Fluidized roasting device and roasting method
By designing the holes and ring beams on the upper part of the furnace body in a fluidized roasting furnace, and combining the integrated design of refractory materials and steel furnace shells, the structural instability problem of large roasting furnaces is solved and the length of the furnace body is achieved Stable time operation and improved resource utilization.
Patent Information
- Application Number
- CN202411191962.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
Large fluidized roasting furnaces can easily lead to unstable furnace structure under high temperature and large span conditions, causing over-temperature distortion and deformation of the furnace shell, affecting safety and reliability.
A fluidized roasting device is designed, including a circular hole and a rectangular hole above the smoke exhaust port on the upper part of the furnace body, and a ring beam is arranged on the top of the furnace, combining the integrated design of refractory materials and steel furnace shells to increase heat. Stress releases space and airtightness, and reinforcement ribs are arranged along the height and circumference to enhance stability.
It effectively stabilizes the ball crown furnace top of a large fluidized roasting furnace, extends the continuous and stable production time of the furnace body, reduces the proportion of SO2 converted into SO3 in the flue gas, improves resource utilization and reduces production costs.
Smart Images

Figure CN118936071A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of pyrometallurgy, and in particular relates to a fluidized roasting device and a roasting method. Background Art
[0002] The hydrometallurgical zinc smelting process accounts for more than 80% of the world's zinc production capacity. In addition to the direct leaching of zinc sulfide concentrate by pressurized oxygen leaching, most hydrometallurgical zinc smelting uses roasted ore (also known as roasted sand) for leaching. Fluidized roasting furnace is the main equipment for roasting zinc sulfide concentrate. Since the large-scale fluidized roasting furnace is conducive to increasing the production capacity of a single equipment, reducing labor quotas, and improving the level of automation, it has become a direction of continuous research and exploration in the zinc smelting industry.
[0003] However, as the furnace area continues to increase, the production capacity of a single device continues to increase, the gas flow rate increases exponentially, the vibration caused by the air flow movement increases, and the thermal vibration effect caused by temperature changes will increase the destructive effect on the stability of the furnace structure. In particular, the spherical crown furnace top of a large roasting furnace has a large design span, high furnace construction precision, high operating temperature (900-1100℃), large temperature gradient between the upper and lower surfaces, and complex stress changes, which poses a major challenge to the safety and reliability of the roasting furnace body.
[0004] The Chinese patent with publication number CN101900484B discloses a fluidized roasting furnace, comprising: a furnace body, the furnace body having a feeding port, a discharging port and a smoke outlet; a furnace top, the furnace top is integrated and arranged on the top of the furnace body; and a bellows, the bellows having an air inlet and an air outlet, the bellows being located below the furnace body and communicating with the interior of the furnace body through the air outlet. The furnace body comprises an outermost metal furnace shell, an innermost refractory brick layer, and an insulating brick layer located in the middle. The outermost metal furnace shell serves as a frame for the entire furnace body, so that other furnace body layers can be arranged inside the metal furnace shell. The innermost layer of the furnace body is a refractory brick layer, and by arranging an insulating brick layer in the middle, the temperature of the metal furnace shell can be prevented from being too high. Since the refractory brick layer has good thermal conductivity, the heat in the furnace can be prevented from being conducted from the refractory brick layer to the metal furnace shell by arranging the insulating brick layer. This technical solution can easily lead to overheating and distortion of the furnace shell during production, causing serious safety hazards, and necessitating the shutdown of the roasting furnace for maintenance. Summary of the invention
[0005] The present invention aims to provide a fluidized roasting device and a roasting method, wherein the fluidized roasting device is not prone to causing overheating and distortion of the furnace shell during production.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A fluidized roasting device comprises a furnace body, wherein the bottom of the furnace body is provided with an operation port, a material discharge port and a heat exhaust device, the upper part of the furnace body is provided with a smoke exhaust port, the top of the furnace body is provided with a furnace top, and a hole is provided on the furnace body above the smoke exhaust port.
[0008] The holes above the smoke outlet of the furnace body make the furnace body integrated with each other, increase the release space of the thermal stress of the spherical crown furnace top of the large fluidized roasting furnace, and are beneficial to the stability of the furnace top.
[0009] According to the embodiments of the present invention, the present invention can be further optimized. The following is the technical solution formed after optimization:
[0010] The holes include circular holes opened along the circumferential direction of the furnace body, and rectangular holes are opened below the circular holes in an offset manner.
[0011] Preferably, the center line of the circular hole is offset from the center line of the rectangular hole.
[0012] Preferably, the fluidized roasting device is a large-scale fluidized roasting furnace body, and the diameter of the fluidized bed is greater than 14m.
[0013] Preferably, the diameter of the circular hole is 150-300 mm, the side length of the rectangular hole is 150 mm x 300 mm, and the rectangular hole is located 300-500 mm below the circular hole.
[0014] The round hole and the square hole of the furnace shell make the furnace body integrated with each other.
[0015] In one of the preferred embodiments, 1 to 4 ring beams are arranged on the upper part of the furnace body, and the ring beams are located above the smoke exhaust port.
[0016] 1 to 4 ring beams are arranged above the exhaust port of the fluidized bed roasting furnace to make the furnace bodies merge with each other, disperse the thermal stress of the furnace top, effectively stabilize the arch foot beam of the large-span spherical crown furnace top, and change the way traditional boiling furnaces are supported by the internal support plate of the furnace shell.
[0017] In one of the preferred embodiments, the furnace body includes a furnace shell, a heat insulation material and a heating surface from the outside to the inside, the furnace shell includes an upper furnace shell, a middle furnace shell and a lower furnace shell, and the heating surface is refractory bricks and castables are laid in intervals or staggered.
[0018] In one of the preferred embodiments, the upper furnace shell, the heat insulating material and the heating surface of the upper furnace shell are designed in an integrated manner.
[0019] The holes above the smoke outlet of the furnace body and 1 to 4 ring beams are arranged on the upper part of the smoke outlet to make the refractory material of the heating surface and the furnace shell merge with each other. The integration of the upper furnace shell and the refractory material increases the airtightness of the spherical crown top of the roasting furnace, is beneficial to the uniformity of the flow field and temperature field in the fluidized roasting furnace, and reduces the proportion of SO2 converted to SO3 in the flue gas.
[0020] The refractory material of the heating surface of the fluidized bed roasting furnace is integrated with the steel furnace shell, which increases the release space of the thermal stress of the spherical crown furnace top of the large fluidized bed roasting furnace and is beneficial to the stability of the furnace top.
[0021] Preferably, the filling thickness of the thermal insulation material is 10-25 mm.
[0022] Preferably, the thermal insulation material is an asbestos board or multiple layers of aluminum silicate fiberboard arranged in staggered layers.
[0023] Preferably, the furnace shell is provided with furnace shell reinforcing ribs along the height direction and the circumferential direction.
[0024] The upper, middle and lower shells of the fluidized bed roasting furnace are provided with reinforcing ribs in the height and circumferential directions to increase the overall stability of the fluidized bed roasting furnace. Under the thermal shock caused by airflow and temperature changes, the refractory materials on the heating surface are not prone to shear stress that destroys the thermal stability of the furnace body and causes overheating of the furnace shell. The furnace body can produce continuously and stably for more than 700 days.
[0025] Preferably, the center line of the material discharge port and the center line of the smoke discharge port are in a straight line.
[0026] Preferably, a throwing device is installed on the outer side of the throwing port.
[0027] Preferably, a ceiling is installed on the top of the furnace roof.
[0028] Preferably, the ring beam is an arch foot ring beam.
[0029] Preferably, an inspection platform is installed on the outer edge of the ring beam.
[0030] The present invention also discloses a roasting method of the fluidized roasting device, wherein the zinc concentrate is thrown into the fluidized roasting device according to claim 1 at a speed of not less than 17 m / s, and the zinc concentrate is uniformly mixed with oxygen-enriched air with an oxygen volume concentration of less than 30% in the furnace to perform boiling oxidation desulfurization.
[0031] Under the action of hot air flow, the zinc concentrate jumps up and down in a boiling state, undergoing boiling oxidation desulfurization.
[0032] In one preferred embodiment, the zinc concentrate contains 8% to 12% water and 1.24% to 2.5% lead (impurities).
[0033] In one preferred embodiment, the zinc concentrate particle size D90>53um. (fine)
[0034] In one preferred embodiment, the residence time of the zinc concentrate in the furnace is 2.5 to 3 hours, and the insoluble sulfur content of the roasted sand is controlled to be less than 0.1%.
[0035] In one preferred embodiment, 40-55 wt% of the materials entering the furnace are roasted sand, and 55-40 wt% are roasting dust.
[0036] Preferably, the zinc concentrate is thrown into the fluidized roasting device through a throwing machine.
[0037] Preferably, the calcination temperature is 900-1100°C.
[0038] The zinc concentrate includes Zn: 43% (lean) to 56%, Pb: 1.24% to 2.5%, and S: 31.6% to 40%.
[0039] The invention adopts a new furnace structure, has good heat-gathering and temperature-stabilizing effects, and can process fine, lean, and mixed raw materials. It is a method for improving resource utilization, reducing production costs, and improving the economic benefits of enterprises.
[0040] The specific scheme of the present invention is as follows:
[0041] (1) The complex zinc concentrate is thrown into a large fluidized bed furnace through two throwing machines at a speed of not less than 17 m / s, wherein the particle size of the mineral entering the furnace is D(90)>53 um;
[0042] (2) The feed zinc concentrate contains 8% to 12% water and 1.24% to 2.5% lead.
[0043] (3) The fluidized bed roasting furnace device includes: a ceiling (1), a furnace cover (1), a spherical crown furnace top (1), an inspection platform (1), a furnace shell (1) (upper furnace shell + middle furnace shell + lower furnace shell), refractory materials (lightweight + heavyweight), an upper smoke exhaust port (1), a boiling layer discharge port (1), a boiling layer burner (4-10), a boiling layer operation port (4), a boiling layer heat exhaust device (4-10), a boiling layer throwing port (2), a bellows (1), and main air inlets (1-3).
[0044] (4) The zinc concentrate entering the furnace is evenly mixed with oxygen-rich air (<25%) in the furnace. Under the action of the hot air flow, the ore particles jump up and down in a boiling state to undergo oxidative desulfurization. The material stays in the furnace for 2.5 to 3 hours, and the insoluble sulfur content of the roasted sand is controlled to be less than 0.1%.
[0045] (5) 40-55 wt% of the materials entering the furnace are roasted sand, and 55-40 wt% are roasting dust.
[0046] (6) The fluidized bed roasting furnace is a concentrated fluidized bed with two operating ports, one discharge port and one smoke exhaust port. The feed port and the discharge port are distributed at an angle of 170° to 190°, and the center line of the discharge port and the center line of the smoke duct port are in a straight line.
[0047] (7) The internal heating surface of the fluidized bed roaster is made of refractory bricks and castables laid in intervals or staggered. The space between the heating surface refractory material and the steel furnace shell is filled with insulation material (asbestos board or multi-layer aluminum silicate fiberboard arranged in staggered layers), with a filling thickness of 10-25mm.
[0048] (8) The steel shell of the fluidized bed roasting furnace is welded from steel plates (Q235B or Q345) and is divided into three parts: the cross-sectional area ratio of the upper furnace shell to the lower furnace shell is 1.5-2.0, and the height of the middle furnace shell is 6-7m.
[0049] (9) One to four ring beams are arranged on the upper furnace shell of the fluidized bed roasting furnace smoke outlet, and the spacing between the ring beams is about 400mm to 1000mm.
[0050] (10) The upper, middle and lower shells of the fluidized bed roasting furnace are reinforced with ribs in the height and circumferential directions, and the height and circumferential spacing of the ribs are 2m to 4m and 1.5m to 2.0m respectively.
[0051] (11) A hole with a diameter of 150 to 300 mm is opened in the upper furnace shell of the fluidized roasting furnace exhaust port along the circumferential direction, and a rectangular hole with a size of 150 mm x 300 mm is opened 300 to 500 mm below the center line of the circular hole. The circular hole and the square hole of the furnace shell make the refractory material of the heating surface of the fluidized roasting furnace and the steel furnace shell integrated with each other, increase the release space of the thermal stress of the spherical crown furnace roof of the large fluidized roasting furnace, and benefit the stability of the furnace roof.
[0052] (12) The integration of the upper furnace shell and refractory materials of the fluidized bed roasting furnace increases the airtightness of the spherical crown of the roasting furnace, is conducive to the uniformity of the flow field and temperature field in the fluidized bed roasting furnace, and reduces the proportion of SO2 converted to SO3 in the flue gas.
[0053] (13) An inspection platform is set on the upper part of the arch foot beam of the fluidized bed roasting furnace in the circumferential direction to ensure daily maintenance and repair.
[0054] (14) A ceiling 500 mm larger than the outer diameter of the upper furnace shell is set on the top of the fluidized bed roasting furnace to prevent rainwater from gathering on the spherical crown furnace roof and damaging the lightweight materials on the furnace roof.
[0055] The beneficial effects of the present invention are as follows:
[0056] (1) High-speed feeding of large fluidized bed roasting furnaces is conducive to the uniform distribution of high-humidity materials in the furnace, reducing the sintering of the boiling layer caused by local overheating of the boiling layer and the effect of airflow scouring the furnace wall, and improving the adaptability to complex raw materials, especially high-lead materials.
[0057] (2) Large-scale fluidized bed roasting furnaces use oxygen-enriched roasting, which is conducive to the establishment of thermal balance in the boiling layer, and controls the smoke rate and insoluble sulfur in roasted sand to less than 0.3% and 0.1% respectively, increasing the production capacity of a single fluidized bed roasting furnace by 25%.
[0058] (3) One to four ring beams are arranged above the exhaust port of the fluidized bed roasting furnace to allow the refractory material of the heating surface to fuse with the furnace shell, dispersing the thermal stress on the furnace top and effectively stabilizing the arch foot beam of the large-span spherical crown furnace top, thus changing the traditional way of supporting the boiling furnace by the internal support plate of the furnace shell.
[0059] (4) The upper, middle and lower shells of the fluidized bed roasting furnace are provided with reinforcing ribs in the height and circumferential directions to increase the overall stability of the fluidized bed roasting furnace. Under the thermal shock caused by airflow and temperature changes, the refractory materials on the heating surface are not prone to shear stress that damages the thermal stability of the furnace body and causes overheating of the furnace shell. The furnace body can operate in continuous and stable production for more than 700 days.
[0060] (5) The integrated structure of the upper furnace shell and refractory materials of the fluidized bed roasting furnace extends the airtightness of the spherical crown of the roasting furnace, which is beneficial to the uniformity of the flow field and temperature field in the fluidized bed roasting furnace, reduces the proportion of SO2 in the flue gas converted to SO3, makes the volume fraction of SO3 in the flue gas less than 0.1%, reduces the amount of polluted acid in the acid-making system, and makes the efficiency recovery rate of sulfuric acid production reach more than 96%. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 It is a schematic structural diagram of an embodiment of the present invention.
[0062] Figure 2 This is a partial enlarged schematic diagram of the ring beam.
[0063] Among them, 1—ceiling; 2—ring beam; 3—inspection platform; 4—furnace shell reinforcement ribs; 5—upper furnace shell; 6—middle furnace shell; 7—lower furnace shell; 8—throwing device;
[0064] 9-furnace body; 10-operation port; 11-smoke exhaust port; 12-throwing port, 13-discharging port, 14-furnace top, 15-heat exhaust device, 16-hole, 161-round hole, 162-rectangular hole. DETAILED DESCRIPTION
[0065] like Figure 1-2As shown, a fluidized roasting device comprises a furnace body 9, wherein the furnace body 9 is provided with an operation port 10, a discharge port, and a heat exhaust device 15 at the bottom, a smoke exhaust port 11 is provided at the top of the furnace body 9, a furnace top 14 is provided at the top of the furnace body 9, and a hole 16 is provided on the furnace body above the smoke exhaust port 11. The hole 16 comprises a circular hole 161 provided along the circumferential direction of the furnace body, and a rectangular hole 162 is provided below the circular hole 161. One to four ring beams 2 are arranged on the upper part of the furnace body 9, and the ring beam 2 is located above the smoke exhaust port 10. The furnace body 9 comprises a furnace shell, a heat insulating material, and a heating surface from the outside to the inside, wherein the furnace shell comprises an upper furnace shell 5, a middle furnace shell 6, and a lower furnace shell 7, and the heating surface is made of refractory bricks and castables in intervals or staggered masonry. The upper furnace shell 5, the heat insulating material, and the heating surface of the upper furnace shell 5 are designed in an integrated manner.
[0066] The zinc concentrate is put into the fluidized bed roasting furnace by a throwing machine, and the roasting temperature is controlled at 950℃~1050℃ to produce high-temperature roasted sand and roasted dust.
[0067] Table 1 Device and method for stabilizing the furnace body of a large fluidized roasting furnace
[0068]
[0069] The results show that when Examples 1-4 treat zinc concentrate containing 8-12% water, the insoluble sulfur in roasted dust is less than 0.3%, the insoluble sulfur in roasted sand is less than 0.1%, the boiling layer temperature is less than 1050°C, no sintering occurs, and the furnace body can operate continuously for up to 2 years. In addition, with the increase in the number of ring beams on the upper part of the smoke exhaust port, the refractory material of the heating surface and the furnace shell are integrated with each other, and the continuous operation days of the furnace body are significantly increased.
[0070] Comparative Examples 1-4
[0071] Repeat Example 1-4, except that the throwing speed is 16m / s. It is found that the boiling layer has local overheating of the pile, and the temperature fluctuation of the upper and lower parts of the boiling layer of the roasting furnace is greater than 30°C, resulting in the phenomenon of "blowing through" of the furnace bed and the furnace dead.
[0072] Comparative Examples 5-8
[0073] Repeat Example 1-4, except that the particle size D(90) of the concentrate entering the furnace is 50um and the water content is 7%. It is found that the smoke rate during the roasting process of the roasting furnace is greater than 55wt%, causing the waste heat boiler of the subsequent section of the roasting furnace to be blocked, the boiler outlet smoke temperature is high, the load of the electric dust collector is increased, and the purification of the acid production system is blocked, so the system has to be shut down for maintenance.
[0074] Comparative Examples 9-12
[0075] Repeat Examples 1-4, except that: the upper furnace shell of the smoke outlet has no round hole or square hole, and the upper ring beam cannot be integrated with the heating surface refractory material, and only serves as a reinforcing rib. Production practice has proved that during the start-up and shutdown of the roasting furnace, due to the inconsistency of the thermal expansion coefficients of the heating surface refractory material and the furnace shell, a high-temperature flue gas flow channel is formed between the refractory material inside the furnace shell and the furnace shell, resulting in overheating and distortion of the furnace shell during production, causing serious safety hazards, and the roasting furnace has to be shut down for maintenance.
[0076] Comparative Examples 13-14
[0077] Example 3-4 was repeated, except that the oxygen concentration (vol%) of the wind box was greater than 25%. The results showed that the temperature of the boiling layer of the roasting furnace was greater than 1100°C, the low melting point materials in the charge melted, and the boiling layer heat removal device sintered, resulting in the heat being unable to be removed in time, destroying the fluidization of the charge in the furnace, causing the entire sintering to stop production.
[0078] Comparative Example 15
[0079] Example 4 was repeated, except that the water content of the concentrate entering the furnace was 13%. It was found that the materials entering the furnace adhered to the belt of the throwing machine, and the pressure in the roasting furnace could not be controlled, positive pressure occurred, the belt and other equipment were burned, and the on-site operating environment was bad.
Claims
1. A fluidized bed roasting device, comprising a furnace body (9), wherein the bottom of the furnace body (9) is provided with an operation port (10), a material discharge port, and a heat exhaust device (15), the upper part of the furnace body (9) is provided with a smoke exhaust port (11), and the top of the furnace body (9) is provided with a furnace top (14), characterized in that: A hole (16) is provided on the furnace body above the smoke exhaust port (11).
2. The fluidized bed roasting device according to claim 1, characterized in that: The hole (16) comprises a circular hole (161) opened along the circumferential direction of the furnace body, and a rectangular hole (162) is opened below the circular hole (161) in a staggered manner.
3. The fluidized bed roasting device according to claim 1, characterized in that: One to four ring beams (2) are arranged on the upper part of the furnace body (9), and the ring beam (2) is located above the smoke exhaust port (10).
4. The fluidized roasting device according to any one of claims 1 to 3, characterized in that: The furnace body (9) comprises a furnace shell, a heat insulating material and a heating surface from the outside to the inside, wherein the furnace shell comprises an upper furnace shell (5), a middle furnace shell (6) and a lower furnace shell (7), and the heating surface is constructed by alternately laying refractory bricks and castables.
5. The fluidized bed roasting device according to claim 4, characterized in that: The upper furnace shell (5), the heat insulating material and the heating surface of the upper furnace shell (5) are designed in an integrated manner.
6. A roasting method of the fluidized roasting device according to claim 1, characterized in that: The zinc concentrate is thrown into the fluidized roasting device according to claim 1 at a speed of not less than 17 m / s, and the zinc concentrate is uniformly mixed with oxygen-enriched air with an oxygen volume concentration of less than 25% in the furnace to perform boiling oxidation desulfurization.
7. The roasting method according to claim 6, characterized in that: The zinc concentrate contains 8% to 12% water and 1.24% to 2.5% lead.
8. The roasting method according to claim 6, characterized in that: Zinc concentrate particle size D90>53um.
9. The roasting method according to claim 6, characterized in that: The residence time of zinc concentrate in the furnace is 2.5 to 3 hours, and the insoluble sulfur content of roasted sand is controlled to be less than 0.1%.
10. The roasting method according to claim 6, characterized in that: 40-55wt% of the materials entering the furnace are roasted sand, and 55-40wt% are roasting dust.
Citation Information
Cited By
Pyrogenic desulfurization method and device for complex zinc concentrate
CN122061013A
A method and apparatus for complex zinc concentrate fire desulphurization
CN122061013B
Two-phase fluidized roasting method
CN122147050A
A two-phase fluidized roasting method
CN122147050B