New secondary emulsification primer single-layer gluing process for high-strength and high-transparency medical gluing cover material body paper
Through the secondary emulsified base glue single-layer glue coating process, combined with inorganic pigments and coupling agents, the strength and breathability of medical glue coating cover paper are improved, and the problem of reducing breathability caused by increasing strength in the existing technology is solved, and the problem of increasing strength in the existing technology is achieved. Efficient production of medical packaging materials.
Patent Information
- Application Number
- CN202411028764.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-30
AI Technical Summary
When the existing medical glue-coated cover paper improves strength performance, the breathable performance is significantly reduced, resulting in a decline in product quality. The traditional composite modification process is complex and time-consuming, and is not suitable for industrial production.
Using the secondary emulsified base glue single-layer glue coating process, the high-strength and high-permeability medical glue coating cover paper is prepared through the synergistic effect of inorganic pigments and coupling agents, combining the base paper with the coated composite modified base glue layer to improve the base glue The tensile strength, tear strength and breathable properties of the paper.
It achieves high tensile strength, tear strength and appropriate peel strength, while improving breathability, meeting the needs of clean peeling and ethylene oxide sterilization of medical packaging, and solving the problem of poor breathability in traditional processes.
Smart Images

Figure CN118932778A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a new process for secondary emulsified primer single-layer gluing of base paper for high-strength and high-transparency medical glue-coated cover materials, and in particular to a method for utilizing secondary emulsified primer single-layer gluing to adjust the pore size of primer paper to improve the air permeability and strength of the primer paper for medical glue-coated cover materials, and belongs to the field of applied chemistry. Background Art
[0002] The safety performance of sterile medical devices is increasingly valued, requiring their packaging materials to have long-lasting and excellent protective effects. Blister sterilization packaging materials include heat-sealed substrates and sealed cover materials. Sterile medical coated cover paper is required to have good dialysis performance, including air permeability and antibacterial properties, and can be applied to a variety of sterilization methods such as ethylene oxide, electron beam or Co60 irradiation. Compared with the traditional sterilization and repackaging method, the terminal sterilization mode of medical devices (i.e., medical devices are packaged first and then sterilized) strengthens the control of contamination risks during transportation, storage and use of medical devices, and significantly improves the safety of use. Therefore, high-strength and high-transparency sterile medical coated cover paper is the inevitable development trend and direction of high-end medical packaging materials. High strength is for clean peeling when the medical device packaging is unsealed to prevent contamination of the medical device; high air permeability is to prevent the packaging from bursting due to poor air permeability during ethylene oxide sterilization. At present, the main way to improve the strength of the adhesive paper for medical coated cover materials is to apply adhesive on the surface. However, the adhesive on the surface will significantly reduce the air permeability, resulting in reduced product quality, and can only be used in low-end fields. The traditional composite modification process is often complicated and time-consuming, which is not conducive to industrial production. Therefore, a new process is urgently needed to prepare high-strength and high-transparency adhesive paper for medical coated cover materials to meet the needs of medical packaging.
[0003] In order to solve the problems existing in the prior art, the present invention creatively proposes to effectively improve the strength, permeability and sealing properties of the base paper by adopting a simplified process of single-layer gluing and a composite modification method, thereby providing a better quality material for medical packaging. Summary of the invention
[0004] The technical purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a new process for composite modified single-layer gluing of high-strength and high-permeability medical gluing cover paper and base paper with high tensile strength, tear strength and peel strength and good air permeability. To achieve the above-mentioned technical purpose, the technical solution adopted by the present invention is as follows:
[0005] A new process for secondary emulsification (compound modification) of a single-layer primer coating of a high-strength and high-transparency medical glue-coated cover material base paper, comprising the following steps:
[0006] Step 1, high-strength and high-transparency medical adhesive cover material base paper composition: It is composed of base paper and a composite modified base adhesive layer coated on the surface. Step 2, preparation of inorganic pigment dispersion: Inorganic pigments are modified by coupling agents, first mixed and dispersed at low speed, and then homogenized at high speed to prepare inorganic pigment dispersion.
[0007] Step 3, secondary emulsified primer: the above dispersion and primer are mixed and emulsified in different proportions to obtain secondary emulsified primer.
[0008] Step 4: Apply secondary emulsified primer (dilution ratio 1:2-1:6) on the surface of the base paper to obtain primer paper, and then apply top glue according to a fixed process to obtain medical coated cover paper.
[0009] Step 5: The high-strength and high-transparency medical coated cover paper can be heat-sealed with the hard plastic sheet.
[0010] Preferably, the glue layer coated on the surface of the base paper in step 1 is evenly distributed on the surface of the base paper.
[0011] Preferably, in step 1, the drying temperature of the adhesive layer is 65-105°C.
[0012] Preferably, the inorganic pigment in step 2 includes one or a mixture of calcium carbonate, kaolin, satin white, and white carbon black.
[0013] Preferably, in step 2, one or more inorganic pigments are selected and mixed and dispersed uniformly, and the coupling agent accounts for 1%-15% of the inorganic pigment.
[0014] The preferred preparation conditions of the inorganic pigment dispersion in step 2 are: firstly disperse at low speed for 1-3 hours, stirring speed of 500-1200rpm; then homogenize at high speed for 0.5-1h, stirring speed of 8000-10000rpm. The solid content of the dispersion is 15%-30%, stable for 8 hours, and can be dispersed by secondary homogenization, meeting the requirements for compatibility with the base glue.
[0015] Preferably, in step 3, the primer is ethylene-vinyl acetate copolymer.
[0016] Preferably, in step 4, the dilution ratio of the base glue is (1:2-1:6), the coating amount is (1.5-4.5) ± 0.2 g / m2; and the coating amount of the top glue is 6.0 ± 0.5 g / m2.
[0017] Preferably, the hard plastic sheet in step 5 includes PET, PVC, PS, PETG, etc.
[0018] The beneficial effects of the present invention are:
[0019] 1) The present invention mainly performs secondary emulsification of the base glue by inorganic pigments, coupling agents, etc. to obtain a secondary emulsified base glue, which is diluted and coated to prepare base glue paper, and then coated with surface glue to prepare medical coated cover paper.
[0020] 2) The medical coated cover paper has high tensile strength, tear strength and appropriate peel strength, as well as good air permeability, which enables clean peeling of medical device packaging, prevents contamination of medical devices, and solves the problem of bag bulging during ethylene oxide sterilization.
[0021] 3) The benefits of the synergistic effect of multiple inorganic pigments are that the color, hiding power, glossiness and air permeability of the coating can be adjusted. Silane coupling agent is a type of organic silicon compound that improves the adhesion and durability between inorganic pigments and primers, reacts with the surface of the substrate to form a chemical bond, thereby enhancing the adhesion between the pigment and the substrate. This in turn improves the high strength and high permeability of medical coated cover paper, making its various performance indicators meet the use standards. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 To ensure the stability of the secondary emulsified (compounded and modified) primer;
[0023] Figure 2 It is a high-strength and high-permeability base paper and medical-grade coated cover paper with absorbency;
[0024] Figure 3 It is a high-strength and high-permeability medical coated cover paper with peeling performance;
[0025] Figure 4 It is a heat-sealing paper with high strength and high air permeability for base paper and medical coated cover paper.
[0026] Instruments and test methods
[0027] The test method involved in the present invention is as follows:
[0028] The air permeability, strength (longitudinal / transverse tensile strength, longitudinal / transverse tear strength) and peeling force of base paper, base paper and medical coated cover paper were analyzed respectively.
[0029] The air permeability was measured by an air permeability tester. The longitudinal / transverse tensile strength was measured by a tensile strength tester. The longitudinal / transverse tear strength was measured by a paper tearing tester. The peel strength was measured by an electronic tensile tester. The surface morphology of the coating layer was observed by a scanning electron microscope. DETAILED DESCRIPTION
[0030] A new process for secondary emulsified primer single-layer gluing of high-strength and high-transparency medical glue-coated cover material base paper, comprising the following steps:
[0031] Step 1, high-strength and high-transparency medical adhesive cover material base paper composition: It is composed of base paper and a secondary emulsified base adhesive layer coated on the surface. Step 2, preparation of inorganic pigment dispersion: Inorganic pigments are modified with silane coupling agents, first mixed and dispersed at a low speed, and then homogenized at a high speed to prepare inorganic pigment dispersion.
[0032] Step 3, secondary emulsified primer: the above dispersion liquid and primer are mixed and emulsified in different proportions to obtain secondary emulsified primer liquid.
[0033] Step 4: The surface of the base paper is coated with a secondary emulsified primer to obtain a primer paper, and then the surface glue is coated according to a fixed process to obtain a medical coated cover paper.
[0034] Step 5: The high-strength and high-transparency medical coated cover material coated paper can be heat-sealed with the hard plastic sheet.
[0035] Preferably, the glue layer coated on the surface of the base paper in step 1 is evenly distributed on the surface of the base paper.
[0036] Preferably, in step 1, the drying temperature of the adhesive layer is 65-105°C.
[0037] Preferably, the inorganic pigment in step 2 includes one or a mixture of calcium carbonate, kaolin, satin white, and white carbon black.
[0038] Preferably, in step 2, one or more inorganic pigments are selected and mixed and dispersed uniformly, and the silane coupling agent accounts for 1%-15% of the inorganic pigment.
[0039] The preferred preparation conditions of the inorganic pigment dispersion in step 2 are: firstly disperse at low speed for 1-3 hours, stirring speed of 500-1200rpm, then homogenize at high speed for 0.5-1 hour, stirring speed of 8000-10000rpm. The solid content of the dispersion is 15%-30%, and it is stable for 8 hours, which meets the requirements.
[0040] Preferably, in step 3, the primer is ethylene-vinyl acetate copolymer.
[0041] Preferably, in step 4, the dilution ratio of the base glue is (1:2-1:6), the coating amount is (1.5-4.5) ± 0.2 g / m2; and the coating amount of the top glue is 6.0 ± 0.5 g / m2.
[0042] Preferably, the hard plastic sheet in step 5 includes PET, PVC, PS, PETG, etc.
[0043] The present invention is further described in detail below with reference to specific embodiments.
[0044] Example 1
[0045] 1) Inorganic pigment micron-sized calcium carbonate was mixed with 5% silane coupling agent, first dispersed at 900 rpm for 2 h, and then homogenized at 9000 rpm for 0.5 h to prepare an inorganic pigment dispersion with a solid content of 25%.
[0046] 2) The above 5% inorganic pigment dispersion is mixed with ethylene-vinyl acetate copolymer for secondary emulsification to obtain a secondary emulsified ethylene-vinyl acetate copolymer primer.
[0047] 3) The above-mentioned ethylene-vinyl acetate copolymer primer is diluted at a ratio of 1:4 and coated by an air knife at a speed of 26 m / min, a surface coating amount of 3.5±0.2 g / m2, and a drying temperature of 65°C to produce a primer paper, and then coated with 6±0.5 g / m2 of top glue to obtain a medical coated cover paper.
[0048] The air permeability of the base paper obtained in this example is 120 ml / min, the longitudinal / transverse tensile strength is 105.93N / 67.27N, and the longitudinal / transverse tear strength is 854.48mN / 886.52mN. The air permeability of the finally obtained medical coated cover paper is 80 ml / min, the longitudinal / transverse tensile strength is 116.73N / 76.90N, the longitudinal / transverse tear strength is 862.99mN / 951.90mN, and the peeling force is 2.5N.
[0049] Example 2
[0050] 1) Inorganic pigments were mixed with micron-sized calcium carbonate and nano-sized kaolin (at a ratio of 3:1 for synergistic effect) and 10% silane coupling agent, first dispersed at 900 rpm for 2 h, and then homogenized at 9000 rpm for 0.5 h to prepare an inorganic pigment dispersion with a solid content of 25%.
[0051] 2) The above 6% inorganic pigment dispersion and ethylene-vinyl acetate copolymer are secondary emulsified to prepare a secondary emulsified ethylene-vinyl acetate copolymer primer.
[0052] 3) The above-mentioned ethylene-vinyl acetate copolymer primer is diluted at a ratio of 1:2, and coated by air knife at a speed of 30 m / min, a surface coating amount of 4.5±0.2 g / m2, and a drying temperature of 75°C to produce a primer paper, and then coated with 6±0.5 g / m2 of top glue to obtain a medical coated cover paper.
[0053] The air permeability of the base paper obtained in this example is 105 ml / min, the longitudinal / transverse tensile strength is 102.91 N / 62.71 N, and the longitudinal / transverse tear strength is 801.72 mN / 862.54 mN. The air permeability of the finally obtained medical coated cover paper is 65 ml / min, the longitudinal / transverse tensile strength is 112.53 N / 73.45 N, the longitudinal / transverse tear strength is 813.61 mN / 902.30 mN, and the peeling force is 2.0 N.
[0054] Example 3
[0055] 1) Inorganic pigments were mixed with micronized calcium carbonate and satin white (synergistically reacted at a ratio of 3:1) and 13% silane coupling agent, first dispersed at 1000 rpm for 2 h, then homogenized at 8000 rpm for 1 h, and evenly dispersed to form an inorganic pigment dispersion with a solid content of 15%.
[0056] 2) The above 5% inorganic pigment dispersion and ethylene-vinyl acetate copolymer are secondary emulsified to prepare a secondary emulsified ethylene-vinyl acetate copolymer primer.
[0057] 3) The above-mentioned secondary emulsified ethylene-vinyl acetate copolymer primer is coated by air knife at a speed of 35m / min, a surface coating amount of 2.5±0.2g / m2, and a drying temperature of 85°C to produce a primer paper, and then coated with 6±0.5g / m2 of top glue to obtain a medical coated cover paper.
[0058] The air permeability of the base paper obtained in this example is 130 ml / min, the longitudinal / transverse tensile strength is 129.2N / 71.63N, and the longitudinal / transverse tear strength is 882.91mN / 972.82mN. The air permeability of the finally obtained medical coated cover paper is 85 ml / min, the longitudinal / transverse tensile strength is 125.60N / 87.80N, the longitudinal / transverse tear strength is 893.25mN / 1019.89mN, and the peeling force is 4.2N.
[0059] Example 4
[0060] 1) Inorganic pigment micron-grade calcium carbonate and white carbon black (synergistic effect according to 5:1) were mixed with 8% silane coupling agent, first dispersed at 1000rpm for 2h, then homogenized at 8000rpm for 1h, and dispersed evenly to form inorganic pigment dispersion with a solid content of 20%. 2) The above 5% inorganic pigment dispersion was secondary emulsified with ethylene-vinyl acetate copolymer to obtain secondary emulsified ethylene-vinyl acetate copolymer primer.
[0061] 3) The secondary emulsified ethylene-vinyl acetate copolymer primer is diluted at 1:6 and coated by air knife at a speed of 45 m / min, a surface coating amount of 1.5±0.2 g / m2, and a drying temperature of 85°C to produce a primer paper, and then coated with 6±0.5 g / m2 of top glue to obtain a medical coated cover paper.
[0062] The air permeability of the base paper obtained in this example is 140 ml / min, the longitudinal / transverse tensile strength is 117.80 N / 63.57 N, and the longitudinal / transverse tear strength is 784.53 mN / 805.42 mN. The air permeability of the finally obtained medical coated cover paper is 93 ml / min, the longitudinal / transverse tensile strength is 105.73 N / 67.80 N, the longitudinal / transverse tear strength is 826.65 mN / 989.41 mN, and the peeling force is 6.5 N.
[0063] Example 5
[0064] 1) Inorganic pigments: Nano-scale calcium carbonate, satin white and white carbon black (synergistically reacted at a ratio of 3:1:1) and 15% silane coupling agent were first dispersed at 1200 rpm for 3 h, then homogenized at 10000 rpm for 1 h, and evenly dispersed to form an inorganic pigment dispersion with a solid content of 18%.
[0065] 2) The above 5% inorganic pigment dispersion ethylene-vinyl acetate copolymer is secondary emulsified to obtain a secondary emulsified ethylene-vinyl acetate copolymer primer, and a secondary emulsified ethylene-vinyl acetate copolymer primer is obtained.
[0066] 3) The secondary emulsified ethylene-vinyl acetate copolymer primer is diluted at a ratio of 1:4 and coated by an air knife at a speed of 45 m / min, a surface coating amount of 2.5±0.2 g / m2, and a drying temperature of 95°C to produce a primer paper, and then coated with 6±0.5 g / m2 of top glue to obtain a medical coated cover paper.
[0067] The air permeability of the base paper obtained in this example is 145 ml / min, the longitudinal / transverse tensile strength is 127.60 N / 74.41 N, and the longitudinal / transverse tear strength is 869.22 mN / 976.81 mN. The air permeability of the finally obtained medical coated cover paper is 87 ml / min, the longitudinal / transverse tensile strength is 121.90 N / 67.74 N, the longitudinal / transverse tear strength is 902.75 mN / 981.97 mN, and the peeling force is 3.9 N.
[0068] Example 6
[0069] 1) Inorganic pigments: Nano-grade kaolin and satin white (synergistic effect according to 3:1) and 12% silane coupling agent, first dispersed at 900 rpm for 2.5 h, then homogenized at 9000 rpm for 0.5 h, and evenly dispersed to prepare an inorganic pigment dispersion with a solid content of 20%.
[0070] 2) The above 3% inorganic pigment dispersion ethylene-vinyl acetate copolymer is secondary emulsified to obtain a secondary emulsified ethylene-vinyl acetate copolymer primer, and a secondary emulsified ethylene-vinyl acetate copolymer primer is obtained.
[0071] 3) The secondary emulsified ethylene-vinyl acetate copolymer primer is diluted at 1:4 and coated by air knife at a speed of 40 m / min, a surface coating amount of 2.5±0.2 g / m2, and a drying temperature of 95°C to produce a primer paper, and then coated with 6±0.5 g / m2 of top glue to obtain a medical coated cover paper.
[0072] The air permeability of the base paper obtained in this example is 140 ml / min, the longitudinal / transverse tensile strength is 118.80 N / 75.27 N, and the longitudinal / transverse tear strength is 815.91 mN / 941.44 mN. The air permeability of the finally obtained medical coated cover paper is 86 ml / min, the longitudinal / transverse tensile strength is 117.50 N / 65.70 N, the longitudinal / transverse tear strength is 899.59 mN / 910.06 mN, and the peeling force is 3.8 N.
[0073] Example 7
[0074] 1) Inorganic pigments were synergistically mixed with nano-kaolin and white carbon black (at a ratio of 3:1) and 8% silane coupling agent, first dispersed at 1000 rpm for 2 h, then homogenized at 9000 rpm for 0.7 h, and evenly dispersed to form an inorganic pigment dispersion with a solid content of 20%.
[0075] 2) The above 5% inorganic pigment dispersion ethylene-vinyl acetate copolymer is secondarily emulsified to prepare a second emulsified ethylene-vinyl acetate copolymer primer.
[0076] 3) The secondary emulsified ethylene-vinyl acetate copolymer primer is diluted at a ratio of 1:5.5 and coated by an air knife at a speed of 50 m / min, a surface coating amount of 2.0±0.2 g / m2, and a drying temperature of 105°C to produce a primer paper, and then coated with 6±0.5 g / m2 of top glue to obtain a medical coated cover paper.
[0077] The air permeability of the base paper obtained in this example is 155 ml / min, the longitudinal / transverse tensile strength is 130.57 N / 75.27 N, and the longitudinal / transverse tear strength is 873.45 mN / 1040.43 mN. The air permeability of the finally obtained medical coated cover paper is 95 ml / min, the longitudinal / transverse tensile strength is 123.73 N / 70.60 N, the longitudinal / transverse tear strength is 910.06 mN / 1014.66 mN, and the peeling force is 4.5 N.
[0078] Example 8
[0079] 1) Inorganic pigments were synergistically mixed with nano-kaolin, satin white, and white carbon black (at a ratio of 3:1:1) and 15% silane coupling agent. They were first dispersed at 1200 rpm for 2 h, then homogenized at 10000 rpm for 1 h, and the inorganic pigment dispersion was evenly dispersed to form an inorganic pigment dispersion with a solid content of 18%.
[0080] 2) The above 5% inorganic pigment dispersion and ethylene-vinyl acetate copolymer are secondary emulsified to prepare a secondary emulsified ethylene-vinyl acetate copolymer primer.
[0081] 3) The secondary emulsified ethylene-vinyl acetate copolymer primer is diluted at a ratio of 1:3 and coated by an air knife at a speed of 32 m / min, a surface coating amount of 3.5±0.2 g / m2, and a drying temperature of 105°C to produce a primer paper, and then coated with 6±0.5 g / m2 of top glue to obtain a medical coated cover paper.
[0082] The air permeability of the base paper obtained in this example is 160 ml / min, the longitudinal / transverse tensile strength is 130.57 N / 75.27 N, and the longitudinal / transverse tear strength is 865.31 mN / 971.84 mN. The air permeability of the finally obtained medical coated cover paper is 87 ml / min, the longitudinal / transverse tensile strength is 127.2 N / 71.4 N, the longitudinal / transverse tear strength is 893.45 mN / 962.50 mN, and the peeling force is 3.0 N.
Claims
1. A new process for secondary emulsification (compound modification) of base paper for high-strength and high-transparency medical glue-coated cover material with single-layer glue coating, the specific method of which is as follows: (1) Preparation of inorganic pigment dispersion: Inorganic pigment is modified by silane coupling agent to prepare inorganic pigment dispersion. (2) Secondary emulsified primer: Mix the inorganic pigment dispersion with the primer, and perform secondary emulsified primer application. The primer dilution ratio is 1:2-1:
6. (3) Surface gluing: The secondary emulsified primer solution in step 2 is applied to the surface of the base paper of the medical packaging cover material; (4) Drying: After the surface is coated with primer and top glue, it is dried to finally obtain a high-strength and high-permeability medical coated cover paper.
2. A new process for secondary emulsified primer single-layer gluing of high-strength and high-transparency medical glue-coated cover material base paper according to claim 1, characterized in that: The inorganic pigment includes one or a mixture of calcium carbonate, kaolin, titanium dioxide, and white carbon black.
3. A new process for secondary emulsified primer single-layer gluing of high-strength and high-transparency medical glue-coated cover material base paper according to claim 1, characterized in that: The base glue is ethylene-vinyl acetate copolymer.
4. A new process for secondary emulsified primer single-layer gluing of high-strength and high-transparency medical glue-coated cover material base paper according to claim 1, characterized in that: The surface gluing method includes roller gluing and air knife gluing.
5. A new process for secondary emulsification (compounding and modification) of a single-layer primer coating of a high-strength and high-transparency medical glue-coated cover material base paper according to claim 1, characterized in that: The coating amount of the base glue is 1.5-4.5g / m2, and the number of coating layers is 1.
6. A new process for single-layer gluing of high-strength and high-transparency medical gluing cover paper according to claim 1, characterized in that: The drying method is drying in a drying tunnel.
Citation Information
Patent Citations
Heat-seal self-adhesive high-strength medical dialyzing paper and processing method thereof
CN113089380A
Antistatic breathable film and preparation method thereof
CN115895093A
High-permeability adhesive tape as well as preparation method and application thereof
CN118185490A
Glued dialyzing paper for sterilizing and packaging medical instruments
CN213949323U