bath dipping solution is 15% to 35%, and its dry weight includes: 30% to 70% of phenolic adhesive resin, 20% to 60% of latex and 5% to 15% of sulfur-containing and active proton compounds.
[0010] Furthermore, the solid content of the second dipping solution is 15% to 35%, and its dry weight includes: 10% to 35% of phenolic adhesive resin, 50% to 85% of latex and 5% to 15% of sulfur-containing and active proton compounds.
[0011] Furthermore, the one-bath dipping solution and / or the second dipping solution further include: auxiliary agents with a total proportion less than or equal to 10%; the auxiliary agents include: pH regulators, surfactants, film-forming agents, antioxidants and / or cross-linking catalysts.
[0012] Further, the sulfur-containing and active proton compound includes: a first compound, a second compound and / or a third compound;
[0013] The general structural formula of the first compound is as follows:
[0014]
[0015] In the above formula, b is a positive integer, and the sum of a and c is greater than or equal to 1;
[0016] The general structural formula of the second compound is as follows:
[0017]
[0018] In the above formula, e is a positive integer, and the sum of d and f is greater than or equal to 1;
[0019] The general structural formula of the third compound is as follows:
[0020]
[0021] In the above formula, h is a positive integer, and the sum of g and i is greater than or equal to 1.
[0022] Further, R and R' each include: an unsubstituted or branched substituted alkyl chain, or an unsubstituted or branched substituted alkenyl chain, or an unsubstituted or branched substituted alkynyl chain, or an unsubstituted or branched substituted heterochain, or an unsubstituted or branched substituted cycloalkyl chain, or an unsubstituted or branched substituted cyclic heterochain, or an unsubstituted or branched substituted cyclic double-bond chain, or an unsubstituted or branched substituted cyclic triple-bond chain, or unsubstituted or branched substituted benzene, or an unsubstituted or branched substituted condensed ring, or an unsubstituted or branched substituted heterocycle; the heterochain is a carbon chain containing oxygen atoms, a carbon chain containing nitrogen atoms and / or a carbon chain containing sulfur atoms; the heterocycle includes: pyridine, thiophene or furan; the branched chain includes: an alkyl chain, an alkenyl chain, an alkynyl chain, a heterochain, a cycloalkyl chain, a cyclic heterochain, a cyclic double-bond chain, a cyclic triple-bond chain, benzene, a condensed ring and / or a heterocycle.
[0023] Further, R and R' each include: -(CH2) n -O(CH2CH2O) m -(CH2) n -, m is 1 to 4, n is 1 to 2; or, C1 to C 10Carbon chain; or, an aromatic core structure having 1 to 2 aromatic rings.
[0024] Furthermore, when a, d or g is zero, R also includes: an independent hydrogen atom; when c, f or i is zero, R' also includes: an independent hydrogen atom.
[0025] Furthermore, the alkyl chain, the alkenyl chain, the alkynyl chain, the heterochain, the cycloalkyl chain, the cyclic heterochain, the cyclic double-bond chain, the cyclic triple-bond chain, the benzene, the condensed ring and the heterocycle have substituents, and the substituents include: aromatic groups, alkoxy groups, halogen groups, ester groups and / or amide groups.
[0026] Furthermore, when the number of carbon atoms of R is greater than or equal to 7, the mass fraction of heteroatoms is greater than or equal to 15% to ensure the hydrophilicity of R.
[0027] Furthermore, the phenolic adhesive resin is a pre-condensed resin formed by condensation of phenols and aldehydes under alkaline conditions; the phenols include: resorcinol, phloroglucinol and / or phenol; the aldehydes include: formaldehyde, acetaldehyde, butyraldehyde and / or terephthalaldehyde; the amount of the aldehydes added in the condensation process is 1.0 to 2.0 times the amount of the phenols added.
[0028] Furthermore, the latex includes: styrene-butadiene latex, butadiene-pyridine latex, nitrile-butadiene latex, polybutadiene latex and / or natural latex.
[0029] Furthermore, the styrene-butadiene latex includes: styrene-butadiene latex terminated and / or grafted with carboxyl, hydroxyl, acid anhydride; the butylpyrrolidone latex includes: butylpyrrolidone latex terminated and / or grafted with carboxyl, hydroxyl, acid anhydride; the nitrile latex includes: nitrile latex terminated and / or grafted with carboxyl, hydroxyl, acid anhydride; the polybutadiene latex includes: polybutadiene latex terminated and / or grafted with carboxyl, hydroxyl, acid anhydride; the natural latex includes: natural latex terminated and / or grafted with carboxyl, hydroxyl, acid anhydride.
[0030] Compared with the prior art, this application has the following technical effects:
[0031] The sulfur-containing and active proton compounds in the dipping solution of the present application can form hydrogen bonds or chemical bonds with the phenolic adhesive resin, and can also form chemical bonds with the rubber through sulfur bonds. Therefore, the present application can improve the interaction strength between the dipping adhesive resin and the latex and the rubber, and ultimately achieve the effect of improving the overall bonding force.
[0032] The sulfur-containing and active proton compound of the present application has a simple synthesis method, and the structure is easy to adjust. The molecular structure can be adjusted according to product requirements, which is conducive to further performance improvement and application expansion. Compared with active sulfur-containing substances containing sulfur and reactive groups, the sulfur-containing substances involved in the present application are more stable, easy to store and use, and easier to synthesize, which is conducive to industrialization.
[0033] The present application enhances the affinity between the dipping layer and the rubber layer in the phenolic dipping method, facilitates the implementation of the one-bath dipping method, helps avoid the large amount of energy consumption caused by the two-bath dipping process, effectively improves production efficiency, and reduces production costs. Of course, the present application can also be used in the second dipping of the two-bath dipping method.
[0034] Compared with other traditional RF formulas, the present invention avoids the addition of phenolic toxic and harmful substances. Compared with other one-bath dipping formulas, chemical cross-linking can be generated between the dipping glue and the rubber during the dipping process, thereby achieving a better bonding effect.
[0035] The present application has good compatibility with the preparation and use of traditional dipping solutions in terms of equipment and process, which facilitates the factory to organize production and switch between different categories. DETAILED DESCRIPTION
[0036] The present application is further described below in conjunction with the examples, but the implementation and protection of the present application are not limited thereto. It should be noted that if there are any processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. If the manufacturer of the reagents or instruments used is not indicated, they are deemed to be conventional products that can be purchased commercially.
[0037] The following reagents are used in Examples 1 to 5:
[0038] Sodium persulfide: prepare by mixing commercially available sodium sulfide nonahydrate and commercially available sodium polysulfide solution in proportion, dilute with water to make a 20% solution, stir at room temperature for more than 48 hours, and use after the polysulfide in the solution has basically reached equilibrium.
[0039] 3-Chloro-1-propanol: adamas, 98+%;
[0040] 6-Chloro-1-hexanol: Adamas, 98+%;
[0041] 3-Chloro-1,2-propanediol-Adamas, 98+%;
[0042] 3-Chloro-1-propionic acid-Adamas, 98+%;
[0043] 3-Chloro-1-propylamine hydrochloride: 99+%;
[0044] Sodium thiosulfate pentahydrate: Greagent, 99+%;
[0045] Potassium iodide: adamas, 99%;
[0046] Tert-butyl hydroperoxide: adamas, 70% aqueous solution;
[0047] Ethyl acetate: commercially available, analytical grade;
[0048] Methanol: commercially available, analytical grade;
[0049] 37% hydrochloric acid: dilute to 20%;
[0050] Sodium hydroxide: analytical grade, prepared into 20% solution for use.
[0051] This embodiment proposes a dipping solution for a fiber skeleton material, including: a one-bath dipping solution suitable for a one-bath dipping method or a second dipping solution suitable for a two-bath dipping method; the one-bath dipping solution has a solid content of 8% to 45%, and its dry weight includes: 15% to 70% of a phenolic adhesive resin, 20 to 70% of a latex, and 3% to 20% of a sulfur-containing and active proton compound; the second dipping solution has a solid content of 8% to 45%, and its dry weight includes: 10% to 60% of a phenolic adhesive resin, 30 to 85% of a latex, and 3% to 20% of a sulfur-containing and active proton compound.
[0052] The sulfur-containing and active proton compounds in the dipping solution of the present application can form hydrogen bonds or chemical bonds with the phenolic adhesive resin, and can also form chemical bonds with the rubber through sulfur bonds. Therefore, the present application can improve the interaction strength between the dipping adhesive resin and the latex and the rubber, and ultimately achieve the effect of improving the overall adhesion. The following is an example of specific embodiments.
[0053] Example 1
[0054] The sulfur-containing and active proton compound has the following chemical structure, namely compound A:
[0055]
[0056] The specific preparation process of compound A is as follows:
[0057] Weigh 47g of 3-chloro-1-propanol into a 1L round-bottom flask, add 130g of sodium thiosulfate pentahydrate, and add about 400ml of water to dissolve. When the sodium thiosulfate pentahydrate is completely dissolved, no solid remains in the reaction mixture. Add 400ml of methanol to the above mixture, seal the lid and stir the reaction at 80°C for 40 hours to obtain the intermediate Bonte salt. After the reaction, the reaction mixture is evaporated on a rotary evaporator to a total volume of about 300-400ml, washed twice with ethyl acetate, and the organic phase is discarded. At room temperature, the aqueous phase is diluted to 500ml, 0.5g of potassium iodide is added, and then 60g of tert-butyl hydroperoxide is added dropwise under stirring over 3 hours. After the reaction is completed, the reaction mixture is stirred for 2 hours, then transferred into a separatory funnel and left to stand overnight.
[0058] The reaction mixture was separated into layers, with the organic phase as the upper layer and the aqueous phase as the lower layer. The aqueous phase was washed twice with ethyl acetate, the organic phases were combined, dried with anhydrous sodium sulfate, and then evaporated in a rotary evaporator and a vacuum oven at room temperature to remove the solvent, to obtain a colorless, clear, viscous liquid, which was used directly as compound A. The liquid was shown as a mixture of disulfide and a small amount of trisulfide on the peak area normalization method (GC-MS), with no other visible impurities.
[0059] Example 2
[0060] The sulfur-containing and active proton compound has the following chemical structure, namely compound B:
[0061]
[0062] The specific preparation process of compound B is as follows:
[0063] Weigh 68.5g of 6-chloro-1-hexanol into a 1L round-bottom flask, add 130g of sodium thiosulfate pentahydrate, and add about 400ml of water to dissolve. When the sodium thiosulfate pentahydrate is completely dissolved, no solid remains in the reaction mixture. Add 400ml of methanol to the above mixture, seal the lid and react at 80°C for 40 hours to obtain the intermediate Bonte salt. After the reaction, the reaction mixture is evaporated on a rotary evaporator to a total volume of about 300-400ml, washed twice with ethyl acetate, and the organic phase is discarded. At room temperature, the aqueous phase is diluted to 500ml, 0.5g of potassium iodide is added, and then 60g of tert-butyl hydroperoxide is added dropwise over 3 hours. After the reaction is completed, the reaction mixture is stirred for 2 hours, then transferred into a separatory funnel and left to stand overnight.
[0064] The reaction mixture was separated into layers, with the organic phase as the upper layer and the aqueous phase as the lower layer. The aqueous phase was washed twice with ethyl acetate, and the organic phases were combined, dried with anhydrous sodium sulfate, and then evaporated in a rotary evaporator and a vacuum oven at room temperature to remove the solvent, obtaining a colorless, clear, viscous liquid, which condensed into a white ointment-like solid after being stored in a refrigerator at 4°C and was used directly as compound B. The liquid was shown as a mixture of monosulfide, disulfide and a small amount of trisulfide on GC-MS, with no other visible impurities.
[0065] Example 3
[0066] The sulfur-containing and active proton compound has the following chemical structure, namely compound C:
[0067]
[0068] The specific preparation process of compound C is as follows:
[0069] 55g of 3-chloro-1,2-propanediol was placed in a 250ml round-bottom flask and kept cool in a cold water bath. Using a magnetic stirrer to maintain rapid stirring, 137g of sodium persulfide solution containing 0.25mol of sodium persulfide was slowly added dropwise through a constant pressure dropping funnel within 2 hours. After stirring for 2 hours, it was dried using a rotary evaporator. 200ml of ethanol was added to the obtained paste, and ultrasonic oscillation was performed for about 10min. The particles of the paste species were all broken into fine powders, and no large particles visible to the naked eye remained. Suction filtration was used for solid-liquid separation, and the filter cake was washed 3 times with 50ml of ethanol. After combining the filtrate and the washing liquid, the ethanol was removed by rotary evaporation and drying in a vacuum oven at room temperature to obtain a colorless, clear, viscous solution, which was compound C with a yield of 86%. GC-MS was used to confirm the purity, and only disulfide and a small amount of trisulfide were found, and no other impurities were found.
[0070] Example 4
[0071] The sulfur-containing and active proton compound has the following chemical structure, namely compound D:
[0072]
[0073] The specific preparation process of compound D is as follows:
[0074] 54g of 3-chloropropionic acid was placed in a 500ml round-bottom flask, 100ml of water was added, and 100g of 20% sodium hydroxide solution was slowly added dropwise in 1 hour after sufficient stirring. 137g of sodium persulfide solution was slowly added dropwise in 2 hours to the obtained solution, and stirring was continued for 2 hours after the addition was completed, and 20% hydrochloric acid was added dropwise to neutralize until the pH was lower than 4, that is, about 110g of hydrochloric acid was consumed, and the mixture was spin-dried. 300ml of ethanol was added to the resulting paste, and then ultrasonicated and filtered, and the filter cake was washed with 2*100ml of ethanol. The filtrate was combined and spin-dried, and then fully dried at room temperature in a vacuum oven to obtain a white waxy solid. GC-MS analysis showed disulfide, a small amount of trisulfide, about 2% of 3-hydroxy-1-propionic acid and about 5% of the starting material, and no other impurities were found.
[0075] Example 5
[0076] The sulfur-containing and active proton compound has the following chemical structure, namely compound E:
[0077]
[0078] The specific preparation process of compound E is as follows:
[0079] Weigh 65 ml of 3-chloro-1-propylamine hydrochloride into a 1L round-bottom flask, add 300 ml of water to dissolve, and neutralize with sodium hydroxide to neutrality (consume about 100 g of 20% sodium hydroxide solution).
[0080] After sufficient stirring, slowly drop 100g of 20% sodium hydroxide solution in 1 hour. Slowly drop 137g of sodium persulfide solution into the obtained solution in 2 hours, continue stirring for 2 hours after the addition is completed, spin dry, add 300ml of ethanol to the resulting paste, ultrasonicate, filter, and wash the filter cake with 2*100ml of ethanol. Combine the filtrate and spin dry, then fully dry at room temperature in a vacuum oven to obtain a white waxy solid. GC-MS analysis shows disulfide and a small amount of trisulfide, but no other impurities.
[0081] The reagents used in the following Examples 6 to 33 and Comparative Examples 1 to 16 are:
[0082] Among them, latex includes:
[0083] Butylpyrrolidone latex (VP): commercially available, 40%;
[0084] Styrene butadiene latex (SBR): commercially available, 40%;
[0085] Natural rubber latex (NR): commercially available, 40%;
[0086] Resorcinol: Commercially available, 99.5%;
[0087] Formaldehyde: commercially available, 37%;
[0088] Sodium hydroxide: Adamas, analytical grade;
[0089] 25%-28% ammonia water: Adamas, analytical grade;
[0090] First bath components: DuPont D417 diluted solution with a solid content of about 3%;
[0091] Resorcinol-formaldehyde linear pre-condensation resin solution: The average molecular weight is about 300. It is formed by polycondensation of resorcinol and formaldehyde under the catalysis of 1% oxalic acid and then diluted with water. It is an amber viscous solution with a mass fraction of 50%;
[0092] Water: homemade deionized water;
[0093] PET cord: Hailide Company, 1000D.
[0094] Example 6
[0095] This embodiment is a one-bath dipping solution formulation, which is suitable for one-bath dipping of polyester. The specific addition amount is shown in Table 1.
[0096] Step 1: Prepare Liquid I. Dissolve 5 g of resorcinol in 77 g of water, add 8 g of formaldehyde, and then add 5 g of ammonia water. Stir at 25°C for 10 min, then slowly add 70 g of butyl pyrrolidone latex over 10 min, and then slowly add 35 g of styrene butadiene latex over 5 min. The total mass of the mixture is 200 g. The above product is slowly stirred at room temperature and aged for 3 days to form Liquid I.
[0097] Step 2: Prepare liquid II. Add 80g of pre-condensed RF resin in a 50% aqueous solution to 25g of ammonia water and 86g of deionized water, and stir evenly to form a uniform and stable aqueous solution. Under rapid stirring, the solution presents a brown, uniform and stable state, forming liquid II.
[0098] Step 3: Mixing the glue. After the preparation of Solution II is completed, it is immediately mixed with Solution I, and then 9 g of the compound A prepared in Example 1 is added to obtain a dipping solution.
[0099] The PET cord was dipped using a single-line dip machine. The dipping time in the dip tank was about 8 seconds. The dipped cord was dried in the first oven at 170°C and then cured in the second oven at 240°C. The residence time in both ovens was about 2 minutes. The cord tension was maintained between 4.0 and 5.0N during the dipping and drying process. The first bath formula of D417 and the second dip tank used the formula of this embodiment. The cord after drying and curing showed a color ranging from reddish brown to tan.
[0100] The CRA peel test was performed using the test method of GB / T40725-2021, and the total peel force of the five cords and the grade of the rubber covering the cord surface were recorded, represented by grades A to E. The CRA peel force of the dipped cord in this embodiment was 101.37N, and the amount of rubber attached to the peeled surface was determined to be grade A.
[0101] Example 7
[0102] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that this embodiment adds the largest amount of pre-condensed RF resin in Examples 6 to 19 of the present application. The specific amount added is shown in Table 1. After testing, the CRA peeling force of the dipped cord is 93.12N, and the amount of adhesive on the peeling surface is judged to be Class B.
[0103] Example 8
[0104] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that this embodiment adds the least amount of latex in Examples 6 to 19 of the present application. The specific amount added is shown in Table 1. After testing, the CRA peeling force of the dipped cord is 94.84N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0105] Example 9
[0106] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that this embodiment adds the least amount of sulfur-containing and active proton compounds in Examples 6 to 19 of the present application. The specific amount of addition is shown in Table 1. After testing, the CRA peeling force of the dipped cord is 81.03N, and the amount of adhesive on the peeling surface is judged to be Class B.
[0107] Example 10
[0108] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that this embodiment adds the largest amount of sulfur-containing and active proton compounds in Examples 6 to 19 of the present application. The specific amount of addition is shown in Table 1. After testing, the CRA peeling force of the dipped cord is 86.55N, and the amount of adhesive on the peeling surface is judged to be Class B.
[0109] Embodiment 11
[0110] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that compound A is replaced by compound B in this embodiment. The specific addition amount is shown in Table 1. After testing, the CRA peeling force of the dipped cord is 107.94N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0111] Example 12
[0112] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that compound A is replaced by compound C in this embodiment. The specific addition amount is shown in Table 1. After testing, the CRA peeling force of the dipped cord is 88.11N, and the amount of adhesive on the peeling surface is judged to be Class B.
[0113] Embodiment 13
[0114] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that compound A is replaced by compound D in this embodiment. The specific addition amount is shown in Table 2. After testing, the CRA peeling force of the dipped cord is 85.08N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0115] Embodiment 14
[0116] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that compound E is used to replace compound A in this embodiment. The specific addition amount is shown in Table 2. After testing, the CRA peeling force of the dipped cord is 89.72N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0117] Embodiment 15
[0118] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that in this embodiment, nylon 66 cord is used for dipping treatment. The specific addition amount is shown in Table 2. After testing, the CRA peeling force of the dipped cord is 112.05N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0119] Example 16
[0120] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that natural latex is used to replace styrene-butadiene latex in this embodiment. The specific addition amount is shown in Table 2. After testing, the CRA peeling force of the dipped cord is 95.47N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0121] Embodiment 17
[0122] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that phenol is used instead of resorcinol in this embodiment. The specific addition amount is shown in Table 2. After testing, the CRA peeling force of the dipped cord is 83.59N, and the amount of adhesive on the peeling surface is judged to be Class B.
[0123] Embodiment 18
[0124] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that furfural is used to replace formaldehyde in this embodiment. The specific addition amount is shown in Table 2. After testing, the CRA peeling force of the dipped cord is 89.46N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0125] Embodiment 19
[0126] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 6. The difference from Example 6 is that sodium hydroxide is used instead of ammonia water in this embodiment. The specific addition amount is shown in Table 2. After testing, the CRA peeling force of the dipped cord is 77.31N, and the amount of adhesive on the peeling surface is judged to be Class B.
[0127] Embodiment 20
[0128] This embodiment is a two-bath dipping solution formulation, which is suitable for the second bath of polyester two-bath dipping and also suitable for one-bath direct dipping of nylon. For specific addition amounts, see Table 3.
[0129] Step I: Prepare phenolic pre-shrinkage solution. Dissolve 7.5g of resorcinol and 0.2g of sodium hydroxide in 80g of deionized water. Add 11g of formaldehyde in batches and stir and ripen at room temperature for 3 hours.
[0130] Step II: Addition of sulfur-containing and active proton compounds. Disperse 3.7 g of compound A prepared in Example 1 in 50 g of deionized water under rapid stirring, and adjust the pH to 9-10 with aqueous ammonia to obtain a sulfur-containing compound dispersion. The sulfur-containing compound dispersion is used immediately after preparation. Add the above sulfur-containing compound dispersion into the phenolic pre-shrinkage solution under stirring.
[0131] Step III: Adding latex: 170 g of latex was added to the reaction mixture, and then 20 g of deionized water and 8 g of ammonia water were stirred and mixed and then dropped in. The mixture was stirred and aged at room temperature for 30 minutes to obtain an RFL impregnation solution with sulfur-containing components added thereto.
[0132] The PET cord was dipped using a single-line dipping machine. The cord was dipped in each dipping tank for about 8 seconds. After each dipping, the cord was dried in the first oven at 170°C and then cured in the second oven at 240°C. The residence time in both ovens was about 2 minutes. The cord tension was maintained between 4.0 and 5.0 N during the dipping and drying process. In the dipping machine, the first dipping tank used the well-known D417 first bath formula, and the second dipping tank used the formula of each embodiment and comparative example of the present invention. The cord after drying and curing showed a color ranging from light yellow to light brown.
[0133] The CRA peel test was performed using the test method of GB / T40725-2021, and the total peel force of the five cords and the grade of the rubber covering the cord surface were recorded, represented by grades A to E. The CRA peel force of the dipped cord in this embodiment was 112.53N, and the amount of rubber attached to the peeled surface was determined to be grade A.
[0134] Embodiment 21
[0135] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that this embodiment adds the least amount of pre-condensed RF resin in Examples 20 to 33 of the present application. The specific amount added is shown in Table 3. After testing, the CRA peeling force of the dipped cord is 99.84N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0136] Embodiment 22
[0137] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that this embodiment adds the largest amount of latex in Examples 20 to 33 of the present application. The specific amount added is shown in Table 3. After testing, the CRA peeling force of the dipped cord is 107.62N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0138] Embodiment 23
[0139] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that this embodiment adds the least amount of sulfur-containing and active proton compounds in Examples 20 to 33 of the present application. The specific amount of addition is shown in Table 3. After testing, the CRA peeling force of the dipped cord is 97.15N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0140] Embodiment 24
[0141] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that this embodiment adds the largest amount of sulfur-containing and active proton compounds in Examples 20 to 33 of the present application. The specific amount of addition is shown in Table 3. After testing, the CRA peeling force of the dipped cord is 101.39N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0142] Embodiment 25
[0143] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that compound A is replaced by compound B in this embodiment. The specific addition amount is shown in Table 3. After testing, the CRA peeling force of the dipped cord is 110.63N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0144] Embodiment 26
[0145] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that compound A is replaced by compound C in this embodiment. The specific addition amount is shown in Table 3. After testing, the CRA peeling force of the dipped cord is 103.95N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0146] Embodiment 27
[0147] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that compound A is replaced by compound D in this embodiment. The specific addition amount is shown in Table 4. After testing, the CRA peeling force of the dipped cord is 98.16N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0148] Embodiment 28
[0149] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that compound E is used to replace compound A in this embodiment. The specific addition amount is shown in Table 4. After testing, the CRA peeling force of the dipped cord is 104.57N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0150] Embodiment 29
[0151] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that this embodiment uses nylon 66 cord for dipping treatment. The specific addition amount is shown in Table 4. After testing, the CRA peeling force of the dipped cord is 122.24N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0152] Embodiment 30
[0153] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that in addition to adding VP latex, this embodiment also adds butadiene styrene latex. The specific amount of addition is shown in Table 4. After testing, the CRA peeling force of the dipped cord is 111.75N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0154] Embodiment 31
[0155] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that phenol is used instead of resorcinol in this embodiment. The specific addition amount is shown in Table 4. After testing, the CRA peeling force of the dipped cord is 92.08N, and the amount of adhesive on the peeling surface is judged to be Class B.
[0156] Embodiment 32
[0157] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that furfural is used instead of formaldehyde in this embodiment. The specific addition amount is shown in Table 4. After testing, the CRA peeling force of the dipped cord is 88.66N, and the amount of adhesive on the peeling surface is judged to be Class A.
[0158] Embodiment 33
[0159] In this embodiment, the dipping solution is prepared and the dipping test is completed according to the method of Example 20. The difference from Example 20 is that 20% sodium hydroxide is used instead of ammonia water in this embodiment. The specific addition amount is shown in Table 4. After testing, the CRA peeling force of the dipped cord is 90.13N, and the amount of adhesive on the peeling surface is judged to be Class B.
[0160] Comparative Example 1
[0161] This comparative example serves as a comparison with the above-mentioned Examples 6 and 9 to 14.
[0162] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 6. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 5. After testing, the CRA peeling force of the dipped cord was 61.98N, and the amount of adhesive on the peeling surface was judged to be Class C.
[0163] Comparative Example 2
[0164] This comparative example serves as a control for Example 7.
[0165] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 6. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 5. After testing, the CRA peeling force of the dipped cord was 82.24N, and the amount of adhesive on the peeling surface was judged to be Class B.
[0166] Comparative Example 3
[0167] This comparative example serves as a control for Example 8.
[0168] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 6. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 5. After testing, the CRA peeling force of the dipped cord was 79.46N, and the amount of adhesive on the peeling surface was judged to be Class B.
[0169] Comparative Example 4
[0170] This comparative example serves as a control for Example 16.
[0171] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 6. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 5. After testing, the CRA peeling force of the dipped cord was 66.70N, and the amount of adhesive on the peeling surface was judged to be Class C.
[0172] Comparative Example 5
[0173] This comparative example serves as a control for Example 17.
[0174] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 6. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 5. After testing, the CRA peeling force of the dipped cord was 72.15N, and the amount of adhesive on the peeling surface was judged to be Class C.
[0175] Comparative Example 6
[0176] This comparative example serves as a control for Example 18.
[0177] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 6. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 5. After testing, the CRA peeling force of the dipped cord was 59.37N, and the amount of adhesive on the peeling surface was judged to be Class D.
[0178] Comparative Example 7
[0179] This comparative example serves as a control for Example 19.
[0180] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 6. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 5. After testing, the CRA peeling force of the dipped cord was 55.02N, and the amount of adhesive on the peeling surface was judged to be Class C.
[0181] Comparative Example 8
[0182] This comparative example serves as a control for Example 15.
[0183] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 6. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 5. After testing, the CRA peeling force of the dipped cord was 99.73N, and the amount of adhesive on the peeling surface was judged to be Class A.
[0184] Comparative Example 9
[0185] This comparative example serves as a control for Example 20 and Example 23 to Example 28.
[0186] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 20. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 6. After testing, the CRA peeling force of the dipped cord was 90.37N, and the amount of adhesive on the peeling surface was judged to be Class A.
[0187] Comparative Example 10
[0188] This comparative example serves as a control for Example 21.
[0189] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 20. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 6. After testing, the CRA peeling force of the dipped cord was 81.01N, and the amount of adhesive on the peeling surface was judged to be Class B.
[0190] Comparative Example 11
[0191] This comparative example serves as a control for Example 22.
[0192] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 20. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 6. After testing, the CRA peeling force of the dipped cord was 87.77N, and the amount of adhesive on the peeling surface was judged to be Class A.
[0193] Comparative Example 12
[0194] This comparative example serves as a control for Example 29.
[0195] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 20. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 6. After testing, the CRA peeling force of the dipped cord was 105.23N, and the amount of adhesive on the peeling surface was judged to be Class A.
[0196] Comparative Example 13
[0197] This comparative example serves as a control for Example 30.
[0198] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 20. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 6. After testing, the CRA peeling force of the dipped cord was 84.26N, and the amount of adhesive on the peeling surface was judged to be Class A.
[0199] Comparative Example 14
[0200] This comparative example serves as a control for Example 31.
[0201] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 20. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 6. After testing, the CRA peeling force of the dipped cord was 76.35N, and the amount of adhesive on the peeling surface was judged to be Class B.
[0202] Comparative Example 15
[0203] This comparative example serves as a control for Example 32.
[0204] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 20. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 6. After testing, the CRA peeling force of the dipped cord was 79.54N, and the amount of adhesive on the peeling surface was judged to be Class B.
[0205] Comparative Example 16
[0206] This comparative example serves as a control for Example 33.
[0207] In this comparative example, the dipping solution was prepared and the dipping test was completed according to the method of Example 20. The difference from the above-mentioned comparative example is that this comparative example does not contain the sulfur-containing and active proton compounds, and the addition amounts of other raw materials refer to Table 6. After testing, the CRA peeling force of the dipped cord was 68.81N, and the amount of adhesive on the peeling surface was judged to be Class C.
[0208] Table 1 Data summary of Examples 6 to 12
[0209]
[0210]
[0211]
[0212] Table 2 Data summary of Examples 13 to 19
[0213]
[0214]
[0215]
[0216] Table 3 Data summary of Examples 20 to 26
[0217]
[0218]
[0219] Table 4 Data summary of Examples 27 to 33
[0220]
[0221]
[0222] Table 5 Data summary of Comparative Examples 1 to 8
[0223]
[0224]
[0225] Table 6 Data summary of Comparative Examples 9 to 16
[0226]
[0227]
[0228]
[0229] The above embodiments are only used to illustrate the technical solution of the present application but not to limit it. The present application is described in detail with reference to the preferred embodiments. It should be understood by those skilled in the art that the technical solution of the present application can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application, and should be included in the scope of the claims of the present application.
Claims
1. A dipping solution for a fiber skeleton material, characterized in that: include: A first-bath dipping solution suitable for a one-bath dipping method or a second dipping solution suitable for a two-bath dipping method; The solid content of the one-bath dipping solution is 8% to 45%, and its dry weight includes: 15% to 70% of phenolic adhesive resin, 20% to 70% of latex and 3% to 20% of sulfur-containing and active proton compounds; the solid content of the second dipping solution is 8% to 45%, and its dry weight includes: 10% to 60% of phenolic adhesive resin, 30% to 85% of latex and 3% to 20% of sulfur-containing and active proton compounds.
2. The impregnation solution for the fiber skeleton material according to claim 1, characterized in that: The solid content of the one-bath dipping solution is 15% to 35%, and its dry weight comprises: 30% to 70% of phenolic adhesive resin, 20% to 60% of latex and 5% to 15% of sulfur-containing and active proton compounds.
3. The impregnation solution for the fiber skeleton material according to claim 1, characterized in that: The solid content of the second dipping solution is 15% to 35%, and its dry weight includes: 10% to 35% of phenolic adhesive resin, 50% to 85% of latex and 5% to 15% of sulfur-containing and active proton compounds.
4. The impregnation solution for the fiber skeleton material according to any one of claims 1 to 3, characterized in that: The one-bath dipping solution and / or the second dipping solution further include: auxiliary agents with a total proportion of less than or equal to 10%; the auxiliary agents include: pH regulators, surfactants, film-forming agents, antioxidants and / or cross-linking catalysts.
5. The impregnation solution for the fiber skeleton material according to any one of claims 1 to 3, characterized in that: The sulfur-containing and active proton compound includes: a first compound, a second compound and / or a third compound; The general structural formula of the first compound is as follows: In the above formula, b is a positive integer, and the sum of a and c is greater than or equal to 1; The general structural formula of the second compound is as follows: In the above formula, e is a positive integer, and the sum of d and f is greater than or equal to 1; The general structural formula of the third compound is as follows: In the above formula, h is a positive integer, and the sum of g and i is greater than or equal to 1.
6. The impregnation solution for fiber skeleton material according to claim 5, characterized in that: R and R' each include: an unsubstituted or branched substituted alkyl chain, or an unsubstituted or branched substituted alkenyl chain, or an unsubstituted or branched substituted alkynyl chain, or an unsubstituted or branched substituted hetero chain, or an unsubstituted or branched substituted cycloalkyl chain, or an unsubstituted or branched substituted cyclic hetero chain, or an unsubstituted or branched substituted cyclic double bond containing chain, or an unsubstituted or branched substituted cyclic triple bond containing chain, or an unsubstituted or branched substituted benzene, or an unsubstituted or branched substituted condensed ring, or an unsubstituted or branched substituted hetero ring; The heterochain is a carbon chain containing an oxygen atom, a carbon chain containing a nitrogen atom and / or a carbon chain containing a sulfur atom; The heterocyclic ring includes: pyridine, thiophene or furan; The branched chains include: alkyl chains, alkenyl chains, alkynyl chains, hetero chains, cycloalkyl chains, cyclic hetero chains, cyclic chains containing double bonds, cyclic chains containing triple bonds, benzene, condensed rings and / or hetero rings.
7. The impregnation solution for fiber skeleton material according to claim 6, characterized in that: When a, d or g is zero, R also includes: an independent hydrogen atom; when c, f or i is zero, R' also includes: an independent hydrogen atom.
8. The impregnation solution for fiber skeleton material according to claim 6, characterized in that: The alkyl chain, the alkenyl chain, the alkynyl chain, the hetero chain, the cycloalkyl chain, the cyclic hetero chain, the cyclic double bond-containing chain, the cyclic triple bond-containing chain, the benzene, the condensed ring and the hetero ring have substituents, and the substituents include: aromatic groups, alkoxy groups, halogens, ester groups and / or amide groups.
9. The impregnation solution for fiber skeleton material according to any one of claims 1 to 3, characterized in that: The phenolic adhesive resin is a pre-condensed resin formed by polycondensation of phenols and aldehydes under alkaline conditions; The phenols include: resorcinol, phloroglucinol and / or phenol; the aldehydes include: formaldehyde, acetaldehyde, butyraldehyde and / or terephthalaldehyde.
10. The impregnation solution for fiber skeleton material according to claim 9, characterized in that: The amount of the aldehyde added in the polycondensation process is 1.0 to 2.0 times the amount of the phenol added.
11. The impregnation solution for fiber skeleton material according to any one of claims 1 to 3, characterized in that: The latex includes: styrene-butadiene latex, butylpyrrolidone latex, nitrile-butadiene latex, polybutadiene latex and / or natural latex.
12. The impregnation solution for fiber skeleton material according to claim 11, characterized in that: The styrene butadiene latex includes: styrene butadiene latex terminated by carboxyl, hydroxyl, acid anhydride and / or grafted; the butyl pyrrolidone latex includes: butyl pyrrolidone latex terminated by carboxyl, hydroxyl, acid anhydride and / or grafted; the nitrile butadiene latex includes: nitrile butadiene latex terminated by carboxyl, hydroxyl, acid anhydride and / or grafted; the polybutadiene latex includes: polybutadiene latex terminated by carboxyl, hydroxyl, acid anhydride and / or grafted; the natural latex includes: natural latex terminated by carboxyl, hydroxyl, acid anhydride and / or grafted.
Citation Information
Patent Citations
Non-phenolic aldehyde type environment-friendly dipping solution for fiber framework material
CN117779453A
Dipping solution for fiber skeleton material
CN117779473A