Continuous pretreatment process of viscose fabric
Through continuous pretreatment process, using enzyme treatment and multifunction finishing agents and other technologies, the wet strength and gloss of viscose fabrics are improved, the problem of decreasing wet strength is solved, and product quality and production efficiency are improved.
Patent Information
- Application Number
- CN202411263256.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-12
AI Technical Summary
After the alkaline agent and hydrogen peroxide treatment of viscose fabrics in the printing and dyeing factory, the wet strength decreases, affecting their value and life.
Continuous pretreatment technology is adopted, including grey cloth flip flops, burning hair, rolling bioenzyme stacking, padding bioenzyme loose steaming, water washing, wet rolling cloth, tenter drying, long-line continuous rolling and dyeing, soft tentering and anti-shrinkage treatment, through alkaline pectinase, α-amylase, pectinase, cellulase, hydrogen peroxide and other enzyme treatment, combined with infrared drying and multi-function finishing agent treatment, the wet strength and gloss of the fabric are improved.
It significantly improves the wet strength and gloss of viscose fiber fabrics, reduces production costs and environmental pollution, improves production efficiency and product quality, and enhances the softness and water absorption of the fabric.
Smart Images

Figure CN118932731A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of printing and dyeing, and in particular relates to a continuous pre-treatment process for viscose fabrics. Background Art
[0002] Viscose fabric is the full name of viscose fiber, which uses wood as raw material, and is obtained by extracting and reshaping fiber molecules from natural wood cellulose. It has good softness and wear resistance, and is widely used in clothing, household goods and other fields. However, due to the low bonding strength of viscose fiber, the wet strength of semi-finished products of viscose fabric after being treated with alkali agents and hydrogen peroxide in the printing and dyeing factory is greatly reduced. The wet strength of the finished cloth is generally 3 to 4N (100% wet detection), which greatly affects the wearing value of high-end clothing and affects its wearing life and performance. Therefore, how to improve the wet strength of viscose fabric has become a hot topic in current research. Summary of the invention
[0003] The present invention provides a continuous pre-treatment process for viscose fabrics, aiming to solve the problems that the wet strength of semi-finished products of viscose fabrics treated with alkali agents and hydrogen peroxide in printing and dyeing factories is greatly reduced due to the low bonding strength of viscose fibers, and the wet strength of finished fabrics is generally 3-4N (100% wet detection), which greatly affects the wearing value of high-end clothing and affects its wearing life and performance.
[0004] The present invention is implemented in this way. The continuous pretreatment process of viscose fabric comprises the following steps: turning over the seam ends of the grey cloth, singeing, rolling bio-enzyme stacking, impregnating bio-enzyme loose steaming, washing, wet dropping, tenter drying, long-line continuous pad dyeing, soft tentering and shrinkage prevention treatment, the rolling bio-enzyme stacking time is 20-25°C / 6-8 hours, the impregnating bio-enzyme loose steaming time is 95-98°C / 30 minutes, and the production speed is 80 meters / minute.
[0005] Preferably, the grey fabric turning and sewing includes: first checking the quality of the grey fabric and classifying it according to the length, width, weight, etc. of the fabric; unrolling the grey fabric on the roll to check whether the fabric surface has defects or stains, and ensuring that the fabric surface is flat. When turning the fabric, ensure that the fabric is not subjected to unnecessary stretching or compression; divide the grey fabric into appropriate batches according to production requirements, and the quantity of fabric in each batch should be suitable for subsequent processing; print the batch number, fabric type, length and other information at the designated position of the grey fabric for subsequent tracking and management; sew strong thread ends at both ends of each piece of fabric to prevent the fabric from frayed or damaged during processing, and the seam ends are made of thread with a sharp contrast to the color of the grey fabric; re-roll the grey fabric after turning the fabric to ensure that the roll is tight and flat to avoid wrinkles or curling; record the detailed information of each batch of grey fabric, including batch number, total length, weight, etc., for inventory management and quality tracking; store the processed grey fabric in a suitable environment to avoid direct sunlight, moisture or pollution; after the grey fabric turning and sewing is completed, the next step of pre-processing can be carried out.
[0006] Preferably, the singeing method is: cutting burning, one front and one back, 120m / min, the front side of the singeing is cutting burning, and the singeing flame temperature is 900-1000°C.
[0007] Preferably, the rolling bio-enzyme stacking uses alkaline pectinase, a wetting and penetrating agent is added to the alkaline pectinase, the pH value of the enzyme treatment solution is usually controlled between 8.6-10.0, and during the heat preservation stacking process, unsaturated steam is used for steaming, the steaming temperature is controlled at 45-65°C, and the time is within 30-100 minutes.
[0008] Preferably, the padding bio-enzyme loose steaming comprises the following steps:
[0009] Pretreatment, the fabric is first soaked in cold water and then pretreated with hot water to remove some of the size and impurities;
[0010] Desizing enzyme treatment, including padding desizing enzyme solution and steaming, using α-amylase treatment solution, pH value controlled at 6-7, liquid carrying rate at 50%-120%, steaming conditions at 50-100°C, time 20-120 minutes;
[0011] Washing: After desizing enzyme treatment, the cotton fabric must be fully washed to remove the size on the surface;
[0012] Bio-enzyme scouring treatment, including padding with bio-enzyme scouring solution and steaming, the composition of the enzyme scouring solution may include pectinase and cellulase, and non-ionic or anionic surfactant as a wetting and penetrating agent, the steaming temperature is 30-70°C, and the time is 20-120 minutes;
[0013] To inactivate the enzyme, increase the pH or the temperature to 75-95°C for 10-20 minutes, and then or simultaneously wash with water;
[0014] The oxygen bleaching treatment includes padding with hydrogen peroxide bleaching liquid and steaming, wherein the bleaching liquid is composed of 30% hydrogen peroxide, sodium silicate, and the pH is adjusted to 9-11, the steaming temperature is 50-120°C, the time is 20-120 minutes, and then fully washed with water.
[0015] Preferably, the washing method includes pre-treating, washing, rinsing, dehydrating and drying the fabric, adding detergent, softener and water during the washing process, adjusting the water temperature and water level, and washing. The washing method is: taking the viscose fabric and placing it in a washing machine, leveling the fabric after washing to obtain a fabric washing material, and the washing also includes sand washing, neutralization and re-washing. The sand washing is to place the fabric washing material in an industrial washing machine, and then add water, soda ash and a multifunctional finishing agent in sequence, first heating each material to 85-90°C and then cooling to room temperature to obtain a fabric sand washing material; the neutralization is to add a neutralizing acid to the fabric sand washing material for neutralization to obtain a fabric neutralized material; the re-washing is to add water to the fabric neutralized material, wash off the neutralizing acid on the fabric neutralized material, and dry to obtain a viscose fiber fabric.
[0016] Preferably, the tenter drying utilizes the plasticity of certain fibers under wet conditions to gradually widen the width of the fabric to a specified size, and then dries the fabric to stabilize the shape of the fabric and reduce deformation during use. The tenter drying uses a tenter dryer for heating, and the heating method is to install an infrared heating tube in the tenter dryer, and utilize infrared light waves and hot air to act on the fabric together to accelerate the drying of internal moisture.
[0017] Preferably, the long-line continuous pad dyeing includes pad dyeing, color fixing, flat washing, drying and steaming.
[0018] Preferably, the soft stretching is performed by treating with a softener, and then utilizing the plasticity of certain fibers in a wet state or the thermoplasticity of synthetic fibers to slowly stretch the width of the fabric to a specified size, eliminate some internal stress, adjust the state of the warp and weft yarns in the fabric, and make the width of the fabric uniform and the shape stable.
[0019] Preferably, the shrinkage-proof treatment method is to reduce the hydrophilicity of the fiber or treat the fabric with chemical agents such as resin shrinkage bodies and cross-linking agents to reduce the swelling and shrinkage of the fiber in water.
[0020] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0021] The invention improves the wet strength and glossiness of viscose fiber fabrics, reduces production costs and environmental pollution, namely reduces sewage by two-thirds, improves production efficiency and product quality, is suitable for the production of various viscose fabrics, has broad application prospects, and uses water washing, sand washing, neutralization, and water washing again to treat fabric raw materials with soda ash, a multifunctional finishing agent, and a neutralizing acid, thereby increasing the softness, whiteness, and water absorption of the prepared fabric, so that the fabric has good hand feel and color. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the continuous pre-treatment process flow of the viscose fabric of the present invention; DETAILED DESCRIPTION
[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.
[0024] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0025] The embodiment of the present invention provides a continuous pretreatment process for viscose fabric, as shown in the figure, comprising the following steps: turning over the seam ends of the grey cloth, singeing, rolling bio-enzyme stacking, padding bio-enzyme loose steaming, washing, wet dropping, tenter drying, long-line continuous pad dyeing, soft tentering and shrinkage-proof treatment, the rolling bio-enzyme stacking time is 20-25°C / 6-8 hours, the padding bio-enzyme loose steaming time is 95-98°C / 30 minutes, and the production speed is 80 meters / minute.
[0026] The existing technical process is: grey cloth turning over the seam ends-----singeing----overflow cylinder for enzyme retardation and alkaline oxygen bleaching (bath ratio 1:18-20)----water washing----overflow dyeing----water washing----acid neutralization----dehydration----stretching and drying----soft stretching----calendering----anti-shrinkage----finished product.
[0027] The production is time-consuming, intermittent, and the pre-treatment process consumes a lot of material. The reactive dyeing time is longer. It is easy to produce cylinder difference, the cloth surface is not smooth, there are many short hairs, the cloth surface taste is poor, and customer satisfaction is poor. The tear strength and wet strength of the finished fabric are poor, and the finished fabric is prone to wrinkles.
[0028] The process of the present invention is: turning over the seam ends of the grey cloth, singeing, rolling bio-enzyme stacking (20-25°C / 6-8 hours), rolling bio-enzyme loose steaming (95-98°C / 30 minutes, production speed 80 meters / minute), washing, wet dropping, stenter drying, long-line continuous roller dyeing, soft stentering, shrinkage prevention, and finished product.
[0029] The invention has short production time and continuous production, and the consumption of the pre-treatment process is small; the continuous dyeing time of the reactive dye is short; the cloth surface is smooth and clean, the cloth surface taste is good, and the customer satisfaction is high; the finished fabric has the tear strength and wet strength; the cloth surface is flat, smooth and soft.
[0030] The process of turning the grey fabric and sewing the ends includes: first check the quality of the grey fabric and classify it according to its length, width, weight, etc.; unroll the grey fabric on the roll to check if there are any defects or stains on the fabric and ensure that the fabric is flat. When turning the fabric, make sure that the fabric is not stretched or compressed unnecessarily; divide the grey fabric into appropriate batches according to production requirements, and the quantity of each batch should be suitable for subsequent processing; print the batch number, fabric type, length and other information at the designated position of the grey fabric for subsequent tracking and management; sew strong threads on both ends of each piece of fabric to prevent the fabric from frayed or damaged during processing, and use threads with a contrasting color to the grey fabric; reroll the grey fabric after turning it, ensure that the roll is tight and flat, and avoid wrinkles or curling; record the detailed information of each batch of grey fabric, including batch number, total length, weight, etc., for inventory management and quality tracking; store the processed grey fabric in a suitable environment to avoid direct sunlight, moisture or pollution; after the turning and sewing of the grey fabric is completed, the next step of pre-processing can be carried out.
[0031] The singeing method is: cutting burning, one positive and one negative, 120m / min, the front side of singeing is cutting burning, and the singeing flame temperature is 900~1000℃.
[0032] Alkaline pectinase is used in rolling bio-enzyme stacking. Wetting and penetrating agent is added to the alkaline pectinase. The pH value of the enzyme treatment solution is usually controlled between 8.6-10.0. During the heat preservation stacking process, unsaturated steam is used for steaming. The steaming temperature is controlled at 45-65℃ and the time is within 30-100 minutes.
[0033] The padding bio-enzyme loose steaming process includes the following steps:
[0034] Pretreatment, the fabric is first soaked in cold water and then pretreated with hot water to remove some of the size and impurities;
[0035] Desizing enzyme treatment, including padding desizing enzyme solution and steaming, using α-amylase treatment solution, pH value controlled at 6-7, liquid carrying rate at 50%-120%, steaming conditions at 50-100°C, time 20-120 minutes;
[0036] Washing: After desizing enzyme treatment, the cotton fabric must be fully washed to remove the size on the surface;
[0037] Bio-enzyme scouring treatment, including padding with bio-enzyme scouring solution and steaming, the composition of the enzyme scouring solution may include pectinase and cellulase, and non-ionic or anionic surfactant as a wetting and penetrating agent, the steaming temperature is 30-70°C, and the time is 20-120 minutes;
[0038] To inactivate the enzyme, increase the pH or the temperature to 75-95°C for 10-20 minutes, and then or simultaneously wash with water;
[0039] The oxygen bleaching treatment includes padding with hydrogen peroxide bleaching liquid and steaming, wherein the bleaching liquid is composed of 30% hydrogen peroxide, sodium silicate, and the pH is adjusted to 9-11, the steaming temperature is 50-120°C, the time is 20-120 minutes, and then fully washed with water.
[0040] The washing method includes pre-treatment, washing, rinsing, dehydration and drying of the fabric. Detergent, softener and water are added during the washing process, and the water temperature and water level are adjusted to wash. The washing method is: taking the viscose fabric and placing it in a washing machine, leveling the fabric after washing to obtain a fabric washing material, and further comprising sand washing, neutralization and re-washing after washing. Sand washing, placing the fabric washing material in an industrial washing machine, then adding water, soda ash and a multifunctional finishing agent in sequence, first heating each material to 85-90°C and then cooling to room temperature to obtain a fabric sand washing material; neutralization, adding a neutralizing acid to the fabric sand washing material for neutralization to obtain a fabric neutralized material; re-washing, adding water to the fabric neutralized material, washing off the neutralizing acid on the fabric neutralized material, and drying to obtain the viscose fiber fabric.
[0041] Preferably, the washing machine is a three-tank washing machine, and the water temperatures in the three tanks are respectively in the ranges of 30-35°C, 70-75°C, and 30-35°C;
[0042] Preferably, the heating rate of the fabric washing material is 2-3°C / min, and the cooling rate is 6-7°C / min;
[0043] Preferably, the mass ratio of soda ash to water is (10-15):1000;
[0044] Preferably, the mass ratio of the multifunctional finishing agent to water is (1-3): 1000;
[0045] Preferably, the multifunctional finishing agent is mainly composed of 70-80 parts by mass of aminoethylaminopropyl polydimethylsiloxane and 30-40 parts by mass of polyvinyl amide by stirring and mixing;
[0046] Preferably, the functional finishing agent further comprises 2-4 parts of dopamine;
[0047] Preferably, the neutralization time of the fabric sand washing material is 5-10min;
[0048] Preferably, the neutralizing acid is glacial acetic acid, citric acid or a mixture of both, and the mass ratio of the neutralizing acid to water is (5-10):1000.
[0049] Tenter drying uses the plasticity of certain fibers under wet conditions to gradually widen the width of the fabric to a specified size, and then dries it to stabilize the shape of the fabric and reduce deformation during use. Tenter drying uses a tenter dryer for heating. The heating method is to install infrared heating tubes in the tenter dryer, and use infrared light waves and hot air to act on the fabric together to speed up the drying of internal moisture.
[0050] Long-line continuous pad dyeing includes pad dyeing, color fixing, flat washing, drying and steaming.
[0051] Soft stretching is to use softener treatment, and then use the plasticity of certain fibers in a wet state or the thermoplasticity of synthetic fibers to slowly stretch the width of the fabric to a specified size, eliminate some internal stress, adjust the state of the warp and weft yarns in the fabric, and make the width of the fabric uniform and the shape stable.
[0052] The shrinkage-proof treatment method is to reduce the hydrophilicity of the fiber or treat the fabric with chemical agents such as resin shrinkage agents and cross-linking agents to reduce the swelling and shrinkage of the fiber in water.
[0053] Example:
[0054] For example: Product specification 30 s *30 s / 80*68 reactive dyes dark navy data comparison is as follows:
[0055]
[0056]
[0057]
[0058] The present invention can effectively improve the gloss of the viscose fabric surface, and the wet strength is greatly improved. The process is simple, feasible and economical, and is suitable for the production of various viscose fabrics. The continuous pretreatment process of the present invention has broad application prospects in the field of textile technology.
[0059] It should be noted that, for the above-mentioned embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the described order of actions, because according to the present invention, some steps may be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present invention.
[0060] In the several embodiments provided in the present application, it should be understood that the disclosed devices can be implemented in other ways. For example, the device embodiments described above are merely schematic, such as the division of the above-mentioned units. There may be other division methods in actual implementation, such as multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or communication connection shown or discussed can be through some interfaces, and the indirect coupling or communication connection between devices or units can be in the form of telecommunication or other forms.
[0061] The units described above as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed on multiple network units. Some or all of the units may be selected according to actual needs to achieve the purpose of the solution of this embodiment.
[0062] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still combine, add, delete or make other adjustments to the features in the various embodiments of the present invention according to the circumstances without conflict, without making creative work, so as to obtain different other technical solutions that do not deviate from the concept of the present invention in essence, and these technical solutions also belong to the scope of protection of the present invention.
Claims
1. A continuous pre-treatment process for viscose fabrics, characterized in that: The following steps are involved: The grey cloth is subjected to cloth turning, seaming, singeing, bio-enzyme padding, bio-enzyme loose steaming, washing, wet dropping, tentering and drying, long-line continuous pad dyeing, soft tentering and shrinkage prevention treatment. The bio-enzyme padding time is 20-25°C / 6-8 hours, the bio-enzyme loose steaming time is 95-98°C / 30 minutes, and the production speed is 80 m / min.
2. The continuous pretreatment process of viscose fabric according to claim 1, characterized in that: The grey fabric turning and sewing process includes: first checking the quality of the grey fabric and classifying it according to the length, width, weight, etc. of the fabric; unrolling the grey fabric on the roll to check whether there are defects or stains on the fabric surface and ensure that the fabric surface is flat. When turning the fabric, ensure that the fabric is not stretched or compressed unnecessarily; divide the grey fabric into appropriate batches according to production requirements, and the quantity of fabric in each batch should be suitable for subsequent processing; print the batch number, fabric type, length and other information at the designated position of the grey fabric for subsequent tracking and management; sew strong threads at both ends of each piece of fabric to prevent the fabric from loosening or being damaged during processing, and the seam line is a thread with a sharp contrast to the color of the grey fabric; re-roll the grey fabric after turning the fabric to ensure that the roll is tight and flat to avoid wrinkles or curling; record the detailed information of each batch of grey fabric, including batch number, total length, weight, etc., for inventory management and quality tracking; store the processed grey fabric in a suitable environment to avoid direct sunlight, moisture or pollution; after the grey fabric turning and sewing process is completed, the next step of pre-processing can be carried out.
3. The continuous pretreatment process of viscose fabric according to claim 2, characterized in that: The singeing method is: cutting burning, one front and one back, 120m / min, the front side of the singeing is cutting burning, and the singeing flame temperature is 900-1000°C.
4. The continuous pretreatment process for viscose fabric according to claim 1, characterized in that: The rolling bio-enzyme stacking adopts alkaline pectinase, and a wetting and penetrating agent is added to the alkaline pectinase. The pH value of the enzyme treatment solution is usually controlled between 8.6 and 10.
0. During the heat preservation stacking process, unsaturated steam is used for steaming, and the steaming temperature is controlled at 45-65° C. for 30-100 minutes.
5. The continuous pre-treatment process of viscose fabric according to claim 1, characterized in that: The padding bio-enzyme loose steaming comprises the following steps: Pretreatment, the fabric is first soaked in cold water and then pretreated with hot water to remove some of the size and impurities; Desizing enzyme treatment, including padding desizing enzyme solution and steaming, using α-amylase treatment solution, pH value controlled at 6-7, liquid carrying rate at 50%-120%, steaming conditions at 50-100°C, time 20-120 minutes; Washing: After desizing enzyme treatment, the cotton fabric must be fully washed to remove the size on the surface; Bio-enzyme scouring treatment, including padding with bio-enzyme scouring solution and steaming, the composition of the enzyme scouring solution may include pectinase and cellulase, and non-ionic or anionic surfactant as a wetting and penetrating agent, the steaming temperature is 30-70°C, and the time is 20-120 minutes; To inactivate the enzyme, increase the pH or the temperature to 75-95°C for 10-20 minutes, and then or simultaneously wash with water; The oxygen bleaching treatment includes padding with hydrogen peroxide bleaching liquid and steaming, wherein the bleaching liquid is composed of 30% hydrogen peroxide, sodium silicate, and the pH is adjusted to 9-11, the steaming temperature is 50-120°C, the time is 20-120 minutes, and then fully washed with water.
6. The continuous pre-treatment process of viscose fabric according to claim 1, characterized in that: The washing method includes pre-treating, washing, rinsing, dehydrating and drying the fabric. Detergent, softener and water are added during the washing process, and the water temperature and water level are adjusted to wash. The washing method is: taking the viscose fabric and placing it in a washing machine, leveling the fabric after washing to obtain a fabric washing material. The washing also includes sand washing, neutralization and re-washing. The sand washing is to place the fabric washing material in an industrial washing machine, and then add water, soda ash and a multifunctional finishing agent in sequence, first heat up the materials to 85-90° C. and then cool to room temperature to obtain a fabric sand washing material; the neutralization is to add a neutralizing acid to the fabric sand washing material for neutralization to obtain a fabric neutralized material; the re-washing is to add water to the fabric neutralized material, wash off the neutralizing acid on the fabric neutralized material, and dry to obtain the viscose fiber fabric.
7. The continuous pre-treatment process for viscose fabric according to claim 1, characterized in that: The tenter drying utilizes the plasticity of certain fibers under wet conditions to gradually widen the width of the fabric to a specified size, and then dries the fabric to stabilize the shape of the fabric and reduce deformation during use. The tenter drying uses a tenter dryer for heating. The heating method is to install an infrared heating tube in the tenter dryer, and utilize infrared light waves and hot air to act on the fabric together to accelerate the drying of internal moisture.
8. The continuous pre-treatment process for viscose fabric according to claim 1, characterized in that: The long-line continuous pad dyeing includes pad dyeing, color fixing, flat washing, drying and steaming.
9. The continuous pre-treatment process for viscose fabric according to claim 1, characterized in that: The soft stretching is to use a softener treatment, and then use the plasticity of certain fibers in a wet state or the thermoplasticity of synthetic fibers to slowly stretch the width of the fabric to a specified size, eliminate part of the internal stress, adjust the state of the warp and weft yarns in the fabric, and make the width of the fabric uniform and the shape stable.
10. The continuous pre-treatment process of viscose fabric according to claim 1, characterized in that: The shrink-proof treatment method is to reduce the hydrophilicity of the fiber or use chemical agents such as resin shrinkage bodies and cross-linking agents to treat the fabric to reduce the swelling and shrinkage of the fiber in water.