Flame-retardant composite paper core with high outer-layer flexibility and high inner-layer hardness and preparation method of flame-retardant composite paper core
By using hierarchical structure and modified materials in the paper core, the flexibility and hardness of the paper core are improved, and the problems of existing paper cores are easily broken and insufficient glue performance when winding, achieving high flame retardancy and water resistance reduces production costs.
Patent Information
- Application Number
- CN202411256384.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-12
AI Technical Summary
Existing paper cores are prone to rupture when wrapping fragile rolls such as photo paper or aluminum foil, and the adhesive strength, flame retardancy and water resistance of the glue are insufficient, which affects product performance.
The flame-retardant composite paper core with high outer flexibility and high inner hardness is adopted. The hierarchical structure design of hard flame-retardant kraft paper layer, flame-retardant glue layer, foam paper layer and soft flame-retardant kraft paper layer is used, and modified potato starch is used. Phenolic resin, graphene oxide modified 2-carboxyethylphenylphosphoric acid and other materials are prepared to prepare flame retardant glue with excellent adhesive strength, flame retardant properties and water resistance.
It realizes the high radial pressure, green and environmentally friendly and safe, high flame retardant and low moisture content of the paper core, improves the impact resistance and service life of the product, and reduces production costs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of paper tube processing, and in particular to a flame-retardant composite paper core having high flexibility in the outer layer and high hardness in the inner layer, and a preparation method thereof. Background Art
[0002] Paper tube refers to a tubular object made of paper, which is widely used in the carrying packaging of various films.
[0003] In the printing and packaging industries, paper cores are often used as support for the storage and transportation of rolls of materials such as photo paper or aluminum foil. Existing paper cores are mostly composed of a single layer of kraft paper, which has very high strength and hardness. However, when winding fragile rolls such as photo paper or aluminum foil, a paper core with too high a hardness may cause the roll to break.
[0004] Glue is used when preparing multi-layer paper cores. Current glue has problems such as poor bonding strength, poor flame retardancy, and poor water resistance, which directly affect the performance of the final product paper core. Summary of the invention
[0005] The purpose of this application is to provide a flame-retardant composite paper core with high outer flexibility and high inner hardness and a preparation method thereof in view of the shortcomings of the current technology. The preparation method of the flame-retardant composite paper core with high outer flexibility and high inner hardness of the application has the advantages of simple preparation and low cost, and the flame-retardant composite paper core with high outer flexibility and high inner hardness obtained at the same time has high radial pressure, green environmental protection and safety, high flame retardancy and low moisture content (6-7%). The flame-retardant glue prepared by the application has excellent water resistance, flame retardancy and bonding strength, and is also highly safe and green and environmentally friendly.
[0006] In a first aspect, the present application provides a flame-retardant composite paper core with high outer layer flexibility and high inner layer hardness, using the following technical solution: A flame-retardant composite paper core with high flexibility in the outer layer and high hardness in the inner layer, which comprises, from the inside to the outside, a hard flame-retardant kraft paper layer, a flame-retardant glue layer, a foam paper layer and a soft flame-retardant kraft paper layer, wherein the flame-retardant glue layer is prepared by coating the flame-retardant glue on the surface of the hard flame-retardant kraft paper layer and bonding the foam paper layer, wherein the flame-retardant glue comprises, by weight, the following raw materials: 50-60 parts of modified potato starch, 3-5 parts of phenolic resin, 5-7 parts of flame retardant, 5-6 parts of waterproofing agent, 6-7 parts of urethane acrylate, 0.5-0.6 parts of preservative and 280-300 parts of water.
[0007] By adopting the above technical scheme, the hard flame retardant kraft paper layer: as the inner layer of the paper core, it provides hardness and support to ensure the structural stability and certain flame retardancy of the paper core. The flame retardant glue layer: the flame retardant glue is coated on the surface of the hard flame retardant kraft paper layer to bond the foam paper layer. The flame retardant glue has excellent water resistance, flame retardancy and bonding strength, which can effectively prevent bacteria from breeding and flame spread, and at the same time firmly bond the foam paper layer to the hard flame retardant kraft paper layer. The foam paper layer: located outside the flame retardant glue layer, provides buffering and protection, and increases the flexibility and impact resistance of the paper core. The soft flame retardant kraft paper layer: as the outer layer of the paper core, it has high flexibility, can adapt to a certain degree of deformation, protect the internal structure from damage and certain flame retardancy. Modified potato starch: as the main component of the adhesive, it is modified by wheat bran enzymatic hydrolysate to improve the gel strength and water holding capacity of the mixed slurry, which is conducive to improving the bonding strength and water resistance of the flame retardant glue. Phenolic resin: It works together with modified potato starch to provide good bonding properties and thermal stability, which helps to improve the overall performance of the composite paper core. Flame retardant (graphene oxide modified-2-carboxyethylphenyl hypophosphite): As the main flame retardant component, after being modified by γ-aminopropyltrimethoxysilane, it forms a three-dimensional network structure with graphene oxide, improving the compatibility and dispersibility in the flame retardant glue, thereby enhancing the flame retardant effect of the composite paper core. Waterproofing agent: It increases the waterproof performance of paper products, making them less susceptible to damage even when soaked in water, and greatly improves the bonding strength. Amino ester acrylate: It provides additional bonding and flexibility, which helps to improve the flexibility of the outer layer of the composite paper core. Preservatives (sodium benzoate and potassium sorbate): Sodium benzoate effectively inhibits the growth of bacteria and fungi in an acidic environment, while potassium sorbate, as a natural organic acid salt, is safer and prolongs the antibacterial performance of the flame retardant glue by inhibiting the growth of mold and bacteria. The two work synergistically to jointly improve the antibacterial performance of the flame retardant composite paper core. Water: As a solvent, it adjusts the viscosity and fluidity of the adhesive and ensures that the components are evenly mixed. In summary, the components in this application work together through a specific ratio and preparation process to form a flame-retardant composite paper core with high flexibility in the outer layer and high hardness in the inner layer. The composite paper core has the characteristics of high radial pressure, green environmental protection and safety, high flame retardancy and low moisture content, and the preparation method is simple and low cost.
[0008] Preferably, the inner diameter of the flame retardant composite paper core is 74-76 mm, the thickness is 9-9.5 mm, the thickness of the hard flame retardant kraft paper layer is 1.5-2 mm, the thickness of the soft flame retardant kraft paper layer is 1.5-2 mm, and the thickness of the foam paper layer is 5-6.5 mm.
[0009] Preferably, the method for preparing the modified potato starch comprises the following steps: S31, according to the mass fraction, grind 200 parts of wheat bran through an 80-mesh sieve, mix with 700g of water and stir for 30min to obtain a suspension, add 40 parts of α-amylase, and the enzymolysis time is 10h; after the enzymolysis is completed, heat to 115°C and inactivate the enzyme for 12min; then add 250 parts of a 20g / L sodium hydroxide aqueous solution, stir for 6h, adjust the pH value of the system to 4 with 35% hydrochloric acid, then centrifuge at 10000rpm for 50min, collect the supernatant, add 250 parts of a 75% ethanol aqueous solution to precipitate the supernatant, stir for 30min, filter, collect the precipitate, and freeze-dry at 30°C for 20h to obtain a wheat bran hydrolysate; S32. According to the mass fractions, 100 parts of potato starch are added to 70 parts of an aqueous solution of wheat bran hydrolysate having a mass concentration of 15%, stirred at 65°C for 60 minutes, then heated to 95°C, stirred for 30 minutes, cooled to 35°C, stirred for 30 minutes, and then centrifuged at 10,000 rpm for 50 minutes. The precipitate is then collected and freeze-dried at 30°C for 26 hours to obtain modified potato starch.
[0010] By adopting the above technical scheme, the role and synergistic effect of the prepared modified potato starch in the flame-retardant composite paper core are mainly reflected in the following aspects: 1. Improving bonding strength: The modified potato starch can improve the gel strength of the mixed slurry and the water holding capacity of the potato starch gel through the hydrogen bond interaction between the wheat bran enzymatic hydrolysate and the potato starch. This is conducive to improving the bonding strength and water resistance of the flame-retardant glue, so that the composite paper core has higher radial pressure and compressive strength. 2. Improving flame retardant properties: As one of the main components of the flame-retardant glue, the modified potato starch works together with other raw materials (such as phenolic resin, flame retardant, etc.) to form a glue layer with excellent flame retardancy. This glue layer can effectively prevent the spread of flames and improve the flame retardant properties of the composite paper core. 3. Green, environmentally friendly and safe: Modified potato starch is a natural and degradable polymer material with good biocompatibility and environmental friendliness. Using modified potato starch as the main component of the adhesive can reduce environmental pollution and improve the safety and environmental performance of the product. 4. Reduce costs: Modified potato starch has lower costs than other synthetic polymer adhesives, and the preparation method is simple. Therefore, using modified potato starch as the main adhesive component of the flame-retardant composite paper core can reduce production costs and improve product competitiveness. In summary, the modified potato starch of the present application plays a key role in the flame-retardant composite paper core, and achieves the preparation of a flame-retardant composite paper core with high flexibility in the outer layer and high hardness in the inner layer by improving bonding strength, enhancing flame retardant properties, ensuring green environmental protection and safety, and reducing costs.
[0011] Preferably, the flame retardant is graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid.
[0012] Preferably, the method for preparing the graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid comprises the following steps: S51, dispersing 100 parts of 2-carboxyethylphenylphosphorous acid and 10 parts of graphene oxide in a solution consisting of 12 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 30 parts of water according to mass fractions to obtain a mixed solution; S52, heating the mixed solution to 46°C, stirring at a rate of 800 rpm, reacting for 500 min, filtering, and vacuum drying at 75°C for 24 h, grinding and sieving to obtain graphene oxide-modified 2-carboxyethylphenylphosphorous acid with a particle size of 3-5 μm.
[0013] By adopting the above technical scheme, the prepared graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid plays a key role as a flame retardant in flame retardant glue. 1. Improve the flame retardant effect: Graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid as a gas source promotes the flame retardant to form a foam layer, releases a large amount of non-flammable gas, dilutes the oxygen in the environment, and thus improves the flame retardant effect. 2. Enhance compatibility and dispersibility: Modification by γ-aminopropyltrimethoxysilane helps the combination between graphene oxide and 2-carboxyethylphenyl hypophosphorous acid, enhances the interaction between them, and improves the compatibility and dispersibility in flame retardant glue. 3. Form a three-dimensional network structure: Graphene oxide forms a three-dimensional network structure, which further enhances the flame retardant effect of the composite paper core. 4. Synergistic effect: Graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid works together with other ingredients (such as phenolic resin, urethane acrylate, etc.) to improve the water resistance, flame retardancy and bonding strength of the flame retardant glue, while being highly safe and green.
[0014] Preferably, the waterproofing agent comprises the following raw materials, measured by weight: 40 parts of tannic acid, 35 parts of maltodextrin, 30 parts of sodium sulphate, and 38 parts of water.
[0015] Preferably, the preparation method of the waterproofing agent is to mix maltodextrin, sodium sulfate and water in proportions by mass, heat to 30°C, react for 60 minutes, then add tannic acid, heat to 50°C, and react for 4 hours to obtain the waterproofing agent.
[0016] By adopting the above technical solution, the prepared waterproof agent can increase the waterproof performance of paper products, which is not easily damaged even if soaked in water, and greatly improves the bonding strength. The waterproof agent works synergistically with other components in the flame retardant glue to jointly improve the water resistance and flame retardancy of the composite paper core.
[0017] Preferably, the preservative is composed of sodium benzoate and potassium sorbate in a mass ratio of 1:2.
[0018] In a second aspect, the present application provides a method for preparing a flame-retardant composite paper core with high outer layer flexibility and high inner layer hardness, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the flame-retardant composite paper core having high outer layer flexibility and high inner layer hardness, comprising the following steps: S91. Evenly stir the modified potato starch, phenolic resin, flame retardant, waterproofing agent, urethane acrylate, preservative and water according to their weight proportions to obtain a flame retardant glue; S92, selecting hard flame retardant kraft paper of specified thickness as raw material, and rolling to form a hard flame retardant kraft paper layer paper core; S93. Evenly apply flame retardant glue on the outer surface of the hard flame retardant kraft paper core, and then adhere one side of the foam paper to the outer surface of the hard flame retardant kraft paper core to make them tightly combined through the bonding process, and then roll the soft flame retardant kraft paper layer on the outer layer of the foam paper again, and dry it at a temperature of 90°C for 30-35 minutes to obtain a flame retardant composite paper core with a moisture content of 6%-7% and high flexibility of the outer layer and high hardness of the inner layer.
[0019] In summary, the beneficial technical effects of this application are: 1. High flame retardant performance: The flame retardant effect of the composite paper core is improved by using graphene oxide modified 2-carboxyethylphenylphosphite as a flame retardant and combining it with γ-aminopropyltrimethoxysilane as a coupling agent. This flame retardant can promote the formation of a foam layer, release a large amount of non-flammable gas, dilute oxygen, and thus improve flame retardant performance.
[0020] 2. Excellent bonding strength and water resistance: Modified potato starch is used as the main adhesive ingredient, and wheat bran enzymatic hydrolysate is used to improve its gel strength and water holding capacity, so that the flame retardant glue has better bonding strength and water resistance.
[0021] 3. Enhanced waterproof performance: The addition of waterproofing agent improves the waterproof ability of paper products, making them less susceptible to damage even when soaked in water, while also enhancing the bonding strength.
[0022] 4. Green, environmentally friendly and safe: The selected preservative combination (sodium benzoate and potassium sorbate) is highly safe and environmentally friendly, which helps to improve the environmental attributes of the product.
[0023] 5. Structural optimization: The composite paper core includes a hard flame-retardant kraft paper layer, a flame-retardant glue layer, a foam paper layer and a soft flame-retardant kraft paper layer from the inside to the outside. This hierarchical structure design enables the product to maintain hardness while having good flexibility on the outer layer.
[0024] 6. Low moisture content: The preparation method ensures that the composite paper core has a low moisture content (6-7%), which helps prevent degradation and reduced flame retardant properties caused by moisture.
[0025] 7. Antibacterial performance: Through the combined action of sodium benzoate and potassium sorbate, the antibacterial performance of the composite paper core is improved, extending the service life of the product.
[0026] 8. Cost-effectiveness: The preparation method is simple and the cost of raw materials is relatively low, making the composite paper core more competitive in the market. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following is a brief introduction to the drawings used in the embodiments: Figure 1 This is a physical picture of the flame retardant composite paper core prepared in Example 3 of the present application. DETAILED DESCRIPTION
[0028] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0029] In the following examples and preparation examples, 1 part means 100 g.
[0030] Preparation Example 1 Preparation of modified potato starch The preparation method of modified potato starch comprises the following steps: S31, according to the mass fraction, grind 200 parts of wheat bran through an 80-mesh sieve, mix with 700g of water and stir for 30min to obtain a suspension, add 40 parts of α-amylase, and the enzymolysis time is 10h; after the enzymolysis is completed, heat to 115°C and inactivate the enzyme for 12min; then add 250 parts of a 20g / L sodium hydroxide aqueous solution, stir for 6h, adjust the pH value of the system to 4 with 35% hydrochloric acid, then centrifuge at 10000rpm for 50min, collect the supernatant, add 250 parts of a 75% ethanol aqueous solution to precipitate the supernatant, stir for 30min, filter, collect the precipitate, and freeze-dry at 30°C for 20h to obtain a wheat bran hydrolysate; S32. According to the mass fractions, 100 parts of potato starch are added to 70 parts of an aqueous solution of wheat bran hydrolysate having a mass concentration of 15%, stirred at 65°C for 60 minutes, then heated to 95°C, stirred for 30 minutes, cooled to 35°C, stirred for 30 minutes, and then centrifuged at 10,000 rpm for 50 minutes. The precipitate is then collected and freeze-dried at 30°C for 26 hours to obtain modified potato starch.
[0031] Preparation Example 2 Preparation of Graphene Oxide Modified 2-Carboxyethylphenyl Hypophosphorous Acid The preparation method of graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid comprises the following steps: S51, dispersing 100 parts of 2-carboxyethylphenylphosphorous acid and 10 parts of graphene oxide in a solution consisting of 12 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 30 parts of water according to mass fractions to obtain a mixed solution; S52, heating the mixed solution to 46°C, stirring at a rate of 800 rpm, reacting for 500 min, filtering, and vacuum drying at 75°C for 24 h, grinding and sieving to obtain graphene oxide-modified 2-carboxyethylphenylphosphorous acid with a particle size of 3-5 μm.
[0032] Preparation Example 3 Preparation of waterproofing agent The waterproofing agent comprises the following raw materials by weight: 40 parts of tannic acid, 35 parts of maltodextrin, 30 parts of sodium sulfate, and 38 parts of water. The preparation method of the waterproofing agent is to mix maltodextrin, sodium sulfate and water evenly by weight, heat to 30°C, react for 60 minutes, then add tannic acid thereto, heat to 50°C, and react for 4 hours to obtain the waterproofing agent.
[0033] Example 1 A flame-retardant composite paper core with high flexibility in the outer layer and high hardness in the inner layer, which comprises, from the inside to the outside, a hard flame-retardant kraft paper layer, a flame-retardant glue layer, a foam paper layer and a soft flame-retardant kraft paper layer in sequence, wherein the flame-retardant glue layer is prepared by coating the flame-retardant glue on the surface of the hard flame-retardant kraft paper layer and bonding the foam paper layer, wherein the flame-retardant glue comprises the following preparation raw materials by weight: 50 parts of modified potato starch, 3 parts of phenolic resin, 5 parts of flame retardant, 5 parts of waterproofing agent, 6 parts of amino acrylate, 0.5 parts of preservative, and 280 parts of water, wherein the flame retardant is graphene oxide modified 2-carboxyethyl phenyl hypophosphorous acid, the inner diameter of the flame-retardant composite paper core is 74 mm, the thickness is 9 mm, the thickness of the hard flame-retardant kraft paper layer is 2 mm, the soft flame-retardant kraft paper layer is 2 mm, the foam paper layer is 5 mm, and the preservative is composed of sodium benzoate and potassium sorbate in a mass ratio of 1:2.
[0034] The method for preparing the flame-retardant composite paper core having high outer layer flexibility and high inner layer hardness comprises the following steps: S91. Evenly stir the modified potato starch, phenolic resin, flame retardant, waterproofing agent, urethane acrylate, preservative and water according to their weight proportions to obtain a flame retardant glue; S92, selecting hard flame retardant kraft paper of specified thickness as raw material, and rolling to form a hard flame retardant kraft paper layer paper core; S93. Evenly apply flame retardant glue on the outer surface of the hard flame retardant kraft paper core, and then adhere one side of the foam paper to the outer surface of the hard flame retardant kraft paper core to make them tightly combined through the bonding process, and then roll the soft flame retardant kraft paper layer on the outer layer of the foam paper again, and dry it at a temperature of 90°C for 30 minutes to obtain a flame retardant composite paper core with a moisture content of 7% and a high outer layer flexibility and a high inner layer hardness.
[0035] Example 2 A flame-retardant composite paper core with high flexibility in the outer layer and high hardness in the inner layer, which comprises, from the inside to the outside, a hard flame-retardant kraft paper layer, a flame-retardant glue layer, a foam paper layer and a soft flame-retardant kraft paper layer, wherein the flame-retardant glue layer is prepared by coating the flame-retardant glue on the surface of the hard flame-retardant kraft paper layer and bonding the foam paper layer, wherein the flame-retardant glue, by weight, comprises the following raw materials: 60 parts of modified potato starch, 5 parts of phenolic resin, 7 parts of flame retardant, 6 parts of waterproofing agent, 7 parts of amino acrylate, 0.6 parts of preservative, 300 parts of water, the flame retardant is graphene oxide modified 2-carboxyethyl phenyl hypophosphorous acid, the inner diameter of the flame retardant composite paper core is 76mm, the thickness is 9.5mm, the thickness of the hard flame retardant kraft paper layer is 1.5mm, the soft flame retardant kraft paper layer is 1.5mm, the foam paper layer is 6.5mm, and the preservative is composed of sodium benzoate and potassium sorbate in a mass ratio of 1:2.
[0036] The method for preparing the flame-retardant composite paper core having high outer layer flexibility and high inner layer hardness comprises the following steps: S91. Evenly stir the modified potato starch, phenolic resin, flame retardant, waterproofing agent, urethane acrylate, preservative and water according to their weight proportions to obtain a flame retardant glue; S92, selecting hard flame retardant kraft paper of specified thickness as raw material, and rolling to form a hard flame retardant kraft paper layer paper core; S93. Evenly apply flame retardant glue on the outer surface of the hard flame retardant kraft paper core, and then adhere one side of the foam paper to the outer surface of the hard flame retardant kraft paper core to make them tightly combined through the bonding process, and then roll the soft flame retardant kraft paper layer on the outer layer of the foam paper again, and dry it at a temperature of 90°C for 35 minutes to obtain a flame retardant composite paper core with a moisture content of 6% and high flexibility of the outer layer and high hardness of the inner layer.
[0037] Example 3 A flame-retardant composite paper core with high flexibility in the outer layer and high hardness in the inner layer, which comprises, from the inside to the outside, a hard flame-retardant kraft paper layer, a flame-retardant glue layer, a foam paper layer and a soft flame-retardant kraft paper layer, wherein the flame-retardant glue layer is prepared by coating the flame-retardant glue on the surface of the hard flame-retardant kraft paper layer and bonding the foam paper layer, wherein the flame-retardant glue, by weight, comprises the following raw materials: 55 parts of modified potato starch, 4 parts of phenolic resin, 6 parts of flame retardant, and 5.5 parts of waterproofing agent , 6.5 parts of amino acrylate, 0.55 parts of preservative, and 290 parts of water. The flame retardant is graphene oxide modified 2-carboxyethyl phenyl hypophosphorous acid. The inner diameter of the flame retardant composite paper core is 75 mm and the thickness is 9.3 mm. The thickness of the hard flame retardant kraft paper layer is 2 mm, the soft flame retardant kraft paper layer is 1.5 mm, and the foam paper layer is 5.8 mm. The preservative is composed of sodium benzoate and potassium sorbate in a mass ratio of 1:2.
[0038] The method for preparing the flame-retardant composite paper core having high outer layer flexibility and high inner layer hardness comprises the following steps: S91. Evenly stir the modified potato starch, phenolic resin, flame retardant, waterproofing agent, urethane acrylate, preservative and water according to their weight proportions to obtain a flame retardant glue; S92, selecting hard flame retardant kraft paper of specified thickness as raw material, and rolling to form a hard flame retardant kraft paper layer paper core; S93. Evenly apply flame retardant glue on the outer surface of the hard flame retardant kraft paper core, and then adhere one side of the foam paper to the outer surface of the hard flame retardant kraft paper core to make them tightly combined through the bonding process, and then roll the soft flame retardant kraft paper layer on the outer layer of the foam paper again, and dry it at a temperature of 90°C for 33 minutes to obtain a flame retardant composite paper core with a moisture content of 6.4%, high flexibility of the outer layer and high hardness of the inner layer.
[0039] Comparative Example 1 Same as Example 3, except that an equal amount of potato starch is used instead of modified potato starch.
[0040] Comparative Example 2 The same as Example 3, except that an equal amount of 2-carboxyethylphenyl hypophosphorous acid is used instead of graphene oxide-modified 2-carboxyethylphenyl hypophosphorous acid.
[0041] Comparative Example 3 The same as Example 3, except that the amount of waterproofing agent added is 0 parts.
[0042] Performance Testing 1. The flame-retardant composite paper cores with high outer layer flexibility and high inner layer hardness obtained in Examples 1 to 3 were sampled and tested as follows. The test results are shown in Table 1.
[0043] Moisture content, radial compression resistance: tested in accordance with BB / T0032-2006 standard.
[0044] 2. The flame retardant glue prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was sampled, and the flame retardant glue was coated on the glass surface and dried to obtain a strip with a thickness of 2 mm. The following tests were performed, and the test results are shown in Table 2.
[0045] Adhesion strength test: Tested using the method described in GB / T6541-2011; Flame retardancy test: Place the sample to be tested in a glass combustion tube, introduce a nitrogen-oxygen mixed gas flow, record the minimum oxygen concentration required for combustion, and take the average value of five tests for each group; Water resistance test: The flame retardant glue prepared in Example 1 to Example 3 and Comparative Example 1 to Comparative Example 3 was coated on 120 g / m 2 The amount of glue applied on the flame retardant kraft paper layer is 10g / m 2 , paste another flame retardant kraft paper, and after drying, put the pasted flame retardant kraft paper into 25℃ water, start timing, and stop timing when the flame retardant kraft paper is separated.
[0046] 3. Security Testing The flame retardant composite paper core prepared in Example 3 was sent to SGS Testing Center for safety testing in accordance with EU RoHS Directive 2011 / 65 / EU and its revised Directive (EU) 2015 / 863. The test basis is shown in Table 3, and the test results are shown in Tables 4 and 5.
[0047] Table 3 Test basis Table 1 Paper core performance test Table 2 Flame retardant glue performance test project Oxygen Index Adhesion strength / N / mm Water resistance / min Example 1 37.9 514 55 Example 2 38.4 498 52 Example 3 38.8 526 58 Comparative Example 1 33.5 352 38 Comparative Example 2 22.6 446 45 Comparative Example 3 36.6 476 29 Table 4 Heavy metal element content Test items result Method detection limit Limits Lead (Pb) 7mg / kg 2mg / kg 1000mg / kg Cadmium (Cd) ND 2mg / kg 100mg / kg Mercury (Hg) ND 2mg / kg 1000mg / kg Table 5 Polybrominated biphenyls (PBBs) Analyzing the data in Tables 1, 2, 4 and 5, we can see that: 1) The flame-retardant composite paper core with high outer layer flexibility and high inner layer hardness prepared in Examples 1 to 3 has high radial pressure, is green, environmentally friendly and safe, has high flame retardancy and low moisture content (6-7%). The flame-retardant glue prepared in this application has excellent water resistance, flame retardancy and bonding strength, and is also highly safe and green.
[0048] 2) The performance comparison analysis of the flame retardant glue prepared in combination with Example 3 and Comparative Example 1 shows that the modified potato starch can improve the gel strength of the mixed slurry and the water holding capacity of the potato starch gel through the hydrogen bond interaction between the wheat bran enzymolyzate and the potato starch. This is conducive to improving the bonding strength and water resistance of the flame retardant glue, so that the composite paper core has higher radial pressure and compressive strength. As one of the main components of the flame retardant glue, the modified potato starch works together with other raw materials (such as phenolic resin, flame retardant, etc.) to form a glue layer with excellent flame retardancy. This glue layer can effectively prevent the spread of flames and improve the flame retardant properties of the composite paper core. Modified potato starch is a natural degradable polymer material with good biocompatibility and environmental friendliness. Using modified potato starch as the main component of the adhesive can reduce pollution to the environment and improve the safety and environmental performance of the product.
[0049] 3) The performance comparison analysis of the flame retardant glue prepared in combination with Example 3 and Comparative Example 2 shows that the graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid prepared in this application is used as a flame retardant to promote the flame retardant to form a foam layer, release a large amount of non-flammable gas, dilute the oxygen in the environment, and thus improve the flame retardant effect. Modification by γ-aminopropyltrimethoxysilane helps the combination between graphene oxide and 2-carboxyethylphenyl hypophosphorous acid, enhances the interaction between them, and improves the compatibility and dispersibility in the flame retardant glue. Graphene oxide forms a three-dimensional network structure, which further enhances the flame retardant effect of the composite paper core. Graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid works together with other ingredients (such as phenolic resin, amino ester acrylate, etc.) to improve the water resistance, flame retardancy and bonding strength of the flame retardant glue, while being highly safe and environmentally friendly.
[0050] 4) The performance comparison analysis of the flame retardant glue prepared in combination with Example 3 and Comparative Example 3 shows that the prepared waterproofing agent can increase the waterproofing performance of paper products, which is not easily damaged even when soaked in water, and greatly improves the bonding strength. The waterproofing agent works synergistically with other components in the flame retardant glue to jointly improve the water resistance and flame retardancy of the composite paper core.
[0051] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.
Claims
1. A flame retardant composite paper core with high outer layer flexibility and high inner layer hardness, characterized in that: From the inside to the outside, it includes a hard flame-retardant kraft paper layer, a flame-retardant glue layer, a foam paper layer and a soft flame-retardant kraft paper layer. The flame-retardant glue layer is prepared by coating the flame-retardant glue on the surface of the hard flame-retardant kraft paper layer and bonding the foam paper layer. The flame-retardant glue includes the following raw materials by mass: 50-60 parts of modified potato starch, 3-5 parts of phenolic resin, 5-7 parts of flame retardant, 5-6 parts of waterproofing agent, 6-7 parts of urethane acrylate, 0.5-0.6 parts of preservative and 280-300 parts of water.
2. According to claim 1, a flame-retardant composite paper core with high outer layer flexibility and high inner layer hardness, characterized in that: The inner diameter of the flame retardant composite paper core is 74-76 mm, and the thickness is 9-9.5 mm. The thickness of the hard flame retardant kraft paper layer is 1.5-2 mm, the thickness of the soft flame retardant kraft paper layer is 1.5-2 mm, and the thickness of the foam paper layer is 5-6.5 mm.
3. The flame-retardant composite paper core according to claim 1, characterized in that: The preparation method of the modified potato starch comprises the following steps: S31, according to the mass fraction, grind 200 parts of wheat bran through an 80-mesh sieve, mix with 700g of water and stir for 30min to obtain a suspension, add 40 parts of α-amylase, and the enzymolysis time is 10h; after the enzymolysis is completed, heat to 115°C and inactivate the enzyme for 12min; then add 250 parts of a 20g / L sodium hydroxide aqueous solution, stir for 6h, adjust the pH value of the system to 4 with 35% hydrochloric acid, then centrifuge at 10000rpm for 50min, collect the supernatant, add 250 parts of a 75% ethanol aqueous solution to precipitate the supernatant, stir for 30min, filter, collect the precipitate, and freeze-dry at 30°C for 20h to obtain a wheat bran hydrolysate; S32. According to the mass fractions, 100 parts of potato starch are added to 70 parts of an aqueous solution of wheat bran hydrolysate having a mass concentration of 15%, stirred at 65°C for 60 minutes, then heated to 95°C, stirred for 30 minutes, cooled to 35°C, stirred for 30 minutes, and then centrifuged at 10,000 rpm for 50 minutes. The precipitate is then collected and freeze-dried at 30°C for 26 hours to obtain modified potato starch.
4. The flame-retardant composite paper core according to claim 1, characterized in that: The flame retardant is graphene oxide modified 2-carboxyethyl phenyl hypophosphorous acid.
5. The flame-retardant composite paper core according to claim 4, characterized in that: The preparation method of graphene oxide modified 2-carboxyethylphenyl hypophosphorous acid comprises the following steps: S51, dispersing 100 parts of 2-carboxyethylphenylphosphorous acid and 10 parts of graphene oxide in a solution consisting of 12 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 30 parts of water according to mass fractions to obtain a mixed solution; S52, heating the mixed solution to 46°C, stirring at a rate of 800 rpm, reacting for 500 min, filtering, and vacuum drying at 75°C for 24 h, grinding and sieving to obtain graphene oxide-modified 2-carboxyethylphenylphosphorous acid with a particle size of 3-5 μm.
6. The flame-retardant composite paper core according to claim 1, characterized in that: The waterproofing agent comprises the following raw materials, calculated by weight: 40 parts of tannic acid, 35 parts of maltodextrin, 30 parts of sodium sulphate and 38 parts of water.
7. The flame-retardant composite paper core according to claim 6, characterized in that: The preparation method of the waterproofing agent comprises the following steps: uniformly mixing maltodextrin, sodium sulfate and water according to their weight fractions, heating to 30° C., reacting for 60 minutes, then adding tannic acid thereto, heating to 50° C., and reacting for 4 hours to obtain the waterproofing agent.
8. The flame-retardant composite paper core according to claim 1, characterized in that: The preservative is composed of sodium benzoate and potassium sorbate in a mass ratio of 1:
2.
9. A method for preparing a flame-retardant composite paper core having high outer layer flexibility and high inner layer hardness as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: S91. Evenly stir the modified potato starch, phenolic resin, flame retardant, waterproofing agent, urethane acrylate, preservative and water according to their weight proportions to obtain a flame retardant glue; S92, selecting hard flame retardant kraft paper of specified thickness as raw material, and rolling to form a hard flame retardant kraft paper layer paper core; S93. Evenly apply flame retardant glue on the outer surface of the hard flame retardant kraft paper core, and then adhere one side of the foam paper to the outer surface of the hard flame retardant kraft paper core to make them tightly combined through the bonding process, and then roll the soft flame retardant kraft paper layer on the outer layer of the foam paper again, and dry it at a temperature of 90°C for 30-35 minutes to obtain a flame retardant composite paper core with a moisture content of 6%-7% and high flexibility of the outer layer and high hardness of the inner layer.
Citation Information
Patent Citations
Phosphor-rich graphene flame-retardant agent and preparation method thereof
CN106883450A
Composite material for high-strength corrugated board and preparation method of composite material
CN115384164A
Glue for paper products and preparation method thereof
CN116515420A
Environment-friendly seamless paper tube and processing method thereof
CN117507493A
Environmental protection packaging material and its manufacturing method
CN207291180U