Method for preparing sizing carbon fiber by using aliphatic polyamide-containing pre-sizing agent, application of sizing carbon fiber, sizing carbon fiber and application of sizing carbon fiber

By using pre-sizing agent containing aliphatic polyamide and epoxy resin on carbon fiber and secondary sizing technology of resorcinol formaldehyde latex on carbon fiber, the problem of poor binding force between carbon fiber and rubber matrix is ​​solved, and the composite material is significantly improved Mechanical properties and temperature resistance achieve simple and efficient industrial production.

CN118932723APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310536589.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The poor surface bonding force between carbon fiber and rubber matrix leads to poor load transfer and the inability to effectively exert the reinforcement effect of fibers. At the same time, the brittleness and low elongation of carbon fibers are problematic. The existing technology processing process is complex and costly, so it is impossible to achieve large-scale application.

Method used

The carbon fiber is pre-sizing and pre-dryed with aliphatic polyamide and epoxy resin, followed by secondary sizing and drying with resorcinol formaldehyde latex, controlled infiltration time ≤22 seconds and viscosity ≤100 centimeters Poir, improve the adhesion and temperature resistance of carbon fiber to rubber matrix.

Benefits of technology

It significantly improves the mechanical properties and temperature resistance of sizing carbon fiber and rubber composite materials, and the compression strength after impact reaches more than 430MPa. The process is simple and stable, and it is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004226498590000111
    Figure BDA0004226498590000111
  • Figure BDA0004226498590000112
    Figure BDA0004226498590000112
  • Figure BDA0004226498590000121
    Figure BDA0004226498590000121
Patent Text Reader

Abstract

The invention relates to the field of carbon fiber sizing agents, and discloses a method for preparing sizing carbon fibers by using an aliphatic polyamide-containing pre-sizing agent, application of the sizing carbon fibers, the sizing carbon fibers and application of the sizing carbon fibers. The method comprises the following steps: S1, carrying out pre-sizing and pre-drying on carbon fibers by adopting a pre-sizing agent containing aliphatic polyamide and epoxy resin to obtain initial carbon fibers; s2, carrying out secondary sizing and secondary drying on the initial carbon fiber by adopting resorcinol formaldehyde latex to obtain sized carbon fiber; the infiltration time of the pre-sizing agent is less than or equal to 22 seconds, and the viscosity at 25 DEG C is less than or equal to 100 centipoises. According to the pre-sizing agent, due to the existence of aliphatic polyamide, the stress concentration phenomenon of multiple interface phases after thermocuring can be remarkably improved, the mechanical property of a sizing carbon fiber-rubber composite material prepared from the sizing carbon fiber is remarkably improved, meanwhile, the bonding force between the sizing carbon fiber and a rubber matrix is improved, and the mechanical property of the sizing carbon fiber-rubber composite material is improved. And the sizing carbon fiber has relatively good temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of carbon fiber sizing agents, and in particular to a method for preparing sized carbon fibers by utilizing a pre-sizing agent containing aliphatic polyamide and its application, and the sized carbon fibers and their application. Background Art

[0002] Compared with carbon fiber reinforced resin-based composites, carbon fiber reinforced rubber-based composites are more excellent in toughness, elasticity, fatigue resistance and other aspects, and have the prospect of being widely used in transportation equipment, industrial parts, sporting goods, energy and chemical industries. However, the surface and interface properties of carbon fiber and rubber matrix are very different, and it is difficult to effectively combine them into a solid integrated material, resulting in poor load transfer and inability to effectively play the reinforcing role of the fiber. At the same time, carbon fiber itself has excellent comprehensive properties such as high specific strength, high modulus, and high thermal conductivity, but it is a brittle material with low elongation, and it is usually necessary to use a surface sizing agent to toughen and modify the fiber. However, there is no mature product of high-performance sizing agents that can simultaneously improve fiber toughness and rubber interface bonding.

[0003] CN111484654A discloses a thermally conductive rubber material, in which carbon fibers are first treated with a silane coupling agent, then etched with CO2 plasma, and combined with pretreated hexagonal boron nitride powder and pretreated nanopowder to improve the thermal conductivity and mechanical properties of the rubber material. This solution can improve the interface bonding between the carbon fibers and the rubber material to a certain extent, but the processing process is relatively complicated, continuous production is impossible, and the cost is high, and large-scale application cannot be achieved. Summary of the invention

[0004] The purpose of the present invention is to overcome the problems of poor interface bonding between sized carbon fiber and rubber matrix, poor temperature resistance, and poor mechanical properties of sized carbon fiber-rubber composite materials in the prior art, and to provide a method and application of preparing sized carbon fiber using a pre-sizing agent containing aliphatic polyamide, and sized carbon fiber and application. The method is to coat a layer of pre-sizing agent containing aliphatic polyamide and epoxy resin on the surface of carbon fiber and pre-dry it, and then use resorcinol formaldehyde latex (hereinafter referred to as RFL emulsion) for secondary sizing and secondary drying, which can improve the coupling effect of the pre-sizing agent between carbon fiber and RFL emulsion, further enhance the bonding force between sized carbon fiber and rubber matrix, and due to the presence of aliphatic polyamide in the pre-sizing agent, it can improve the stress concentration phenomenon of sized carbon fiber after thermal curing, and when applied to rubber materials, significantly improve the mechanical properties of sized carbon fiber-rubber composite materials prepared by the sized carbon fiber.

[0005] In order to achieve the above object, the present invention provides a method for preparing sized carbon fiber using a pre-sizing agent containing aliphatic polyamide, wherein the method comprises:

[0006] S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing aliphatic polyamide and epoxy resin to obtain initial carbon fiber;

[0007] S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber;

[0008] The pre-sizing agent has a wetting time of ≤22 seconds and a viscosity of ≤100 centipoise at 25°C.

[0009] The second aspect of the present invention provides a sized carbon fiber prepared by the method described in the first aspect of the present invention.

[0010] The third aspect of the present invention provides an application of the method described in the first aspect of the present invention and the sized carbon fiber described in the second aspect of the present invention in a rubber material.

[0011] Through the above technical scheme, the method and application of preparing sized carbon fiber using aliphatic polyamide pre-sizing agent, and the sized carbon fiber and application provided by the present invention achieve the following technical effects:

[0012] (1) The present invention utilizes a pre-sizing agent and an RFL emulsion to perform pre-sizing and secondary sizing on carbon fibers, respectively, which can significantly improve the bonding strength between the prepared sized carbon fibers and the rubber matrix while improving the temperature resistance of the sized carbon fibers.

[0013] (2) The present invention uses epoxy resin and aliphatic polyamide as the main components in the pre-sizing agent, and adopts an RFL emulsion sizing agent with good affinity to the rubber matrix in the secondary sizing process, which can significantly improve the mechanical properties of the sized carbon fiber-rubber composite material and enhance the bonding force between the sized carbon fiber and the rubber matrix.

[0014] (3) The present invention controls the infiltration time of the pre-sizing agent to be ≤22 seconds, the viscosity at 25°C to be ≤100 centipoise, and specific pre-sizing and secondary sizing processes, thereby finally preparing sized carbon fibers with high temperature resistance (capable of withstanding high temperatures above 250°C) and good bonding strength with the rubber matrix (bonding strength can reach above 130N), thereby significantly improving the mechanical properties of the sized carbon fiber-rubber composite material, specifically, the post-impact compressive strength reaches above 430MPa.

[0015] (4) The method of the present invention is simple in process, highly stable, safe and pollution-free, and can be completed using an existing carbon fiber preparation production line, thus having broad industrial prospects. DETAILED DESCRIPTION

[0016] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0017] In one aspect, the present invention provides a method for preparing sized carbon fiber using a pre-sizing agent containing aliphatic polyamide, wherein the method comprises:

[0018] S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing aliphatic polyamide and epoxy resin to obtain initial carbon fiber;

[0019] S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber;

[0020] The pre-sizing agent has a wetting time of ≤22 seconds and a viscosity of ≤100 centipoise at 25°C.

[0021] In the present invention, the inventors found that RFL emulsion is often used as a sizing agent in the prior art to improve the interface problem between carbon fiber and rubber matrix. However, since RFL emulsion is an aqueous emulsion, it is easy to have poor wetting and spreading on the surface of carbon fiber, resulting in poor bonding ability with the surface of carbon fiber, and it is also unable to effectively improve the mechanical properties, temperature resistance and bonding strength with the rubber matrix of the sized carbon fiber-rubber composite material.

[0022] In the present invention, the inventors have found that a layer of pre-sizing agent containing aliphatic polyamide and epoxy resin is coated on the surface of carbon fiber in advance, and then RFL emulsion is used to perform secondary sizing to achieve preliminary bonding with the surface of carbon fiber. Furthermore, due to its good hydrophilicity, RFL emulsion can fully play its role on the surface of carbon fiber coated with pre-sizing agent. At the same time, when aliphatic polyamide is introduced into the pre-sizing agent and the prepared sized carbon fiber is applied to the rubber material, the stress concentration of the multi-interface phase after thermal curing can be effectively alleviated, and the occurrence of cracks can be effectively alleviated, and the mechanical properties of the sized carbon fiber-rubber composite material prepared by the sized carbon fiber are significantly improved, and at the same time, the sized carbon fiber and the rubber matrix have good bonding force and temperature resistance.

[0023] In the present invention, further research results show that only when the pre-sizing agent has an impregnation time of ≤22 seconds and a viscosity of ≤100 centipoise at 25°C, can a good coupling enhancement effect be achieved between the FRL and carbon fiber phases, and can it cooperate well with the RFL emulsion. When the impregnation time is greater than 22 seconds, the hydrophilicity is insufficient, and the binding ability of the pre-sizing agent with the carbon fiber and the RFL emulsion is insufficient, and the coupling enhancement effect cannot be effectively played. When the viscosity at 25°C is greater than 100 centipoise, the pre-sizing agent cannot be evenly infiltrated and spread on the surface of the carbon fiber, and it is easy to produce stress concentration after later curing, thereby reducing the comprehensive properties of the sized carbon fiber-rubber composite material such as mechanical properties and fatigue resistance.

[0024] In the present invention, the epoxy resin is a glycidyl ether epoxy resin containing two or more epoxy groups in the molecule, for example, it may be at least one of bisphenol A, bisphenol F, and bisphenol S.

[0025] In the present invention, the epoxy equivalent of the epoxy resin is 160-6000.

[0026] In the present invention, the epoxy equivalent of the epoxy resin satisfies the above range, so that the wetting time and viscosity of the prepared pre-sizing agent at 25° C. can meet the requirements.

[0027] In the present invention, the pre-sizing agent may further contain components such as antioxidants, lubricants, surfactants, etc. The surfactant is preferably a non-ionic surfactant.

[0028] According to a preferred embodiment of the present invention, the nonionic surfactant is selected from at least one of alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyoxyethylene amine, polyoxyethylene amide, sorbitan ester and fluorocarbon surfactant.

[0029] In the present invention, there is no particular limitation on the types and contents of the antioxidant, lubricant and surfactant contained in the pre-sizing agent, and they can be adjusted according to the needs in the art.

[0030] According to a particularly preferred embodiment of the present invention, the pre-sizing agent contains 35-65 parts of epoxy resin, 4-25 parts of aliphatic polyamide, 1-5 parts of antioxidant, 1-5 parts of lubricant and 15-50 parts of surfactant. When each component meets the above range, when the pre-sizing agent is applied to sized carbon fiber, the prepared sized carbon fiber-rubber composite material has more excellent comprehensive properties.

[0031] In the present invention, the epoxy resin, antioxidant, lubricant and surfactant may be provided in the form of an epoxy resin aqueous emulsion.

[0032] In the present invention, the epoxy resin, antioxidant, lubricant and surfactant are configured into an epoxy resin aqueous emulsion for addition, and further combined with the RFL emulsion to improve the synergistic effect between the components, and can significantly improve the mechanical properties of the sized carbon fiber-rubber composite material prepared from the sized carbon fiber, and improve the bonding force between the sized carbon fiber and the rubber matrix, and the sized carbon fiber has good temperature resistance.

[0033] In the present invention, the preparation method of the pre-sizing agent in step S1 can adopt the preparation method of the emulsion generally used in the art, such as phase inversion emulsification method, ultrasonic emulsification method and colloid mill emulsification method.

[0034] In the present invention, the RFL emulsion is a mixed emulsion formed by the reaction of resorcinol, formaldehyde and rubber emulsion. The specific preparation process is: sodium hydroxide and resorcinol are added to the first reaction kettle, and then an appropriate amount of water is added, the temperature is controlled to 20-40°C, and then formaldehyde is slowly added, and a prepolymer is obtained after aging reaction for 2-4 hours; rubber latex is added to the second reaction kettle, the temperature is controlled to 20-40°C, and the synthesized prepolymer is slowly added dropwise, and the reaction is continued for 10-30 hours to finally prepare the RFL emulsion.

[0035] In the present invention, the rubber emulsion in the RFL emulsion can be acrylic rubber emulsion, acrylonitrile-butadiene rubber emulsion, isoprene rubber emulsion, polyurethane rubber emulsion, ethylene-propylene rubber emulsion, chloroprene rubber emulsion, silicone rubber emulsion, hydrogenated nitrile rubber emulsion, styrene-butadiene rubber emulsion, polysulfide rubber emulsion, natural rubber emulsion, butadiene rubber emulsion and butyl rubber emulsion, etc.

[0036] According to the present invention, the pre-sizing agent has a wetting time of ≤10 seconds and a viscosity of ≤90 centipoise at 25°C.

[0037] According to the present invention, the average particle size of the aliphatic polyamide is ≤0.9 micrometer.

[0038] In the present invention, the average particle size of the aliphatic polyamide meets the above range, which can ensure that the pre-sizing agent is infiltrated and spread on the surface of the carbon fiber and improve its two-phase coupling effect.

[0039] Furthermore, the average particle size of the aliphatic polyamide is ≤0.5 micrometer.

[0040] According to the present invention, in the pre-sizing agent, the mass ratio of the epoxy resin to the aliphatic polyamide is 1:0.1-0.7.

[0041] In the present invention, the mass ratio of the epoxy resin and the aliphatic polyamide satisfies the above range, so that the wetting time and viscosity of the pre-sizing agent at 25°C meet the requirements, improve the temperature resistance of the sized carbon fibers, and further enhance the mechanical properties of the sized carbon fibers and the rubber matrix.

[0042] Furthermore, in the pre-sizing agent, the mass ratio of the epoxy resin to the aliphatic polyamide is 1:0.2-0.3.

[0043] According to the present invention, the number average molecular weight of the aliphatic polyamide is 8000-45000 g / mol, preferably 15000-30000 g / mol.

[0044] According to one embodiment of the present invention, the aliphatic polyamide includes a structural unit A provided by a diamine and a structural unit B provided by an aliphatic dibasic acid.

[0045] In the present invention, when the aliphatic polyamide is added to the pre-sizing agent, compared with the aromatic polyamide, it can further improve the mechanical properties of the sized carbon fiber-rubber composite material prepared from the sized carbon fiber when used in combination with the RFL emulsion.

[0046] In the present invention, the diamine can be commercially available, for example, it can be at least one of ethylenediamine, hexamethylenediamine, and decanediamine.

[0047] In the present invention, the aliphatic dibasic acid can be commercially available, for example, it can be at least one of oxalic acid, adipic acid, sebacic acid, and dodecanedioic acid.

[0048] In the present invention, “the aliphatic polyamide includes a structural unit A provided by a diamine and a structural unit B provided by an aliphatic dibasic acid” means that the aliphatic polyamide is prepared by polycondensation of a diamine and a dibasic acid.

[0049] According to the present invention, the molar ratio of the structural unit A to the structural unit B is 1-2:1.

[0050] According to one embodiment of the present invention, the aliphatic polyamide comprises a structural unit C provided by a lactam.

[0051] In the present invention, “the aliphatic polyamide comprises a structural unit C provided by lactam” means that the aliphatic polyamide is prepared by ring-opening of lactam.

[0052] In the present invention, the lactam can be commercially available, for example, it can be at least one of valerolactam, caprolactam, β-lactam, and γ-lactam.

[0053] In the present invention, in order to further obtain sized carbon fibers with better comprehensive performance, aliphatic polyamide is preferably prepared by polycondensation of diamine and aliphatic dibasic acid.

[0054] In the present invention, the aliphatic polyamide can be obtained commercially.

[0055] According to the present invention, the pre-drying temperature is 70-110°C.

[0056] In the present invention, the inventors have found that when the pre-drying temperature is too low, the drying time is too long and the dehydration efficiency is low; when the pre-drying temperature is too high, it is easy to cause too fast dehydration and the moisture content is difficult to control. When the pre-drying temperature meets the above range, the carbon fiber after pre-drying can retain appropriate moisture to promote the rapid spreading and penetration of the subsequent RFL emulsion.

[0057] Furthermore, the pre-drying temperature is 80-100°C.

[0058] According to the present invention, the temperature of the secondary drying is 100-250°C, preferably 150-200°C.

[0059] According to the present invention, in the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:1-20, preferably 1:5-15.

[0060] According to the present invention, based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%.

[0061] In the present invention, if the pre-sizing amount of the pre-sizing agent is too small, the coupling effect of improving the interface cannot be achieved; if the pre-sizing amount is too large, the fiber bundling and fiber opening ability will be affected.

[0062] Furthermore, based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.5-20wt%.

[0063] According to the present invention, based on the mass of the carbon fiber, the sizing amount of the RFL emulsion is 5-35wt%.

[0064] In the present invention, when the sizing amount of the RFL emulsion is less than 5wt%, the adhesion between the sized carbon fiber and the rubber matrix is ​​insufficient; when it exceeds 35wt%, the post-processing of the sized fiber will be difficult and the fatigue resistance will be reduced.

[0065] Furthermore, based on the mass of the carbon fiber, the sizing amount of the RFL emulsion is 10-20wt%.

[0066] The second aspect of the present invention provides a sized carbon fiber prepared by the method described in the first aspect of the present invention.

[0067] The third aspect of the present invention provides an application of the method described in the first aspect of the present invention and the sized carbon fiber described in the second aspect of the present invention in a rubber material.

[0068] In the present invention, when the sized carbon fiber is used in a rubber material to prepare a reinforced rubber composite material, the content of the sized carbon fiber in the reinforced rubber composite material is 15-30wt%.

[0069] In the present invention, the reinforced rubber composite material may further contain zinc oxide, stearic acid, carbon black N330, accelerator DM, accelerator TMTD and sulfur.

[0070] In the present invention, there is no particular limitation on the rubber material, and it may be, for example, acrylic rubber, acrylonitrile-butadiene rubber, isoprene rubber, polyurethane rubber, ethylene-propylene rubber, chloroprene rubber, silicone rubber, hydrogenated nitrile rubber, styrene-butadiene rubber, polysulfide rubber, natural rubber, butadiene rubber, or butyl rubber, and is preferably of the same type as the rubber emulsion in the RFL emulsion described in the present invention.

[0071] The present invention will be described in detail below through examples. In the following examples, each parameter is obtained by the following method.

[0072] Wetting time: The pre-sizing agent was evenly coated on the glass slide, placed at room temperature for 12 hours, and then dried at 50°C to obtain a film sample. Using the OCA20 high-speed contact angle meter, 3 microliters of deionized water was dropped onto the surface of the glass slide, and the time required for the water drop to completely wet the surface was recorded. Complete wetting was measured when the contact angle was 0.

[0073] Viscosity: The pre-sizing agent was diluted to a concentration of 2 wt %, and the viscosity was tested using a rotational viscometer at a temperature of 25° C. and a torque range of 30-70%.

[0074] Adhesion: The sizing carbon fiber is buried in an unvulcanized natural rubber block (wherein the mass of the sizing carbon fiber is 20% of the mass of the natural rubber block), and vulcanized at 140°C, 40 minutes, and a stamping pressure of 3MPa. The vulcanization formula system includes 100 parts of natural rubber, 4 parts of zinc oxide, 1.5 parts of stearic acid, 15 parts of carbon black N330, 1.2 parts of accelerator DM, 0.2 parts of accelerator TMTD, and 3 parts of sulfur. On a universal strength tester, the sizing carbon fiber is pulled out at a speed of 200mm / min. The tension required to pull out a length of 1 cm is the adhesion between the fiber and the rubber.

[0075] Sizing amount: Weigh the mass of carbon fiber before and after sizing, and calculate the sizing amount according to the formula: Sizing amount % = (mass of carbon fiber after sizing - mass of carbon fiber before sizing) / mass of carbon fiber before sizing × 100%.

[0076] Temperature resistance: Take an appropriate amount of sizing carbon fiber and test the weight loss rate in the range of room temperature-300°C using a TGA thermogravimetric analyzer under a nitrogen atmosphere (weight loss rate % = loss weight / sizing agent weight × 100%). The temperature corresponding to 5wt% weight loss rate is used as the temperature resistance index.

[0077] Compression strength after impact: Referring to SACMA SRM 2R-94 standard, a 6.7 J / mm drop hammer impact is applied to the center of the sized carbon fiber-rubber composite sample to calculate the compression strength after impact.

[0078] Aliphatic polyamide was purchased from Sinopharm Reagent with the brands SZ70 and SZ20.

[0079] KTM-3F epoxy emulsion was purchased from Sinopharm Reagent.

[0080] SS-4W epoxy emulsion was purchased from Sinopharm Reagent.

[0081] Examples 1-6

[0082] A quantitative epoxy resin, a surfactant, an aliphatic polyamide, an antioxidant, and a lubricant are placed in a reaction kettle, and an appropriate amount of deionized water is added, and a uniformly distributed stable emulsion is prepared by high-speed stirring and phase inversion emulsification, which is a pre-sizing agent. The components and amounts of the pre-sizing agent are shown in Table 1, and the infiltration time of the obtained pre-sizing agent is shown in Table 2.

[0083] Among them, the brands of epoxy resin are: E21, 6445, 6420, 6421, 6458, E51;

[0084] The surfactants are: fatty amine polyoxyethylene ether AC-1210, allyl polyethylene glycol APEG1000, sorbitan fatty acid ester S-60, polypropylene glycol PPG-1500, polyethylene glycol PEG-6000, alkylphenol polyoxyethylene ether APEO-20;

[0085] The lubricant is dimethyl phthalate DMP;

[0086] The grades of aliphatic polyamide are: SZ70 (number average molecular weight is 30000) and SZ20 (number average molecular weight is 15000).

[0087] In the first reactor equipped with a stirrer and a temperature control device, 10g of sodium hydroxide and a certain amount of resorcinol were added, and then 90g of water was added, stirred and heated to 35°C, and a certain amount of formaldehyde was slowly added, wherein the total amount of resorcinol and formaldehyde was 30g. After reacting for 3 hours, the temperature was slowly lowered to obtain a resin prepolymer; in the second reactor, 97g of natural rubber latex was added, stirred and heated to 35°C, and the synthesized resin prepolymer was slowly added dropwise, and the reaction continued for 20 hours, and the temperature was slowly lowered to obtain an RFL emulsion. The molar ratio of resorcinol to formaldehyde in the RFL emulsion is shown in Table 2.

[0088] The unsized carbon fiber is pre-sized in the first sizing tank filled with a certain viscosity dilution of the above-mentioned pre-sizing agent (specific viscosity see Table 2), and then dried at a set drying temperature for 2 minutes; then secondary sizing is performed in the second sizing tank filled with a certain viscosity dilution of the above-mentioned RFL emulsion (specific viscosity see Table 2), and then dried at a set temperature for 3 minutes, and the sized carbon fiber for reinforcing rubber composite materials is prepared after winding and collecting. The pre-sizing amount and pre-drying temperature, the secondary sizing amount and the secondary drying temperature are shown in Table 2.

[0089] Comparative Example 1

[0090] The carbon fiber was impregnated and sized with a commercially available KTM-3F epoxy emulsion sizing agent, with a sizing amount of 5wt%, a drying temperature of 110°C, and winding to obtain sized carbon fiber.

[0091] Comparative Example 2

[0092] The RFL emulsion of Example 2 was used to impregnate and size the unsized carbon fiber, with a sizing amount of 10 wt % and a drying temperature of 160° C. to prepare the sized carbon fiber by winding and collecting.

[0093] Comparative Example 3

[0094] The unsized carbon fibers were pre-sized using a commercially available SS-4W epoxy emulsion sizing agent with a sizing amount of 5 wt% and a drying temperature of 90°C. The carbon fibers were then secondary-sized using the RFL emulsion of Example 2 with a sizing amount of 10% and a drying temperature of 180°C. The sized carbon fibers were then wound and collected.

[0095] Table 1 Table 2

[0096]

[0097] Table 3

[0098]

[0099] From the results in the above table, it can be seen that Comparative Example 1 only uses traditional epoxy resin emulsion, and Comparative Example 2 only uses RFL emulsion. The bonding force between the prepared carbon fiber and the rubber matrix is ​​low, and the compression strength after impact is poor. Comparative Example 3 uses pre-sizing epoxy emulsion, the complete impregnation time is too long, the viscosity is too large, and the improvement effect is not obvious. Examples 1-6 introduce a pre-sizing agent with epoxy resin and aliphatic polyamide as the main body, an impregnation time of less than 22 seconds, and a viscosity of less than 100 centipoise at 25°C in the pre-sizing process. In the secondary sizing process, an RFL emulsion sizing agent with good affinity to the rubber matrix is ​​used. The prepared carbon fiber has high temperature resistance, good interface adhesion and stability with the rubber matrix, and high compression strength after impact, which can meet the application requirements of higher-level sizing carbon fiber-rubber composite materials.

[0100] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing sized carbon fiber using a pre-sizing agent containing aliphatic polyamide, characterized in that: The method comprises: S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing aliphatic polyamide and epoxy resin to obtain initial carbon fiber; S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber; The pre-sizing agent has a wetting time of ≤22 seconds and a viscosity of ≤100 centipoise at 25°C.

2. The method according to claim 1, wherein: The pre-sizing agent has a wetting time of ≤10 seconds and a viscosity of ≤90 centipoise at 25°C; Preferably, the average particle size of the aliphatic polyamide is ≤0.9 micrometer, preferably ≤0.5 micrometer.

3. The method according to claim 1 or 2, wherein: In the pre-sizing agent, the mass ratio of the epoxy resin to the aliphatic polyamide is 1:0.1-0.7, preferably 1:0.2-0.

3.

4. The method according to any one of claims 1 to 3, wherein: The number average molecular weight of the aliphatic polyamide is 8000-45000 g / mol, preferably 15000-30000 g / mol.

5. The method according to any one of claims 1 to 4, wherein: The aliphatic polyamide comprises a structural unit A provided by a diamine and a structural unit B provided by an aliphatic dibasic acid; Preferably, the molar ratio of the structural unit A to the structural unit B is 1-2:1; Alternatively, the aliphatic polyamide comprises structural units C provided by lactam.

6. The method according to any one of claims 1 to 5, wherein: The pre-drying temperature is 70-110°C, preferably 80-100°C; Preferably, the secondary drying temperature is 100-250°C, preferably 150-200°C.

7. The method according to any one of claims 1 to 6, wherein: In the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:1-20, preferably 1:5-15.

8. The method according to any one of claims 1 to 7, wherein: Based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%, preferably 0.5-20wt%; Preferably, based on the mass of the carbon fiber, the sizing amount of the resorcinol formaldehyde latex is 5-35wt%, preferably 10-20wt%.

9. Sized carbon fiber prepared by the method according to any one of claims 1 to 8.

10. Use of the method according to any one of claims 1 to 8 and the sized carbon fiber according to claim 9 in rubber materials.

Citation Information

Patent Citations

  • Heat-conducting rubber material and rubber track

    CN111484654A

  • Improved carbon fibers

    CN106715784A

  • Sizing-coated carbon fiber bundle, thermoplastic resin composition, molded body, method for manufacturing sizing-coated carbon fiber bundle, and method for manufacturing molded body

    CN110168161A

  • Carbon fiber cord for rubber reinforcement and fiber-reinforced rubber material

    JP2005023481A

  • Polyamide-coated carbon fiber and its production method

    JP2005281464A