Polyurethane (PU) synthetic leather resistant to strong polar solvent and strong acid and base as well as preparation method and application of PU synthetic leather

Through the multi-layer structure and optimized formula preparation method, the problem of insufficient chemical resistance of traditional PU synthetic leather in strong polar solvents and strong acid and alkali environments is solved, and higher heat resistance, weather resistance and Acid and alkali resistance, suitable for passenger car interiors.

CN118932735AInactive Publication Date: 2024-11-12SEIREN SUZHOU CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411189677.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional PU synthetic leather has weak chemical resistance when facing strong polar solvents and strong acid and alkali environments, making it difficult to meet the corrosion resistance needs of passenger car interior materials.

Method used

The preparation method of PU synthetic leather with a multi-layer structure includes a surface layer, a subsequent layer, a first surface treatment layer and a second surface treatment layer. By optimizing the formulation and process, fluorine-containing additives and polyacrylic thickeners are added. Components, improve acid and alkali resistance and chemical resistance, and enhance interlayer adhesion and hardness through two surface treatment layers.

Benefits of technology

It significantly improves the heat, weather resistance and acid and alkali resistance of PU synthetic leather, enhances its application suitability in passenger car interiors, and has high tear resistance and peeling strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932735A_ABST
    Figure CN118932735A_ABST
Patent Text Reader

Abstract

The invention discloses PU (Poly Urethane) synthetic leather resistant to a strong polar solvent and strong acid and alkali as well as a preparation method and application of the PU synthetic leather. The PU synthetic leather structurally comprises a base cloth layer, a bonding layer, a surface layer, a first surface treatment layer and a second surface treatment layer which are sequentially stacked. The preparation method comprises the following steps: S1, manufacturing the surface layer; s2, manufacturing a bonding layer; s3, laminating the base cloth; s4, performing curing treatment; s5, stripping is carried out; s6, first surface layer treatment; and S7, second surface layer treatment. The strength, the heat resistance, the weather resistance and the acid and alkali resistance of the PU synthetic leather are improved by optimizing the structure of the synthetic leather and optimizing the formula and the preparation process of the surface layer and the surface treatment layer. The composite material is applied to passenger car interiors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of artificial leather, and in particular relates to PU synthetic leather resistant to strong polar solvents and strong acids and alkalis, and a preparation method and application thereof. Background Art

[0002] Many existing PU leather materials at home and abroad have high requirements for the chemical resistance of synthetic leather in many design or coating processes. Due to the chemical properties of polyurethane materials themselves, traditional PU synthetic leather is subject to the physical and chemical properties of polyurethane materials themselves. PU leather is relatively weak in acid, alkali and chemical resistance. Improving the chemical corrosion resistance of passenger car interior materials will be the key research direction of PU leather for a long time. Therefore, the present invention is derived from this. Summary of the invention

[0003] In view of one of the above-mentioned technical problems, the object of the present invention is to provide a PU synthetic leather resistant to strong polar solvents and strong acids and alkalis, and a preparation method and application thereof.

[0004] The technical solution of the present invention is:

[0005] One of the objects of the present invention is to provide a method for preparing a PU synthetic leather resistant to strong polar solvents and strong acids and bases, comprising the following steps:

[0006] S1. Surface layer preparation: first prepare the surface layer solution, then perform degassing treatment, coating processing and surface layer drying and molding;

[0007] S2, adhesive layer preparation: first prepare adhesive layer solution, then carry out coating process, adhesive layer drying and forming;

[0008] S3, base fabric bonding: bonding the surface layer obtained in step S1, the adhesive layer obtained in step S2 and the base fabric layer together to form a composite leather blank;

[0009] S4, aging treatment: aging the composite leather stock obtained in step S3 in an oven to form an aged leather stock;

[0010] S5, peeling: peeling the aged leather stock obtained in step S4 from the release paper transfer mold to obtain a PU leather stock;

[0011] S6, surface layer treatment 1: prepare the first surface treatment layer solution, the first surface treatment layer solution is an aqueous polyurethane solution containing fluorine additives and has a viscosity of 300cps to 500cps, and apply the first surface treatment layer solution on the surface of the PU leather blank obtained in S5, with an amount of 10g / m 2 ~15g / m 2 , and then baked to obtain semi-finished PU leather;

[0012] S7, surface layer treatment 2: prepare the second surface treatment layer solution, which is an aqueous polyurethane solution containing fluorine additives and has a viscosity of 500cps to 700cps. Apply the second surface treatment layer solution on the surface of the semi-finished PU leather obtained in S6, with a usage amount of 25g / m 2 ~30g / m 2 , and then baked to obtain the finished PU leather.

[0013] Preferably, the surface layer solution in step S1 comprises, by weight: 65 to 70 parts of aqueous aliphatic polyurethane, 10 to 15 parts of polytetrafluoroethylene, 2 to 4 parts of bridging agent, 5 to 8 parts of pigment, and 10 to 13 parts of water;

[0014] The stirring speed of the surface layer solution is 400 rpm, the stirring time is 30 minutes, and the viscosity of the surface layer solution is 3000±500 cps; the prepared surface layer solution is degassed by a circulating degassing machine, and the degassing time of the surface layer solution is 50 minutes. During the circulating degassing, air is prevented from entering to improve the uniformity of the surface layer coating;

[0015] The surface layer solution coating process speed is 10m / min, and the usage is 40±5g / m 2 ;

[0016] The temperature for drying and forming the surface layer is 100°C, the oven length is 30m, and the baking time is 3min. The bridging agent in the present invention is a blocked isocyanate bridging agent with a solid content of 41%. The pigment can be carbon black. Compared with the existing ordinary PU synthetic leather, the PU synthetic leather of the present invention also has a fluorine-containing additive (polytetrafluoroethylene) added to the surface layer, which can react with the polyurethane material without producing additives. Moreover, through the optimization of the formula, the wettability is improved, which is more conducive to the adhesion of the first surface layer, the second surface layer and the adhesive layer.

[0017] Preferably, the bonding layer solution in step S2 comprises, by weight: 40 to 45 parts of polycarbonate polyol resin, 35 to 40 parts of yellowing-resistant aliphatic diisocyanate, 1 to 4 parts of amine organic acid salt catalyst, and 18 to 24 parts of magnesium hydroxide halogen-free environmentally friendly flame retardant;

[0018] In step S2, the stirring speed of preparing the bonding layer solution is 2500 rpm, and the stirring time is 48 hours;

[0019] The coating speed of the next layer solution is 10m / min, and the amount used is 200±20g / m 2 ;

[0020] The temperature of the next layer drying molding is 90℃~110℃, the oven length is 30m, the baking time is 3min; the drying degree of the next layer is 80%~90%. The viscosity of the polycarbonate polyol resin of the present invention is 4000cps, and the yellowing-resistant aliphatic diisocyanate contains 17% isocyanate group (NCO).

[0021] Preferably, the first surface treatment layer solution in step S6 comprises, by weight: 70-75 parts of waterborne polyurethane, 5-8 parts of carbodiimide, 10-15 parts of fluorine-containing acrylate, and 5-10 parts of water. The fluorine content of the fluorine-containing acrylate is 5% and the solid content is 35%.

[0022] Preferably, the second surface treatment layer solution in step S7 includes: 70 to 75 parts of waterborne polyurethane, 2 to 4 parts of carbodiimide, 1 to 3 parts of polyacrylic thickener, 3 to 7 parts of silicon oxide polymer resin, 10 to 15 parts of fluorinated acrylate, and 5 to 10 parts of water. In the present invention, the solid content of the polyacrylic thickener is 5%-10%. The solid content of the silicon oxide polymer resin is 100%. The fluorine content of the fluorinated acrylate is 5% and the solid content is 35%.

[0023] As can be seen from the above, there are some differences in the formula between the first surface treatment layer solution and the second surface treatment layer solution, which is mainly reflected in the fact that the second surface treatment layer solution contains more polyacrylic thickeners and silicon oxide polymer resins, and the amount of carbodiimide in the second surface treatment layer solution is less than that of the first surface treatment layer solution. The purpose of the first surface treatment layer solution is not only to improve the acid and alkali resistance and chemical resistance of PU synthetic leather by adding fluorinated acrylates, but also to enhance the bonding effect with the surface layer, that is, to increase the interlayer adhesion. The formula of the second surface treatment layer solution has been appropriately adjusted. Its main purpose is still to further enhance the acid and alkali resistance and chemical resistance by adding fluorinated acrylates, and another purpose is to shape, improve interlayer adhesion, increase strength and increase the hardness and peeling force of PU synthetic leather. The peeling force can reach more than 12N after testing. In addition, the surface tension of fluorinated acrylates is low, so that PU synthetic leather has very good tear resistance, which is very suitable for passenger cars.

[0024] Preferably, in step S3, the base fabric is a weft-knitted fabric, the thickness of the base fabric is 0.9±0.05 cm, and the mass surface density is 300±30 g / m 2 ; and / or

[0025] The bonding speed is 10m / min and the bonding pressure is 0.3MPa; and / or

[0026] In step S5, the temperature of the aging treatment is 130° C., the length of the oven is 120 m, and the baking time is 12 min; and / or

[0027] The production environment temperature of step S1 to step S7 is 0°C to 35.0°C, and the production environment humidity is 25% to 75%.

[0028] Preferably, in step S6, the stirring speed of preparing the first surface treatment layer solution is 400 rpm, and the stirring time is 30 min;

[0029] The speed of the first surface treatment layer solution coating process is 10m / min;

[0030] The baking molding temperature of the first surface treatment layer is 100.0°C to 130.0°C, the oven length is 25m, and the baking time is 2.5min.

[0031] Preferably, in step S7, the stirring speed of preparing the second surface treatment layer solution is 400 rpm, and the stirring time is 30 min;

[0032] The speed of the second surface treatment layer solution coating process is 10m / min;

[0033] The baking molding temperature of the second surface treatment layer is 100.0°C to 130.0°C, the oven length is 25m, and the baking time is 2.5min.

[0034] Another object of the present invention is to provide a PU synthetic leather resistant to strong polar solvents and strong acids and alkalis, comprising a base fabric layer, an adhesive layer, a surface layer, a first surface treatment layer and a second surface treatment layer stacked in sequence, wherein the PU synthetic leather is made by any of the preparation methods described above.

[0035] Another object of the present invention is to provide the use of the above-mentioned PU synthetic leather or the PU synthetic leather prepared by any of the above-mentioned preparation methods in passenger car interiors.

[0036] Compared with the prior art, the advantages of the present invention are:

[0037] The present invention optimizes the structure of synthetic leather and the formula and preparation process of the surface layer and the surface treatment layer, thereby improving the strength, heat resistance, weather resistance and acid and alkali resistance of PU synthetic leather, and applies it to the interior decoration of passenger cars. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0039] Figure 1 This is a cross-sectional structural diagram of existing common PU synthetic leather;

[0040] Figure 2 This is a cross-sectional structural diagram of a PU synthetic leather resistant to strong polar solvents and strong acids and alkalis according to an embodiment of the present invention;

[0041] Figure 3 This is a photo of the test results of chemical resistance and washability of ordinary PU synthetic leather in Comparative Example 3;

[0042] Figure 4 This is a photograph of the test results of chemical resistance and washability of the PU synthetic leather resistant to strong polar solvents and strong acids and alkalis according to Example 3 of the present invention.

[0043] Wherein: 10, base fabric layer; 20, adhesive layer; 30, surface layer; 40, first surface treatment layer; 50, second surface treatment layer. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0045] Example 1

[0046] This embodiment provides a method for preparing solvent-resistant and strong acid-base resistant PU synthetic leather, comprising the following steps:

[0047] First, prepare the release paper transfer film and the base fabric layer, wherein the base fabric layer is a weft knitted fabric with a thickness of (0.9±0.05) cm and a mass surface density of (300±20) g / m 2 The production environment temperature is 0.0℃~35.0℃, and the production environment humidity is 25%~75%.

[0048] S1. Surface layer production:

[0049] (1) According to the material components of the surface layer, prepare the raw materials according to the following mass parts: 65 parts of water-based aliphatic polyurethane, 15 parts of polytetrafluoroethylene, 2 parts of bridging agent E-05-MP, 8 parts of pigment, and 10 parts of water;

[0050] (2) Mixing the raw materials prepared in step (1) to prepare a surface layer solution, the stirring speed of the surface layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the obtained surface layer solution is 3500 cps;

[0051] (3) The surface layer solution is fully degassed using a circulating degassing machine for 50 minutes;

[0052] (4) The surface layer solution is coated at a speed of 10 m / min and a usage of 40 g / m 2 ;

[0053] (5) Then the product is dried and formed at a temperature of 100°C, an oven length of 30m, and a time of 3min.

[0054] S2. Making the next layer:

[0055] (1) According to the material components of the adhesive layer, the raw materials are prepared according to the following mass parts: 40 parts of polycarbonate polyol resin, 40 parts of yellowing-resistant aliphatic diisocyanate, 1 part of amine organic acid salt catalyst, and 18 parts of magnesium hydroxide halogen-free environmentally friendly flame retardant;

[0056] (2) Mixing the raw materials prepared in step (1) to prepare a bonding layer solution, wherein the bonding layer solution is stirred at a speed of 2500 rpm for 48 hours;

[0057] (3) The adhesive solution was applied at a speed of 10 m / min and a usage of 200 g / m 2 ;

[0058] (4) Then, the adhesive layer is dried and formed. The drying and forming temperature of the adhesive layer is 90° C., the length of the oven is 30 m, the baking time is 3 min, and the drying degree of the adhesive layer is 80%.

[0059] S3, base fabric bonding: the surface layer obtained in step S1, the adhesive layer obtained in step S2 and the base fabric layer are bonded together to form a composite leather blank; the base fabric bonding speed is 10 m / min, and the bonding pressure is 0.3 MPa.

[0060] S4, aging treatment: the composite leather stock obtained in step S4 is aged in an oven and cooled to obtain an aged leather stock; the aging treatment temperature is 120° C., the oven length is 120 m, and the baking time is 12 min.

[0061] S5, peeling: peeling the aged leather blank obtained in step S4 from the release paper transfer mold to obtain a PU leather blank.

[0062] S6, surface treatment 1:

[0063] (1) According to the material components of the surface treatment layer solution for the surface layer treatment, raw materials are prepared according to the following mass parts: 70 parts of waterborne polyurethane, 8 parts of carbodiimide, 15 parts of fluorine-containing acrylate, and 5 parts of water;

[0064] (2) Mixing the raw materials prepared in step (1) to prepare a first surface treatment layer solution, the stirring speed of the first surface treatment layer solution is adjusted to 400 rpm, the stirring time is 30 min, and the viscosity of the first surface treatment layer solution is 500 cps;

[0065] (3) The first surface treatment layer solution is coated on the surface layer at a coating speed of 10.0 m / min and a usage of 10 g / m 2 The baking molding temperature of the first surface treatment layer solution is 100°C, the oven length is 25m, and the baking time is 2.5min to obtain a semi-finished PU leather.

[0066] S7, surface treatment 2:

[0067] (1) According to the material components of the surface treatment layer solution of the surface treatment layer, raw materials are prepared according to the following mass parts: 70 parts of waterborne polyurethane, 4 parts of carbodiimide, 1 part of polyacrylic thickener, 7 parts of silicon oxide polymer resin, 10 parts of fluorine-containing acrylate, and 10 parts of water;

[0068] (2) Mixing the raw materials prepared in step (1) to prepare a second surface treatment layer solution, the stirring speed of the second surface treatment layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the second surface treatment layer solution is 700 cps;

[0069] (3) The second surface treatment layer solution is coated on the surface of the semi-finished PU leather, i.e., the first surface treatment layer, at a coating speed of 10.0 m / min and a usage of 25 g / m 2 The baking molding temperature of the second surface treatment layer is 100°C, the oven length is 25m, and the baking time is 2.5min to obtain the finished PU leather.

[0070] The solvent-resistant and strong acid-base PU synthetic leather prepared according to the above method includes a base fabric layer 10, an adhesive layer 20, a surface layer 30, a first surface treatment layer 40 and a second surface treatment layer 50, wherein the first surface treatment layer 40 and the second surface treatment layer 50 have different components and different coating amounts, i.e., thicknesses. The preparation method is specifically described above, and the performance is tested. The results are shown in Table 1.

[0071] Example 2

[0072] This embodiment provides a method for preparing solvent-resistant and strong acid-base resistant PU synthetic leather, comprising the following steps:

[0073] First, prepare the release paper transfer film and the base fabric layer, wherein the base fabric layer is a weft knitted fabric with a thickness of (0.9±0.05) cm and a mass surface density of (300±20) g / m 2 The production environment temperature is 0.0℃~35.0℃, and the production environment humidity is 25%~75%.

[0074] S1. Surface layer production:

[0075] (1) According to the material components of the surface layer, raw materials are prepared according to the following mass parts: 70 parts of water-based aliphatic polyurethane, 10 parts of polytetrafluoroethylene, 4 parts of bridging agent, 5 parts of pigment, and 13 parts of water;

[0076] (2) Mixing the raw materials prepared in step (1) to prepare a surface layer solution, the stirring speed of the surface layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the obtained surface layer solution is 2500 cps;

[0077] (3) The surface layer solution is fully degassed using a circulating degassing machine for 50 minutes;

[0078] (4) The surface layer solution is coated at a speed of 10 m / min and a usage of 40 g / m 2 ;

[0079] (5) Then the product is dried and formed at a temperature of 100°C, an oven length of 30m, and a time of 3min.

[0080] S2. Making the next layer:

[0081] (1) According to the material components of the adhesive layer, the raw materials are prepared according to the following mass parts: 45 parts of polycarbonate polyol resin, 35 parts of yellowing-resistant aliphatic diisocyanate, 4 parts of amine organic acid salt catalyst, and 22 parts of magnesium hydroxide halogen-free environmentally friendly flame retardant;

[0082] (2) Mixing the raw materials prepared in step (1) to prepare a bonding layer solution, wherein the bonding layer solution is stirred at a speed of 2500 rpm for 48 hours;

[0083] (3) The adhesive solution was applied at a speed of 10 m / min and a usage of 200 g / m 2 ;

[0084] (4) Then, the adhesive layer is dried and formed. The drying and forming temperature of the adhesive layer is 90° C., the length of the oven is 30 m, the baking time is 3 min, and the drying degree of the adhesive layer is 80%.

[0085] S3, base fabric bonding: the surface layer obtained in step S1, the adhesive layer obtained in step S2 and the base fabric layer are bonded together to form a composite leather blank; the bonding speed is 10 m / min, and the bonding pressure is 0.3 MPa.

[0086] S4, aging treatment: the composite leather stock obtained in step S4 is aged in an oven and cooled to obtain an aged leather stock; the aging treatment temperature is 120° C., the oven length is 120 m, and the baking time is 12 min.

[0087] S5, peeling: peeling the aged leather blank obtained in step S4 from the release paper transfer mold to obtain a PU leather blank.

[0088] S6, surface treatment 1:

[0089] (1) According to the material components of the surface treatment layer solution for the surface layer treatment, raw materials are prepared according to the following mass parts: 75 parts of waterborne polyurethane, 5 parts of carbodiimide, 10 parts of fluorine-containing acrylate, and 10 parts of water;

[0090] (2) Mixing the raw materials prepared in step (1) to prepare a first surface treatment layer solution, the stirring speed of the first surface treatment layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the first surface treatment layer solution is 300 cps;

[0091] (3) The first surface treatment layer solution is coated on the surface layer at a coating speed of 10.0 m / min and a usage of 15 g / m 2 The baking molding temperature of the first surface treatment layer is 100° C., the oven length is 25 m, and the baking time is 2.5 min to obtain a semi-finished PU leather.

[0092] S7, surface treatment 2:

[0093] (1) According to the material components of the surface treatment layer solution for the surface layer treatment, raw materials are prepared according to the following mass parts: 75 parts of waterborne polyurethane, 2 parts of carbodiimide, 5 parts of polyacrylic thickener, 3 parts of silicon oxide polymer resin, 3 parts of fluorine-containing acrylate, and 15 parts of water;

[0094] (2) Mixing the raw materials prepared in step (1) to prepare a second surface treatment layer solution, the stirring speed of the second surface treatment layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the second surface treatment layer solution is 500 cps;

[0095] (3) The second surface treatment layer solution is coated on the surface of the semi-finished PU leather, i.e., the first surface treatment layer, at a coating speed of 10.0 m / min and a usage of 30 g / m 2 The baking molding temperature of the second surface treatment layer is 100°C, the oven length is 25m, and the baking time is 2.5min to obtain the finished PU leather.

[0096] The solvent-resistant and strong acid-base PU synthetic leather prepared according to the above method includes a base fabric layer 10, an adhesive layer 20, a surface layer 30, a first surface treatment layer 40 and a second surface treatment layer 50, wherein the first surface treatment layer 40 and the second surface treatment layer 50 have different components and different coating amounts, i.e., thicknesses. The preparation method is specifically described above, and the performance is tested. The results are shown in Table 1.

[0097] Example 3

[0098] This embodiment provides a method for preparing solvent-resistant and strong acid-base resistant PU synthetic leather, comprising the following steps:

[0099] First, prepare the release paper transfer film and the base fabric layer, wherein the base fabric layer is a weft knitted fabric with a thickness of (0.9±0.05) cm and a mass surface density of (300±20) g / m 2 The production environment temperature is 0.0℃~35.0℃, and the production environment humidity is 25%~75%.

[0100] S1. Surface layer production:

[0101] (1) According to the material components of the surface layer, raw materials are prepared according to the following mass parts: 68 parts of water-based aliphatic polyurethane, 13 parts of polytetrafluoroethylene, 3 parts of bridging agent, 6 parts of pigment, and 12 parts of water;

[0102] (2) Mixing the raw materials prepared in step (1) to prepare a surface layer solution, the stirring speed of the surface layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the obtained surface layer solution is 3000 cps;

[0103] (3) The surface layer solution is fully degassed using a circulating degassing machine for 50 minutes;

[0104] (4) The surface layer solution is coated at a speed of 10 m / min and a usage of 40 g / m 2 ;

[0105] (5) Then the product is dried and formed at a temperature of 100°C, an oven length of 30m, and a time of 3min.

[0106] S2. Making the next layer:

[0107] (1) According to the material components of the bonding layer, raw materials are prepared according to the following mass parts: 43 parts of polycarbonate polyol resin, 37 parts of yellowing-resistant aliphatic diisocyanate, 3 parts of amine organic acid salt catalyst, and 20 parts of magnesium hydroxide halogen-free environmentally friendly flame retardant;

[0108] (2) Mixing the raw materials prepared in step (1) to prepare a bonding layer solution, wherein the bonding layer solution is stirred at a speed of 2500 rpm for 48 hours;

[0109] (3) The adhesive solution was applied at a speed of 10 m / min and a usage of 200 g / m 2 ;

[0110] (4) Then, the adhesive layer is dried and formed. The drying and forming temperature of the adhesive layer is 90° C., the length of the oven is 30 m, the baking time is 3 min, and the drying degree of the adhesive layer is 80%.

[0111] S3, base fabric bonding: the surface layer obtained in step S1, the adhesive layer obtained in step S2 and the base fabric layer are bonded together to form a composite leather blank; the bonding speed is 10 m / min, and the bonding pressure is 0.3 MPa.

[0112] S4, aging treatment: the composite leather stock obtained in step S4 is aged in an oven and cooled to obtain an aged leather stock; the aging treatment temperature is 120° C., the oven length is 120 m, and the baking time is 12 min.

[0113] S5, peeling: peeling the aged leather stock obtained in step S3 from the release paper transfer mold to obtain a PU leather stock.

[0114] S6, surface treatment 1:

[0115] (1) According to the material components of the surface treatment solution for the surface layer treatment, raw materials are prepared according to the following mass parts: 73 parts of waterborne polyurethane, 7 parts of carbodiimide, 13 parts of fluorinated acrylate, and 7 parts of water;

[0116] (2) Mixing the raw materials prepared in step (1) to prepare a first surface treatment layer solution, the stirring speed of the first surface treatment layer solution is adjusted to 400 rpm, the stirring time is 30 min, and the viscosity of the first surface treatment layer solution is 400 cps;

[0117] (3) The first surface treatment layer solution is coated on the surface layer at a coating speed of 10.0 m / min and a usage of 13 g / m 2 The first surface treatment layer is baked at a molding temperature of 100°C, an oven length of 25 m, and a baking time of 2.5 min to obtain a semi-finished PU leather.

[0118] S7, surface treatment 2:

[0119] (1) According to the material components of the surface treatment layer solution for the surface layer treatment, raw materials are prepared according to the following mass parts: 73 parts of waterborne polyurethane, 3 parts of carbodiimide, 7 parts of polyacrylic thickener, 2 parts of silicon oxide polymer resin, 5 parts of fluorine-containing acrylate, and 13 parts of water;

[0120] (2) Mixing the raw materials prepared in step (1) to prepare a second surface treatment layer solution, the stirring speed of the second surface treatment layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the second surface treatment layer solution is 600 cps;

[0121] (3) The second surface treatment layer solution is coated on the semi-finished PU leather, i.e., the first surface treatment layer, at a coating speed of 10.0 m / min and a usage of 27 g / m 2 The baking molding temperature of the second surface treatment layer is 100°C, the oven length is 25m, and the baking time is 2.5min to obtain the finished PU leather.

[0122] The solvent-resistant and strong acid-base PU synthetic leather prepared according to the above method is Figure 2 The structure shown includes a base fabric layer 10, an adhesive layer 20, a surface layer 30, a first surface treatment layer 40 and a second surface treatment layer 50, wherein the first surface treatment layer 40 and the second surface treatment layer 50 have different components and different coating amounts, that is, different thicknesses. The specific preparation method is described above, and the performance is tested. The results are shown in Table 1.

[0123] Comparative Example 1

[0124] This comparative example provides a method for preparing solvent-resistant and strong acid-base resistant PU synthetic leather, which differs from Example 3 mainly in steps S6 and S7:

[0125] First, prepare the release paper transfer film and the base fabric layer, wherein the base fabric layer is a weft knitted fabric with a thickness of (0.9±0.05) cm and a mass surface density of (300±20) g / m 2 The production environment temperature is 0.0℃~35.0℃, and the production environment humidity is 25%~75%.

[0126] S1 surface layer production:

[0127] (1) According to the material components of the surface layer, raw materials are prepared according to the following mass parts: 65 parts of water-based aliphatic polyurethane, 15 parts of polytetrafluoroethylene, 2 parts of bridging agent, 8 parts of pigment, and 10 parts of water;

[0128] (2) Mixing the raw materials prepared in step (1) to prepare a surface layer solution, the stirring speed of the surface layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the obtained surface layer solution is 3500 cps;

[0129] (3) The surface layer solution is fully degassed using a circulating degassing machine for 50 minutes;

[0130] (4) The surface layer solution is coated at a speed of 10 m / min and a usage of 40 g / m 2 ;

[0131] (5) Then the product is dried and formed at a temperature of 100°C, an oven length of 30m, and a time of 3min.

[0132] S2. Making the next layer:

[0133] (1) According to the material components of the adhesive layer, the raw materials are prepared according to the following mass parts: 40 parts of polycarbonate polyol resin, 40 parts of yellowing-resistant aliphatic diisocyanate, 1 part of amine organic acid salt catalyst, and 18 parts of magnesium hydroxide halogen-free environmentally friendly flame retardant;

[0134] (2) Mixing the raw materials prepared in step (1) to prepare a bonding layer solution, wherein the bonding layer solution is stirred at a speed of 2500 rpm for 48 hours;

[0135] (3) The adhesive solution was applied at a speed of 10 m / min and a usage of 200 g / m 2 ;

[0136] (4) Then, the adhesive layer is dried and formed. The drying and forming temperature of the adhesive layer is 90° C., the length of the oven is 30 m, the baking time is 3 min, and the drying degree of the adhesive layer is 80%.

[0137] S3, base fabric bonding: the surface layer obtained in step S1, the adhesive layer obtained in step S2 and the base fabric layer are bonded together to form a composite leather blank; the bonding speed is 10 m / min, and the bonding pressure is 0.3 MPa.

[0138] S4 aging treatment: the composite leather blank obtained in step S4 is aged in an oven and then cooled to obtain an aged leather blank; the aging treatment temperature is 120° C., the oven length is 120 m, and the baking time is 12 min.

[0139] S5 peeling: peeling the aged leather blank obtained in step S4 from the release paper transfer mold to obtain a PU leather blank.

[0140] S6, surface treatment 1:

[0141] (1) According to the material components of the surface treatment solution for the surface layer treatment, raw materials are prepared according to the following mass parts: 73 parts of waterborne polyurethane, 7 parts of carbodiimide, 13 parts of fluorinated acrylate, and 7 parts of water;

[0142] (2) Mixing the raw materials prepared in step (1) to prepare a first surface treatment layer solution, the stirring speed of the first surface treatment layer solution is adjusted to 400 rpm, the stirring time is 30 min, and the viscosity of the first surface treatment layer solution is 400 cps;

[0143] (3) The first surface treatment layer solution is coated on the surface layer at a coating speed of 10.0 m / min and a usage of 10 g / m 2The baking molding temperature of the first surface treatment layer is 100° C., the oven length is 25 m, and the baking time is 2.5 min to obtain a semi-finished PU leather.

[0144] S7, surface treatment 2:

[0145] (1) According to the material components of the surface treatment solution for the surface layer treatment, raw materials are prepared according to the following mass parts: 73 parts of waterborne polyurethane, 7 parts of carbodiimide, 13 parts of fluorinated acrylate, and 7 parts of water;

[0146] (2) Mixing the raw materials prepared in step (1) to prepare a second surface treatment layer solution, the stirring speed of the second surface treatment layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the second surface treatment layer solution is 400 cps;

[0147] (3) The second surface treatment layer solution is coated on the surface of the semi-finished PU leather, i.e., the first surface treatment layer, at a coating speed of 10.0 m / min and a usage of 25 g / m 2 The second surface treatment layer is baked at a molding temperature of 100°C, an oven length of 25 m, and a baking time of 2.5 min to obtain a finished PU leather.

[0148] The solvent-resistant and strong acid-base PU synthetic leather prepared according to the above method includes a base fabric layer, an adhesive layer, a surface layer, a first surface treatment layer and a second surface treatment layer, wherein the components of the first surface treatment layer and the second surface treatment layer are the same and are the same as the components of the first surface treatment layer in Example 3, the difference is that the coating amount, that is, the thickness, of the first surface treatment layer and the second surface treatment layer in this comparative example is different, and performance testing is performed, and the results are shown in Table 1.

[0149] Comparative Example 2

[0150] This comparative example provides a method for preparing solvent-resistant and strong acid-base resistant PU synthetic leather, which differs from Example 3 mainly in steps S6 and S7:

[0151] First, prepare the release paper transfer film and the base fabric layer, wherein the base fabric layer is a weft knitted fabric with a thickness of (0.9±0.05) cm and a mass surface density of (300±20) g / m 2 The production environment temperature is 0.0℃~35.0℃, and the production environment humidity is 25%~75%.

[0152] S1. Surface layer production:

[0153] (1) According to the material components of the surface layer, raw materials are prepared according to the following mass parts: 65 parts of water-based aliphatic polyurethane, 15 parts of polytetrafluoroethylene, 2 parts of bridging agent, 8 parts of pigment, and 10 parts of water;

[0154] (2) Mixing the raw materials prepared in step (1) to prepare a surface layer solution, the stirring speed of the surface layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the obtained surface layer solution is 3500 cps;

[0155] (3) The surface layer solution is fully degassed using a circulating degassing machine for 50 minutes;

[0156] (4) The surface layer solution is coated at a speed of 10 m / min and a usage of 40 g / m 2 ;

[0157] (5) Then the product is dried and formed at a temperature of 100°C, an oven length of 30m, and a time of 3min.

[0158] S2. Making the next layer:

[0159] (1) According to the material components of the adhesive layer, the raw materials are prepared according to the following mass parts: 40 parts of polycarbonate polyol resin, 40 parts of yellowing-resistant aliphatic diisocyanate, 1 part of amine organic acid salt catalyst, and 18 parts of magnesium hydroxide halogen-free environmentally friendly flame retardant;

[0160] (2) Mixing the raw materials prepared in step (1) to prepare a bonding layer solution, wherein the bonding layer solution is stirred at a speed of 2500 rpm for 48 hours;

[0161] (3) The adhesive solution was applied at a speed of 10 m / min and a usage of 200 g / m 2 ;

[0162] (4) Then drying and forming is performed, the drying and forming temperature of the bonding layer is 90° C., the oven length is 30 m, the baking time is 3 min, and the drying degree of the bonding layer is 80%;

[0163] S3, base fabric lamination: the surface layer obtained in step S1, the adhesive layer obtained in step S2 and the base fabric layer are bonded together to form a composite leather blank; the bonding speed is 10 m / min, and the bonding pressure is 0.3 MPa;

[0164] S4, aging treatment: the composite leather stock obtained in step S4 is aged in an oven and cooled to obtain an aged leather stock; the aging treatment temperature is 120° C., the oven length is 120 m, and the baking time is 12 min;

[0165] S5, peeling: peeling the aged leather blank obtained in step S4 from the release paper transfer mold to obtain a PU leather blank.

[0166] S6, surface treatment 1:

[0167] (1) According to the material components of the surface treatment layer solution for the surface layer treatment, the raw materials are prepared according to the following mass parts: 73 parts of waterborne polyurethane, 3 parts of carbodiimide, 7 parts of polyacrylic thickener, 2 parts of silicon oxide polymer resin, 5 parts of fluorine-containing acrylate, and 13 parts of water;

[0168] (2) Mixing the raw materials prepared in step (1) to prepare a first surface treatment layer solution, the stirring speed of the first surface treatment layer solution is adjusted to 400 rpm, the stirring time is 30 min, and the viscosity of the first surface treatment layer solution is 600 cps;

[0169] (3) The first surface treatment layer solution is coated on the surface layer at a coating speed of 10.0 m / min and a usage of 10 g / m 2 The first surface treatment layer is baked at a molding temperature of 100°C, an oven length of 25 m, and a baking time of 2.5 min to obtain a semi-finished PU leather.

[0170] S7, surface treatment 2:

[0171] ((1) According to the material components of the surface treatment layer solution of the surface layer treatment, the raw materials are prepared according to the following mass parts: 73 parts of water-based polyurethane, 3 parts of carbodiimide, 7 parts of polyacrylic thickener, 2 parts of silicon oxide polymer resin, 5 parts of fluorine-containing acrylate, and 13 parts of water;

[0172] (2) Mixing the raw materials prepared in step (1) to prepare a second surface treatment layer solution, the stirring speed of the second surface treatment layer solution is 400 rpm, the stirring time is 30 min, and the viscosity of the second surface treatment layer solution is 600 cps;

[0173] (3) The second surface treatment layer solution is coated on the surface of the semi-finished PU leather, i.e., the first surface treatment layer, at a coating speed of 10.0 m / min and a usage of 25 g / m 2 The second surface treatment layer is baked at a molding temperature of 100°C, an oven length of 25 m, and a baking time of 2.5 min to obtain a finished PU leather.

[0174] The solvent-resistant and strong acid-base PU synthetic leather prepared according to the above method includes a base fabric layer, an adhesive layer, a surface layer, a first surface treatment layer and a second surface treatment layer, wherein the components of the first surface treatment layer and the second surface treatment layer are the same and are the same as the components of the second surface treatment layer in Example 3, the difference is that the coating amount, that is, the thickness, of the first surface treatment layer and the second surface treatment layer in this comparative example is different, and performance testing is performed, and the results are shown in Table 1.

[0175] It should be noted that the reagents and raw materials in the above embodiments and comparative examples can be purchased on the market, so no special description or limitation is made. In addition, the specific structure and working principle of the circulating deaerator are not described or limited, and are conventional circulating deaerators, which are easily known to those skilled in the art.

[0176] Comparative Example 3

[0177] This comparative example is a common polyurethane PU synthetic leather currently on the market. Figure 1 The example shown includes a base fabric layer 10', a bonding layer 20', a surface layer 30' and a surface treatment layer 40' which are stacked in sequence. The difference from the polyurethane PU synthetic leather of Example 3 of the present invention is that in addition to the different structure of the surface treatment layer (this comparative example has only one surface treatment layer), the materials used for the surface layer and the surface treatment layer of the PU synthetic leather in this comparative example are also different from those in Example 3. Specifically, the surface layer of the ordinary polyurethane PU synthetic leather is a polyurethane material that does not contain fluorine-containing additives, and the surface treatment layer is an aqueous polyurethane material to which fluorine-containing additives are not added. In addition, the coating amount of the surface layer of the ordinary polyurethane PU synthetic leather in this comparative example (45±5g / m 2 ) is greater than the coating amount (40±5 g / m 2 ), the coating amount of the surface treatment layer of the ordinary polyurethane PU synthetic leather is also greater than the coating amount of the first surface treatment layer and the second surface treatment layer of Example 3 of the present invention, which will not be described in detail.

[0178] Table 1 Performance test table of PU synthetic leather obtained from Examples 1 to 3 and Comparative Examples 1 and 2

[0179]

[0180]

[0181]

[0182] It should be noted that the above-mentioned testing indicators are all implemented with reference to existing national standards, industry standards or enterprise standards. No specific description or limitation is given, and those skilled in the art can easily understand them.

[0183] It can be seen from Table 1 that the PU synthetic leather prepared by the preparation method of Examples 1 to 3 of the present invention has improved resistance to strong polarity and acidity and alkalinity, and the performance of the PU synthetic leather obtained within the formula range is not much different. However, compared with Example 3 of the present invention, the performance of Comparative Examples 1 and 2 has declined. However, as described above, the first surface treatment layer and the second surface treatment layer have functional differences. Therefore, although the performance of the PU synthetic leather obtained by Comparative Examples 1 and 2 can also achieve the performance of the PU synthetic leather of Examples 1 to 3 of the present invention, there are still some differences. For example, the PU synthetic leather of Comparative Example 1 has a lower breaking strength than that of Examples 1 to 3 of the present invention. This is precisely because of the shaping effect of the second surface treatment layer. The components of the second surface treatment layer of Comparative Example 1 are the same as those of the first surface treatment layer. The only difference is the coating amount. Therefore, it is impossible to achieve better shaping, resulting in a decrease in strength. The components of the first surface treatment layer and the second surface treatment layer of Comparative Example 2 are the same as those of the second surface treatment layer of Example 3 of the present invention. Although most of the test results are stronger than those of Examples 1 and 2 of the present invention, some properties (tear strength) are also lower than those of Examples 1 to 3 of the present invention. In addition, considering the cost issue, the present invention preferably adopts a first surface treatment layer and a second surface treatment layer of different components. In addition to achieving strong heat resistance, weather resistance and acid and alkali resistance through the two surface treatment layers, it also has the characteristics of greater strength, higher adhesion and greater peeling force.

[0184] At the same time, the PU synthetic leather of Example 3 of the present application and the ordinary PU synthetic leather on the market, that is, the PU synthetic leather of Comparative Example 3, were tested for chemical resistance and washability (mainly focusing on sunscreen and hand cream, because there is little difference in other items), as shown in Table 2 below.

[0185] Table 2 Performance test table of PU synthetic leather of Example 3 and ordinary PU synthetic leather of Comparative Example 3

[0186]

[0187] It should be noted that Figure 3 The left side shows the test result of sunscreen resistance of ordinary PU synthetic leather, i.e., the PU synthetic leather of Comparative Example 3, and the right side shows the test result of hand cream resistance. Figure 4 The left side is the test result picture of the sunscreen resistance of the PU synthetic leather of Example 3, and the right side is the test result picture of the hand cream resistance. It can be seen from Table 1 that the performance of the PU synthetic leather in the embodiment of the present invention is improved. The results correspond to the test results in Table 2. It can be seen that the performance of the PU synthetic leather prepared by the preparation method of the embodiment of the present invention, especially the performance of acid, alkali and strong polar solvent resistance and hardness (ordinary PU synthetic leather has only one surface treatment layer, and bubbles are clearly seen in the figure) is improved.

[0188] It can be seen from Table 1 that the PU synthetic leather of the embodiment of the present invention is very suitable for the use requirements of passenger car interiors. Therefore, the embodiment of the present invention also provides the application of the PU synthetic leather of the embodiment above in passenger cars, more specifically in interiors.

[0189] The specified directions in this specific embodiment are only for the convenience of describing the positional relationship and the coordination relationship between the components. The above is only a preferred embodiment of the present invention. The protection scope of the present invention is not limited to the above embodiment. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a PU synthetic leather resistant to strong polar solvents and strong acids and alkalis, characterized in that: The following steps are involved: S1. Surface layer preparation: first prepare the surface layer solution, then perform degassing treatment, coating processing and surface layer drying and molding; S2, adhesive layer preparation: first prepare adhesive layer solution, then carry out coating process, adhesive layer drying and forming; S3, base fabric bonding: bonding the surface layer obtained in step S1, the adhesive layer obtained in step S2 and the base fabric layer together to form a composite leather blank; S4, aging treatment: aging the composite leather stock obtained in step S3 in an oven to form an aged leather stock; S5, peeling: peeling the aged leather stock obtained in step S4 from the release paper transfer mold to obtain a PU leather stock; S6, surface layer treatment 1: prepare the first surface treatment layer solution, the first surface treatment layer solution is an aqueous polyurethane solution containing fluorine additives and has a viscosity of 300cps to 500cps, and apply the first surface treatment layer solution on the surface of the PU leather blank obtained in S5, with an amount of 10g / m 2 ~15g / m 2 , and then baked to obtain semi-finished PU leather; S7, surface layer treatment 2: prepare the second surface treatment layer solution, which is an aqueous polyurethane solution containing fluorine additives and has a viscosity of 500cps to 700cps. Apply the second surface treatment layer solution on the surface of the semi-finished PU leather obtained in S6, with a usage amount of 25g / m 2 ~30g / m 2 , and then baked to obtain the finished PU leather.

2. The preparation method according to claim 1, characterized in that: The surface layer solution in step S1 comprises, by weight: 65 to 70 parts of water-based aliphatic polyurethane, 10 to 15 parts of polytetrafluoroethylene, 2 to 4 parts of a bridging agent, 5 to 8 parts of a pigment, and 10 to 13 parts of water; The stirring speed of the surface layer solution is 400 rpm, the stirring time is 30 minutes, and the viscosity of the surface layer solution is 3000±500 cps; the prepared surface layer solution is degassed by a circulating degassing machine, and the degassing time of the surface layer solution is 50 minutes. During the circulating degassing, air is prevented from entering to improve the uniformity of the surface layer coating; The surface layer solution coating process speed is 10m / min, and the usage is 40±5 g / m 2 ; The temperature for drying and molding the surface layer is 100°C, the length of the oven is 30m, and the baking time is 3min.

3. The preparation method according to claim 1, characterized in that: The bonding layer solution in step S2 comprises, by weight: 40 to 45 parts of polycarbonate polyol resin, 35 to 40 parts of yellowing-resistant aliphatic diisocyanate, 1 to 4 parts of amine organic acid salt catalyst, and 18 to 24 parts of magnesium hydroxide halogen-free environmentally friendly flame retardant; In step S2, the stirring speed of preparing the bonding layer solution is 2500 rpm and the stirring time is 48 hours; The coating speed of the adhesive layer solution is 10m / min and the amount used is 200±20 g / m 2 ; The temperature of the next layer drying and molding is 90℃~110℃, the oven length is 30m, and the baking time is 3min; the drying degree of the next layer is 80%~90%.

4. The preparation method according to claim 1, characterized in that: The first surface treatment layer solution in step S6 includes, by weight: 70 to 75 parts of waterborne polyurethane, 5 to 8 parts of carbodiimide, 10 to 15 parts of fluorine-containing acrylate, and 5 to 10 parts of water.

5. The preparation method according to claim 1, characterized in that: The second surface treatment layer solution in step S7 includes: 70 to 75 parts of aqueous polyurethane, 2 to 4 parts of carbodiimide, 1 to 3 parts of polyacrylic thickener, 3 to 7 parts of silicon oxide polymer resin, 10 to 15 parts of fluorine-containing acrylate, and 5 to 10 parts of water.

6. The preparation method according to claim 1, characterized in that: In step S3, the base fabric is a weft-knitted fabric, the thickness of the base fabric is 0.9±0.05 cm, and the mass surface density is 300±30 g / m 2 ; and / or The bonding speed is 10m / min and the bonding pressure is 0.3MPa; and / or In step S5, the temperature of the aging treatment is 130° C., the length of the oven is 120 m, and the baking time is 12 min; and / or The production environment temperature of step S1 to step S7 is 0°C to 35.0°C, and the production environment humidity is 25% to 75%.

7. The preparation method according to claim 1, characterized in that: In step S6, the stirring speed of the first surface treatment layer solution is 400 rpm and the stirring time is 30 min; The speed of the first surface treatment layer solution coating process is 10m / min; The baking molding temperature of the first surface treatment layer is 100.0°C to 130.0°C, the oven length is 25m, and the baking time is 2.5min.

8. The preparation method according to claim 1, characterized in that: In step S7, the stirring speed of the second surface treatment layer solution is 400 rpm and the stirring time is 30 min; The speed of the second surface treatment layer solution coating process is 10m / min; The baking molding temperature of the second surface treatment layer is 100.0°C to 130.0°C, the oven length is 25m, and the baking time is 2.5min.

9. A PU synthetic leather resistant to strong polar solvents and strong acids and alkalis, characterized in that: The invention comprises a base fabric layer, a bonding layer, a surface layer, a first surface treatment layer and a second surface treatment layer which are stacked in sequence. The PU synthetic leather is made by the preparation method according to any one of claims 1 to 8.

10. Use of the PU synthetic leather according to claim 9 or the PU synthetic leather prepared by the preparation method according to any one of claims 1 to 8 in passenger car interiors.

Citation Information

Patent Citations

  • Water-based PU matte surface finishing agent for synthetic leather

    CN101705621A

  • Aqueous polyurethane-polyacrylate of side-chain fluorinated alkyl and preparation method thereof

    CN101775110A

  • Waterborne polyurethane composite leather and preparation method thereof

    CN111809404A

  • Waterproof and oil-resistant leather and preparation method thereof

    CN113322693A

  • PU (Polyurethane) composite leather and preparation method thereof

    CN113605107A