Composite SERS (Surface Enhanced Raman Scattering) substrate based on titanium dioxide and metal nanoparticles as well as preparation method and application thereof
By constructing titanium dioxide three-dimensional anti-opal structure and metal nanoparticles on SERS substrates and modifying them with thiol molecules, the problem of insufficient detection capabilities of existing SERS substrates is solved, and efficient and rapid detection of polycyclic aromatic hydrocarbons is achieved. It is suitable for Environmental and industrial applications.
Patent Information
- Application Number
- CN202310533319.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
The existing SERS substrates have problems such as simple nanostructure, low incident optical coupling efficiency, insufficient enhancement ability and low adsorption efficiency of target molecules, making it difficult to achieve efficient detection of polycyclic aromatic hydrocarbons.
Using a composite SERS substrate based on titanium dioxide three-dimensional inverse opal structure and metal nanoparticles, a substrate with high coupling effect is formed by spin coating of polystyrene microspheres and metal nanoparticles, and the target molecule is adsorbed to improve detection ability.
It significantly improves the coupling effect between incident light and SERS substrate and the adsorption efficiency of target molecules, enhances the detection signal amplification ability, and realizes rapid, real-time and convenient detection of polycyclic aromatic hydrocarbons, which is suitable for environmental detection and industrial applications.
Smart Images

Figure CN118937298A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of surface enhanced Raman detection, and in particular to a composite SERS substrate based on titanium dioxide and metal nanoparticles, and a preparation method and application thereof. Background Art
[0002] Polycyclic aromatic hydrocarbons (PAHs) are aromatic hydrocarbons with two or more benzene rings, mainly formed by incomplete combustion or pyrolysis under reducing conditions of various mineral fuels (such as coal, oil and natural gas), wood, paper and other hydrocarbons. They are characterized by a wide variety, long degradation cycle, strong mutagenicity and carcinogenicity, and pose a huge threat to the ecological environment and human health. At present, the detection of PAHs mainly includes gas chromatography-mass spectrometry, fluorescence spectroscopy, electrochemical methods, etc. Although these methods are highly sensitive, they have the characteristics of complex sample pretreatment steps, cumbersome operations, and can only be performed under laboratory conditions. Therefore, it is of great significance to establish a set of rapid, real-time and convenient PAH detection technology.
[0003] As an emerging detection method, surface enhanced Raman spectroscopy (SERS) technology has the advantages of strong signal amplification ability, high sensitivity, rich chemical fingerprint information, simple operation, and in-situ detection. It is widely used in material, chemical, biological and medical detection and identification. The detection of PAHs using SERS technology requires, on the one hand, the construction of nano-substrates by gold and silver nanoparticles such as gold nanospheres, silver nanospheres, and gold nanorods; on the other hand, the PAHs are connected to the substrate through non-covalent bonding forces (physical adsorption, hydrophobic interaction, π-π stacking, etc.) to achieve Raman detection. SERS substrates are generally composed of metals such as gold and silver and semiconductors such as titanium dioxide, which can be prepared by chemical synthesis, vapor deposition, physical electron beam evaporation, etc. The adsorption of PAHs can be achieved by modifying molecules with special forces such as thiol and graphene on the SERS substrate. Therefore, how to assemble nanostructures of different shapes and types into SERS substrates with electromagnetic field enhancement areas and adsorb target molecules onto the surface of SERS substrates is the core issue of this detection technology.
[0004] However, the common SERS substrates currently have problems such as simple nanostructure, low coupling efficiency with incident light, insufficient enhancement ability, and low adsorption efficiency for target molecules. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of the existing SERS substrate, such as simple nanostructure, low coupling efficiency with incident light, insufficient enhancement ability, low adsorption efficiency of target molecules, etc., and to provide a SERS substrate and its preparation method and application.
[0006] In order to achieve the above object, the present invention provides a SERS substrate based on titanium dioxide and metal nanoparticles, comprising:
[0007] A substrate, a titanium dioxide three-dimensional inverse opal structure supported on the substrate, metal nanoparticles supported on the surface of the titanium dioxide three-dimensional inverse opal structure, and thiol modified on the metal nanoparticles;
[0008] The size of the metal nanoparticles is 30-300 nm;
[0009] The thickness of the titanium dioxide three-dimensional inverse opal structure is ≥3000 nm.
[0010] Preferably, the pore size of the titanium dioxide three-dimensional inverse opal structure is 200-1000 nm.
[0011] Preferably, the mercaptan is selected from one or more of n-propyl mercaptan, n-hexyl mercaptan and n-dodecyl mercaptan.
[0012] Preferably, the substrate is a glass substrate, a silicon substrate, a metal substrate or a polymer material substrate.
[0013] Preferably, the metal nanoparticles are selected from one or more of gold nanoparticles, silver nanoparticles and copper nanoparticles.
[0014] A second aspect of the present invention provides a method for preparing a composite SERS substrate based on titanium dioxide and metal nanoparticles, the method comprising the following steps:
[0015] (1) immersing the substrate in a polystyrene microsphere solution and then drying it;
[0016] (2) spin coating a solution containing a titanium dioxide precursor onto the substrate obtained in step (1), and then drying and calcining the solution to obtain a substrate loaded with a titanium dioxide three-dimensional inverse opal structure;
[0017] (3) immersing the substrate obtained in step (2) in a metal nanoparticle solution and then drying it;
[0018] (4) placing the substrate obtained in step (3) in a thiol solution for immersion, taking it out, washing it and drying it;
[0019] Wherein, the size of the metal nanoparticles is 30-300nm;
[0020] The thickness of the titanium dioxide three-dimensional inverse opal structure is ≥3000nm.
[0021] Preferably, in step (1), the diameter of the polystyrene microspheres is 200-1000 nm;
[0022] Preferably, the concentration of polystyrene microspheres in the polystyrene microsphere solution is 10-40 wt %;
[0023] Preferably, the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the coating surface to be spin-coated is 1-8 g / cm 2 .
[0024] Preferably, in step (1), the drying conditions include: temperature of 30-80° C. and time of 2-8 h.
[0025] In step (2), the ratio of the weight of titanium element in the solution containing titanium dioxide precursor to the area of the spin-coated coating surface is 0.2-2 mg / cm 2 ;
[0026] Preferably, the titanium dioxide precursor is selected from one or more of di(2-hydroxypropionic acid)diammonium titanium dihydroxide, tetrabutyl titanate, isopropyl titanate and titanyl sulfate.
[0027] Preferably, in step (2), the spin coating conditions include: a rotation speed of 600-6000 r / min and a time of 1-10 min.
[0028] Preferably, in step (2), the drying conditions include: temperature of 40-120° C. and time of 0.2-5 h.
[0029] Preferably, in step (2), the calcination conditions include: temperature of 300-600° C. and time of 2-8 h.
[0030] Preferably, in step (3), the concentration of the metal nanoparticles in the metal nanoparticle solution is 0.1-2.5 mg / L;
[0031] Preferably, the ratio of the weight of the metal nanoparticles in the metal nanoparticle solution to the area of the spin-coated coating surface is 0.1-1.0 mg / cm 2 ;
[0032] Preferably, the metal nanoparticles are selected from one or more of gold nanoparticles, silver nanoparticles and copper nanoparticles.
[0033] Preferably, in step (3), the drying conditions include: a temperature of 50-100° C. and a time of 1-10 h.
[0034] Preferably, in step (4), the mercaptan is selected from one or more of n-propyl mercaptan, n-hexyl mercaptan and n-dodecyl mercaptan;
[0035] Preferably, the concentration of mercaptan in the mercaptan solution is 10 -1 -10 -4 mol / L.
[0036] Preferably, in step (4), the soaking time is 10-45 min.
[0037] The third aspect of the present invention provides a composite SERS substrate based on titanium dioxide and metal nanoparticles prepared by the method described above.
[0038] A fourth aspect of the present invention provides the use of the composite SERS substrate based on titanium dioxide and metal nanoparticles as described above in the detection of polycyclic aromatic hydrocarbons.
[0039] Preferably, the polycyclic aromatic hydrocarbons are selected from at least one of naphthalene, anthracene, phenanthrene, pyrene and benzopyrene;
[0040] Preferably, the detection concentration of polycyclic aromatic hydrocarbons by the composite SERS substrate based on titanium dioxide and metal nanoparticles is ≥10 -8 mol / L.
[0041] A fifth aspect of the present invention provides a method for detecting the concentration of polycyclic aromatic hydrocarbons in a solution, wherein the solution to be tested is dripped onto the composite SERS substrate based on titanium dioxide and metal nanoparticles as described above, and SERS detection is performed using a Raman spectrometer.
[0042] Compared with the prior art, the SERS substrate and method described in the present invention have the following advantages:
[0043] 1. The composite SERS substrate of the present invention has a titanium dioxide three-dimensional inverse opal structure and metal nanoparticles, which can increase the coupling effect between the incident light and the SERS substrate, increase the density and intensity of the electromagnetic field enhancement area, and effectively improve the detection capability of the SERS substrate.
[0044] 2. The composite SERS substrate of the present invention contains thiol molecules, which can specifically adsorb polycyclic aromatic hydrocarbons in water through hydrophobic interaction, and can effectively improve the adsorption efficiency of target molecules, thereby improving the signal amplification capability of the SERS substrate.
[0045] 3. The present invention prepares the substrate by means of solution volatilization self-assembly, which does not involve expensive precision instruments and is simple, fast, practical and economical, thus facilitating further promotion and application.
[0046] 4. The SERS substrate of the present invention can be applied to surface enhanced Raman detection, analytical chemistry and environmental detection. It can realize the qualitative and quantitative detection of trace substances in liquid environment, and is particularly suitable for the trace detection of polycyclic aromatic hydrocarbons in the environment or molecules with benzene rings or hydrophobicity that are difficult to be directly adsorbed by the substrate. It has a good application prospect for the detection of industrial wastewater, river and lake water, and domestic sewage. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 is a schematic diagram of a composite SERS substrate based on titanium dioxide and metal nanoparticles in a specific embodiment of the present invention;
[0048] Figure 2 is a scanning electron microscope image of the product obtained in step (2) of Example 1;
[0049] Figure 3 is a scanning electron microscope image of the composite SERS substrate prepared in Example 1;
[0050] Figure 4 It is the Raman signal diagram of different concentrations of phenanthrene on the composite SERS substrate;
[0051] Figure 5 is a graph showing the relationship between the concentration of phenanthrene and the Raman signal intensity in Test Example 2.
[0052] Description of Reference Numerals
[0053] 1 Substrate; 2 Titanium dioxide three-dimensional inverse opal structure; 3 Metal nanoparticles. DETAILED DESCRIPTION
[0054] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0055] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0056] The first aspect of the present invention discloses a composite SERS substrate based on titanium dioxide and metal nanoparticles, comprising:
[0057] A substrate, a titanium dioxide three-dimensional inverse opal structure supported on the substrate, metal nanoparticles supported on the surface of the titanium dioxide three-dimensional inverse opal structure, and thiol modified on the metal nanoparticles;
[0058] The size of the metal nanoparticles is 30-300 nm;
[0059] The thickness of the titanium dioxide three-dimensional inverse opal structure is ≥3000 nm.
[0060] In a preferred embodiment, the pore size of the titanium dioxide three-dimensional inverse opal structure is 200-1000 nm, more preferably 400-800 nm.
[0061] In a preferred embodiment, the thickness of the titanium dioxide three-dimensional inverse opal structure is ≥4000 nm.
[0062] In a preferred embodiment, the thiol is selected from one or more of n-propyl mercaptan, n-hexyl mercaptan and n-dodecyl mercaptan.
[0063] In a preferred embodiment, the substrate is a glass substrate, a silicon substrate, a metal substrate or a polymer material substrate.
[0064] Further preferably, the polymer material may be polymethyl methacrylate (PMMA) or polyethylene terephthalate (PET).
[0065] In a preferred embodiment, the metal nanoparticles are selected from one or more of gold nanoparticles, silver nanoparticles and copper nanoparticles.
[0066] In a specific embodiment, the metal nanoparticles may be gold nanospheres, gold nanorods or gold nanocubes, and the silver nanoparticles may be silver nanospheres or silver nanotriangles.
[0067] In the composite SERS substrate based on titanium dioxide and metal nanoparticles described in the present invention, the three-dimensional inverse opal structure of titanium dioxide and the metal nanoparticles can increase the coupling effect between the incident light and the SERS substrate, increase the density and intensity of the electromagnetic field enhancement area, and the thiol molecules modified on the gold nanoparticles can promote the adsorption of the substance to be tested. Therefore, the synergistic effect of titanium dioxide, gold nanoparticles and thiol molecules based on the three-dimensional inverse opal structure improves the detection ability of the SERS substrate.
[0068] According to a specific implementation of the present invention, Figure 1 (Cross-sectional view), the composite SERS substrate based on titanium dioxide and metal nanoparticles comprises: a substrate 1, a titanium dioxide three-dimensional inverse opal structure 2 supported on the substrate 1, metal nanoparticles 3 supported on the surface of the titanium dioxide three-dimensional inverse opal structure 2, and thiol modified on the metal nanoparticles 3 (not shown in the figure);
[0069] The size of the metal nanoparticles 3 is 30-300 nm;
[0070] The thickness (h) of the titanium dioxide three-dimensional inverse opal structure 2 is ≥3000 nm;
[0071] The pore size (d) of the titanium dioxide three-dimensional inverse opal structure 2 is 200-1000 nm.
[0072] The second aspect of the present invention discloses a method for preparing a composite SERS substrate based on titanium dioxide and metal nanoparticles, the method comprising the following steps:
[0073] (1) immersing the substrate in a polystyrene microsphere solution and then drying it;
[0074] (2) spin coating a solution containing a titanium dioxide precursor onto the substrate obtained after drying in step (1), and then drying and calcining to obtain a substrate loaded with a titanium dioxide three-dimensional inverse opal structure;
[0075] (3) immersing the substrate obtained in step (2) in a metal nanoparticle solution and then drying it;
[0076] (4) soaking the material obtained in step (3) in a thiol solution, taking it out, washing it and drying it;
[0077] Wherein, the size of the metal nanoparticles is 30-300nm;
[0078] The thickness of the titanium dioxide three-dimensional inverse opal structure is ≥3000nm.
[0079] In the method of the present invention, in step (1), the substrate is immersed in a solution containing polystyrene microspheres and then dried. As the solvent evaporates, the polystyrene microspheres are orderly arranged on the surface of the substrate. Based on this, the polystyrene three-dimensional photonic crystal microspheres are densely stacked on the substrate through the solution evaporation self-assembly method.
[0080] In a specific embodiment, the content of polystyrene microspheres in the polystyrene microsphere solution may be 10 weight %, 15 weight %, 20 weight %, 25 weight %, 30 weight %, 35 weight % or 40 weight %.
[0081] In a specific embodiment, the polystyrene microsphere solution can be a polystyrene microsphere suspension, and the solvent used is water.
[0082] In a preferred embodiment, the size of the metal nanoparticles is 40-100 nm.
[0083] In a preferred embodiment, in step (1), the diameter of the polystyrene microspheres is 200-1000 nm, more preferably 400-800 nm; specifically, it can be 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm or 1000 nm.
[0084] In a specific embodiment, the polystyrene microspheres can be made in the laboratory or purchased commercially.
[0085] In a specific embodiment, in order to mix uniformly, the polystyrene microsphere solution may be subjected to ultrasonic treatment before the substrate is immersed in the polystyrene microsphere solution, and the ultrasonic treatment time is 5-20 minutes.
[0086] In step (1), there is no special requirement for the drying conditions, as long as the polystyrene three-dimensional photonic crystal microspheres are densely stacked on the substrate after the solvent evaporates. In a preferred embodiment, in step (1), the drying conditions include: a temperature of 30-80°C and a time of 2-8h. Specifically, the drying temperature can be 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C; the drying time can be 2h, 3h, 4h, 5h, 6h, 7h, or 8h.
[0087] In the method of the present invention, in step (2), a solution containing a titanium dioxide precursor is spin-coated onto the substrate loaded with polystyrene three-dimensional photonic crystal microspheres obtained in step (1), and the titanium dioxide precursor solution penetrates into the gaps between the polystyrene three-dimensional photonic crystal microspheres. Then, the solution is dried and calcined to remove water and the polystyrene template, thereby obtaining a substrate loaded with a titanium dioxide three-dimensional inverse opal structure, wherein the pore size of the titanium dioxide three-dimensional inverse opal structure is comparable to the diameter of the polystyrene microspheres.
[0088] In the method described in the present invention, the thickness of the titanium dioxide three-dimensional inverse opal structure is controlled to be ≥3000nm. If the thickness of the titanium dioxide three-dimensional inverse opal structure is smaller, the coupling efficiency between the incident light and the structure will be reduced, and the enhancement effect will be weakened.
[0089] In the method of the present invention, the spin-coated coating surface is the surface on the substrate corresponding to the surface when the solution containing the titanium dioxide precursor is spin-coated, that is, the surface on the substrate loaded with the titanium dioxide three-dimensional inverse opal structure.
[0090] In the method of the present invention, in order to further improve the detection capability of the composite SERS substrate, in a preferred embodiment, the amount of polystyrene microspheres can be reasonably controlled, and the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the spin-coated coating surface is 1-8 g / cm 2 .
[0091] In a specific embodiment, the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the spin-coated coating surface can be 1 g / cm 2 , 2g / cm 2 , 3g / cm 2 , 4g / cm 2 , 5g / cm 2 , 6g / cm 2 , 7g / cm 2 or 8g / cm 2 .
[0092] In the method of the present invention, in order to further improve the detection capability of the composite SERS substrate, in a preferred embodiment, the amount of the titanium dioxide precursor can be reasonably controlled, and the ratio of the weight of the titanium element in the solution containing the titanium dioxide precursor to the area of the spin-coated coating surface is 0.2-2 mg / cm 2 ; Specifically, it can be 0.2mg / cm 2 , 0.3mg / cm 2 , 0.4mg / cm 2 , 0.5mg / cm 2 , 0.6mg / cm 2 , 0.7mg / cm 2 , 0.8mg / cm 2 , 0.9mg / cm 2 , 1mg / cm 2 , 1.2mg / cm 2 , 1.4mg / cm 2 , 1.5mg / cm 2 、1.6mg / cm 2 、1.8mg / cm 2 or 2mg / cm 2 .
[0093] In a preferred embodiment, the titanium dioxide precursor is selected from one or more of di(2-hydroxypropionic acid)diammonium titanium dihydroxide, tetrabutyl titanate, isopropyl titanate and titanyl sulfate.
[0094] In a preferred embodiment, the solution containing the titanium dioxide precursor mainly serves to provide a titanium dioxide precursor that can generate titanium dioxide, and can be prepared in a conventional manner in the art.
[0095] In a specific embodiment, the solution containing titanium dioxide precursor can be prepared according to the following method:
[0096] Mix di(2-hydroxypropionic acid) diammonium dihydroxide titanium, water and ammonia water, and stir at a speed of 200-2000 r / min for 20-90 min;
[0097] The volume ratio of di(2-hydroxypropionic acid) diammonium dihydroxide titanium, water and ammonia water is 0.02-1:1:0.2-1, and the concentration of ammonia water is 25-28%.
[0098] In a preferred embodiment, in step (2), the spin coating conditions include: a rotation speed of 600-6000 r / min and a time of 1-10 min. Specifically, the spin coating speed may be 600 r / min, 1000 r / min, 2000 r / min, 3000 r / min, 4000 r / min, 5000 r / min or 6000 r / min; and the spin coating time may be 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min.
[0099] In the method of the present invention, in step (2), the drying process can be preliminary dehydration and decomposition. In a preferred embodiment, the drying conditions include: a temperature of 40-120°C and a time of 0.2-5h. Specifically, the drying temperature can be 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C; the drying time can be 0.2h, 0.5h, 1h, 2h, 3h, 4h or 5h.
[0100] In the method of the present invention, in step (2), the calcination process can further dehydrate and decompose and crack the polystyrene template to obtain titanium dioxide with a three-dimensional inverse opal structure. In a preferred embodiment, the calcination conditions include: a temperature of 300-600°C and a time of 2-8h. Specifically, the calcination temperature can be 300°C, 350°C, 400°C, 450°C, 500°C, 550°C or 600°C.
[0101] In the method described in the present invention, in step (3), the substrate loaded with the titanium dioxide three-dimensional inverse opal structure obtained in step (2) is immersed in a metal nanoparticle solution and then dried, so that the metal nanoparticles are loaded on the nanopore surface of the titanium dioxide three-dimensional inverse opal structure.
[0102] In a preferred embodiment, the metal nanoparticle solution may be a metal nanoparticle aqueous solution, which may be a commercially available metal nanoparticle aqueous solution or may be homemade in a laboratory.
[0103] In a preferred embodiment, the metal nanoparticles are selected from one or more of gold nanoparticles, silver nanoparticles and copper nanoparticles.
[0104] For example, the gold nanoparticles may be gold nanospheres, gold nanorods or gold nanocubes, and the silver nanoparticles may be silver nanospheres or silver nanotriangles.
[0105] In a preferred embodiment, in step (3), the concentration of the metal nanoparticles in the metal nanoparticle solution is 0.1-2.5 mg / mL. Specifically, the concentration of the metal nanoparticles can be 0.1 mg / mL, 0.3 mg / mL, 0.5 mg / mL, 0.8 mg / mL, 1 mg / mL, 1.2 mg / mL, 1.5 mg / mL, 1.8 mg / mL, 2 mg / mL or 2.5 mg / mL.
[0106] In the method of the present invention, in order to further improve the detection capability of the SERS substrate, in a preferred embodiment, the ratio of the weight of the metal nanoparticles in the metal nanoparticle solution to the area of the spin-coated coating surface is 0.1-1 mg / cm 2 ; Specifically, it can be 0.1mg / cm 2 , 0.2mg / cm 2 , 0.3mg / cm 2 , 0.4mg / cm 2 , 0.5mg / cm 2 , 0.6mg / cm 2 , 0.7mg / cm 2 , 0.8mg / cm 2 , 0.9mg / cm 2 or 1.0mg / cm 2 .
[0107] In a specific embodiment, the metal nanoparticle solution may be a gold nanosphere aqueous solution.
[0108] In a preferred embodiment, the method for preparing the gold nanosphere aqueous solution comprises the following steps: mixing a chloroauric acid solution and a sodium citrate solution, then reacting, and then washing;
[0109] Wherein, the molar ratio of chloroauric acid to sodium citrate is 1:0.3-5; the reaction temperature is 110-150°C, and the reaction time is 2-15h.
[0110] In the method of the present invention, in order to further improve the detection capability of the SERS substrate, the sizes of the metal nanoparticles and the polystyrene microspheres can be reasonably controlled. In a preferred embodiment, the ratio of the size of the metal nanoparticles to the diameter of the polystyrene microspheres is 1:5-20. Specifically, it can be 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19 and 1:20.
[0111] In a preferred embodiment, in step (3), the drying conditions include: a temperature of 50-100°C and a time of 1-10 hours. Specifically, the drying temperature may be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C; and the drying time may be 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.
[0112] In the method of the present invention, in step (4), the substrate obtained in step (3) is immersed in a thiol solution, taken out, washed and dried, and thiol can be modified onto the metal nanoparticles.
[0113] In a preferred embodiment, in step (4), the mercaptan is selected from one or more of n-propyl mercaptan, n-hexyl mercaptan and n-dodecyl mercaptan;
[0114] In a preferred embodiment, the concentration of mercaptan in the mercaptan solution is 10 -1 -10 -4 mol / L. Specifically, the thiol concentration can be 10 -1 mol / L, 0.05mol / L, 10 -2 mol / L、10 -3 mol / L or 10 -4 mol / LmL.
[0115] In a specific embodiment, the solvent used in the thiol solution is ethanol.
[0116] In order to further improve the detection capability of the SERS substrate and the ability to capture the sample to be tested, in a preferred embodiment, in step (4), the immersion time is 10-45 minutes. Specifically, it can be 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes or 45 minutes.
[0117] In a preferred embodiment, in step (4), the washing method is water washing to remove free thiol molecules.
[0118] In a preferred embodiment, in step (4), there are no special requirements for the drying conditions, and the drying can be carried out in a conventional manner in the art.
[0119] In a preferred embodiment, the substrate is a glass substrate (eg, a glass sheet), a silicon substrate, a metal substrate, or a polymer material substrate.
[0120] Further preferably, the polymer material may be polymethyl methacrylate (PMMA) or polyethylene terephthalate (PET).
[0121] The method of the present invention uses a solution volatilization self-assembly method to obtain polystyrene three-dimensional photonic crystal microspheres densely packed on the substrate surface, and then uses the polystyrene three-dimensional photonic crystal microspheres as a template to load the substrate surface with a titanium dioxide three-dimensional inverse opal structure, and then loads metal nanoparticles on the titanium dioxide surface, and then uses thiol to modify the metal nanoparticles. Based on this, a composite SERS substrate capable of achieving qualitative and quantitative detection of polycyclic aromatic hydrocarbons is prepared.
[0122] The third aspect of the present invention provides a composite SERS substrate based on titanium dioxide and metal nanoparticles prepared by the method described above.
[0123] A fourth aspect of the present invention provides the use of the composite SERS substrate based on titanium dioxide and metal nanoparticles as described above in the detection of polycyclic aromatic hydrocarbons.
[0124] Preferably, the polycyclic aromatic hydrocarbons are selected from at least one of naphthalene, anthracene, phenanthrene, pyrene and benzopyrene;
[0125] Preferably, the detection concentration of polycyclic aromatic hydrocarbons by the composite SERS substrate based on titanium dioxide and metal nanoparticles is ≥10 -8 mol / L.
[0126] The fifth aspect of the present invention discloses a method for detecting the concentration of polycyclic aromatic hydrocarbons in a solution, wherein the solution to be tested is dripped onto the composite SERS substrate based on titanium dioxide and metal nanoparticles as described above, and SERS detection is performed using a Raman spectrometer.
[0127] The composite SERS substrate based on titanium dioxide and metal nanoparticles of the present invention has the advantages of high coupling efficiency with incident light and strong adsorption capacity for target molecules, and can be applied to the qualitative and quantitative detection of polycyclic aromatic hydrocarbons.
[0128] In a specific embodiment, the polycyclic aromatic hydrocarbons can be quantitatively detected, including the following steps:
[0129] (1) dropping a PAH standard solution onto a composite SERS substrate based on titanium dioxide and metal nanoparticles, drying it, and then performing SERS detection using a Raman spectrometer to record the peak intensity after the solvent evaporates;
[0130] (2) Using the logarithm of the concentration as the abscissa and the peak intensity as the ordinate, fitting is performed to obtain the relationship between the concentration and the peak intensity;
[0131] (3) The test solution is added dropwise onto the SERS substrate, and after the solvent is evaporated, SERS detection is performed using a Raman spectrometer, the peak intensity is recorded, and then the peak intensity is substituted into the relationship for calculation to obtain the concentration of polycyclic aromatic hydrocarbons in the test solution.
[0132] The SERS substrate and the preparation method thereof of the present invention are further described below by way of examples. The examples are implemented based on the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following examples.
[0133] Example 1
[0134] The composite SERS substrate S1 based on titanium dioxide and metal nanoparticles was prepared. The specific process is as follows:
[0135] (1) providing a glass sheet as a glass substrate;
[0136] A polystyrene microsphere (diameter 700nm) suspension (polystyrene content 20 wt%) was ultrasonically treated for 15 minutes, fully mixed, and placed in a beaker. A glass substrate was then vertically inserted and immersed in the polystyrene microsphere suspension, and then placed in a 40°C oven for drying for 6 hours. After the solution evaporated completely, polystyrene three-dimensional photonic crystal microspheres were densely stacked on the glass substrate; wherein the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the spin-coated coating surface was 4 g / cm 2 ;
[0137] (2) A solution containing a titanium dioxide precursor (di(2-hydroxypropionic acid) diammonium dihydroxide titanium) was added dropwise onto the substrate obtained in step (1), and the ratio of the weight of the titanium element in the solution containing the titanium dioxide precursor to the area of the spin-coated coating surface was controlled to be 1.2 mg / cm 2 , spin coating at 1500r / min for 2min, then drying in an oven at 80°C for 3h, taking it out and baking it in a muffle furnace at 450°C for 6h, to obtain a glass substrate loaded with a titanium dioxide three-dimensional inverse opal structure, the pore size of the titanium dioxide three-dimensional inverse opal structure is 700nm, and the thickness of the titanium dioxide three-dimensional inverse opal structure is 4900nm;
[0138] (3) The glass substrate loaded with the titanium dioxide three-dimensional inverse opal structure obtained in step (2) was immersed in a solution of gold nanospheres (with a diameter of 45 nm) with a concentration of 1.5 mg / mL, and the ratio of the weight of the gold nanospheres in the gold nanosphere solution to the area of the spin-coated coating surface was controlled to be 0.4 mg / cm 2 , and then put it into an oven at 70°C for 4 hours for drying. After the solvent evaporates completely, the gold nanospheres are loaded on the three-dimensional inverse opal structure of titanium dioxide;
[0139] (4) placing the substrate obtained in step (3) in an ethanol solution of thiol (n-propyl mercaptan) (the concentration of n-propyl mercaptan is 10 - 2 mol / L) for 30 min, then washed and dried;
[0140] The solution containing the titanium dioxide precursor is prepared according to the following steps: di(2-hydroxypropionic acid) diammonium dihydroxide titanium, water and concentrated ammonia water (concentration of 25-28%) are mixed in a volume ratio of 0.4:1:0.4, and then stirred at a speed of 1000 r / min for 50 minutes;
[0141] The gold nanosphere solution was prepared according to the following steps: 350 μL of 0.5 mol / L chloroauric acid solution was added to 1200 ml of deionized water, and when heated to 130°C at a speed of 900 r / min, 4 mL of 0.06 mol / L sodium citrate solution was added and maintained for 3 h; after the reaction was completed, the solution was washed three times at a speed of 8000 r / min for 15 min to remove excess sodium citrate, thereby obtaining a gold nanosphere solution with a concentration of 1.5 mg / mL and a diameter of 45 nm.
[0142] Example 2
[0143] The composite SERS substrate S2 based on titanium dioxide and metal nanoparticles was prepared. The specific process is as follows:
[0144] (1) providing a glass sheet as a glass substrate;
[0145] A polystyrene microsphere (diameter 700nm) suspension (polystyrene content 15 wt%) was ultrasonically treated for 15 minutes, fully mixed, and placed in a beaker. A glass substrate was then vertically inserted and immersed in the polystyrene microsphere suspension, and then placed in a 40°C oven for drying for 6 hours. After the solution evaporated completely, polystyrene three-dimensional photonic crystal microspheres were densely stacked on the glass substrate; wherein the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the spin-coated coating surface was 3 g / cm 2 ;
[0146] (2) A solution containing a titanium dioxide precursor (di(2-hydroxypropionic acid) diammonium dihydroxide titanium) was added dropwise onto the substrate obtained in step (1), and the ratio of the weight of the titanium element in the solution containing the titanium dioxide precursor to the area of the spin-coated coating surface was controlled to be 0.9 mg / cm 2 , spin coating at 1500r / min for 2min, then drying in an oven at 80°C for 3h, taking it out and baking it in a muffle furnace at 450°C for 6h, to obtain a glass substrate loaded with a titanium dioxide three-dimensional inverse opal structure, the pore size of the titanium dioxide three-dimensional inverse opal structure is 700nm, and the thickness of the titanium dioxide three-dimensional inverse opal structure is 4200nm;
[0147] (3) The glass substrate loaded with the titanium dioxide three-dimensional inverse opal structure obtained in step (2) was immersed in a solution of gold nanospheres (with a diameter of 45 nm) with a concentration of 1.5 mg / mL, and the ratio of the weight of the gold nanospheres in the gold nanosphere solution to the area of the spin-coated coating surface was controlled to be 0.3 mg / cm 2 , and then put it into an oven at 70°C for 4 hours for drying. After the solvent evaporates completely, the gold nanospheres are loaded on the three-dimensional inverse opal structure of titanium dioxide;
[0148] (4) placing the substrate obtained in step (3) in an ethanol solution of thiol (n-propyl mercaptan) (the concentration of n-propyl mercaptan is 10 - 2 mol / L) for 30 min, then washed and dried;
[0149] Wherein, the preparation method of the solution containing titanium dioxide precursor is the same as that in Example 1;
[0150] The preparation method of the gold nanosphere solution is the same as that in Example 1.
[0151] Example 3
[0152] The composite SERS substrate S3 based on titanium dioxide and metal nanoparticles was prepared. The specific process is as follows:
[0153] (1) providing a glass sheet as a glass substrate;
[0154] A polystyrene microsphere (diameter 700nm) suspension (polystyrene content 30 wt%) was ultrasonically treated for 15 minutes, fully mixed, and placed in a beaker. A glass substrate was then vertically inserted and immersed in the polystyrene microsphere suspension, and then placed in a 40°C oven for drying for 6 hours. After the solution evaporated completely, polystyrene three-dimensional photonic crystal microspheres were densely stacked on the glass substrate; wherein the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the spin-coated coating surface was 6 g / cm 2 ;
[0155] (2) A solution containing a titanium dioxide precursor (di(2-hydroxypropionic acid) diammonium dihydroxide titanium) was added dropwise onto the substrate obtained in step (1), and the ratio of the weight of the titanium element in the solution containing the titanium dioxide precursor to the area of the spin-coated coating surface was controlled to be 1.8 g / cm 2 , spin-coated at 1500r / min for 2min, then placed in an oven and dried at 80°C for 3h, taken out and placed in a muffle furnace for calcination at 450°C for 6h, to obtain a glass substrate loaded with a titanium dioxide three-dimensional inverse opal structure, the pore size of the titanium dioxide three-dimensional inverse opal structure is 700nm, and the thickness of the titanium dioxide three-dimensional inverse opal structure is 6300nm; wherein:
[0156] (3) The glass substrate loaded with the titanium dioxide three-dimensional inverse opal structure obtained in step (2) was immersed in a solution of gold nanospheres (with a diameter of 45 nm) with a concentration of 1.5 mg / mL, and the ratio of the weight of the gold nanospheres in the gold nanosphere solution to the area of the spin-coated coating surface was controlled to be 0.6 mg / cm 2 , and then put it into an oven at 70°C for 4 hours for drying. After the solvent evaporates completely, the gold nanospheres are loaded on the three-dimensional inverse opal structure of titanium dioxide;
[0157] (4) placing the substrate obtained in step (3) in an ethanol solution of thiol (n-propyl mercaptan) (the concentration of n-propyl mercaptan is 10 - 2 mol / L) for 30 min, then washed and dried;
[0158] Wherein, the preparation method of the solution containing titanium dioxide precursor is the same as that in Example 1;
[0159] The preparation method of the gold nanosphere solution is the same as that in Example 1.
[0160] Example 4
[0161] The composite SERS substrate S4 based on titanium dioxide and metal nanoparticles was prepared. The specific process is as follows:
[0162] (1) providing a glass sheet as a glass substrate;
[0163] A polystyrene microsphere (diameter 700nm) suspension (polystyrene content 20 wt%) was ultrasonically treated for 15 minutes, fully mixed, and placed in a beaker. A glass substrate was then vertically inserted and immersed in the polystyrene microsphere suspension, and then placed in a 40°C oven for drying for 6 hours. After the solution evaporated completely, polystyrene three-dimensional photonic crystal microspheres were densely stacked on the glass substrate; wherein the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the spin-coated coating surface was 4 g / cm 2 ;
[0164] (2) A solution containing a titanium dioxide precursor (di(2-hydroxypropionic acid) diammonium dihydroxide titanium) was added dropwise onto the substrate obtained in step (1), and the ratio of the weight of the titanium element in the solution containing the titanium dioxide precursor to the area of the spin-coated coating surface was controlled to be 1.2 g / cm 2 , spin coating at 1500r / min for 2min, then drying in an oven at 80°C for 3h, taking it out and baking it in a muffle furnace at 450°C for 6h, to obtain a glass substrate loaded with a titanium dioxide three-dimensional inverse opal structure, the pore size of the titanium dioxide three-dimensional inverse opal structure is 700nm, and the thickness of the titanium dioxide three-dimensional inverse opal structure is 4900nm;
[0165] (3) The glass substrate loaded with the titanium dioxide three-dimensional inverse opal structure obtained in step (2) was immersed in a solution of gold nanospheres (with a diameter of 35 nm) with a concentration of 1 mg / mL, and the ratio of the weight of the gold nanospheres in the gold nanosphere solution to the area of the spin-coated coating surface was controlled to be 0.3 mg / cm 2 , and then put it into an oven at 70°C for 4 hours for drying. After the solvent evaporates completely, the gold nanospheres are loaded on the three-dimensional inverse opal structure of titanium dioxide;
[0166] (4) placing the substrate obtained in step (3) in an ethanol solution of thiol (n-propyl mercaptan) (the concentration of n-propyl mercaptan is 10 - 2 mol / L) for 30 min, then washed and dried;
[0167] Wherein, the preparation method of the solution containing titanium dioxide precursor is the same as that in Example 1;
[0168] The gold nanosphere solution was prepared according to the following steps: 350 μL of 0.3 mol / L chloroauric acid solution was added to 1200 ml of deionized water, and when heated to 130°C at a speed of 900 r / min, 4 mL of 0.06 mol / L sodium citrate solution was added and maintained for 3 h; after the reaction was completed, the solution was washed three times at a speed of 8000 r / min for 15 min to remove excess sodium citrate, thereby obtaining a gold nanosphere solution with a concentration of 1.0 mg / mL and a diameter of 35 nm.
[0169] Example 5
[0170] The composite SERS substrate S5 based on titanium dioxide and metal nanoparticles was prepared. The specific process is as follows:
[0171] (1) providing a glass sheet as a glass substrate;
[0172] A polystyrene microsphere (diameter 700nm) suspension (polystyrene content 20 wt%) was ultrasonically treated for 15 minutes, fully mixed, and placed in a beaker. A glass substrate was then vertically inserted and immersed in the polystyrene microsphere suspension, and then placed in a 40°C oven for drying for 6 hours. After the solution evaporated completely, polystyrene three-dimensional photonic crystal microspheres were densely stacked on the glass substrate; wherein the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the spin-coated coating surface was 4 g / cm 2 ;
[0173] (2) A solution containing a titanium dioxide precursor (di(2-hydroxypropionic acid) diammonium dihydroxide titanium) was added dropwise onto the substrate obtained in step (1), and the ratio of the weight of the titanium element in the solution containing the titanium dioxide precursor to the area of the spin-coated coating surface was controlled to be 1.2 g / cm 2 , spin coating at 1500r / min for 2min, then drying in an oven at 80°C for 3h, taking it out and baking it in a muffle furnace at 450°C for 6h, to obtain a glass substrate loaded with a titanium dioxide three-dimensional inverse opal structure, the pore size of the titanium dioxide three-dimensional inverse opal structure is 700nm, and the thickness of the titanium dioxide three-dimensional inverse opal structure is 4900nm;
[0174] (3) The glass substrate loaded with the titanium dioxide three-dimensional inverse opal structure obtained in step (2) was immersed in a solution of gold nanospheres (diameter 60 nm) with a concentration of 2.1 mg / mL, and the ratio of the weight of the gold nanospheres in the gold nanosphere solution to the area of the spin-coated coating surface was controlled to be 0.45 mg / cm 2 , and then put it into an oven at 70°C for 4 hours for drying. After the solvent evaporates completely, the gold nanospheres are loaded on the three-dimensional inverse opal structure of titanium dioxide;
[0175] (4) placing the substrate obtained in step (3) in an ethanol solution of thiol (n-propyl mercaptan) (the concentration of n-propyl mercaptan is 10 - 2 mol / L) for 30 min, then washed and dried;
[0176] Wherein, the preparation method of the solution containing titanium dioxide precursor is the same as that in Example 1;
[0177] The gold nanosphere solution was prepared according to the following steps: 350 μL of 0.8 mol / L chloroauric acid solution was added to 1200 ml of deionized water, and when heated to 130°C at a speed of 900 r / min, 4 mL of 0.06 mol / L sodium citrate solution was added and maintained for 3 h; after the reaction was completed, the solution was washed three times at a speed of 8000 r / min for 15 min to remove excess sodium citrate, thereby obtaining a gold nanosphere solution with a concentration of 2.1 mg / mL and a diameter of 60 nm.
[0178] Example 6
[0179] The method described in Example 1 is used, except that in step (4), the thiol used is n-hexylthiol, to obtain a composite SERS substrate S6 based on titanium dioxide and metal nanoparticles.
[0180] Example 7
[0181] The method described in Example 1 is used, except that in step (4), the thiol used is n-hexadecene mercaptan, to obtain a composite SERS substrate S7 based on titanium dioxide and metal nanoparticles.
[0182] Example 8
[0183] The composite SERS substrate S8 based on titanium dioxide and metal nanoparticles was prepared. The specific process is as follows:
[0184] (1) providing a glass sheet as a glass substrate;
[0185] A polystyrene microsphere (diameter 800nm) suspension (polystyrene content 20 wt%) was ultrasonically treated for 15 minutes, fully mixed, and placed in a beaker. A glass substrate was then vertically inserted and immersed in the polystyrene microsphere suspension, and then placed in a 40°C oven for drying for 6 hours. After the solution evaporated completely, polystyrene three-dimensional photonic crystal microspheres were densely stacked on the glass substrate; wherein the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the spin-coated coating surface was 5 g / cm 2 ;
[0186] (2) A solution containing a titanium dioxide precursor (di(2-hydroxypropionic acid) diammonium dihydroxide titanium) was added dropwise onto the substrate obtained in step (1), and the ratio of the weight of the titanium element in the solution containing the titanium dioxide precursor to the area of the spin-coated coating surface was controlled to be 1.5 g / cm 2, spin coating at 1500r / min for 2min, then drying in an oven at 80°C for 3h, taking it out and baking it in a muffle furnace at 450°C for 6h, to obtain a glass substrate loaded with a titanium dioxide three-dimensional inverse opal structure, the pore size of the titanium dioxide three-dimensional inverse opal structure is 800nm, and the thickness of the titanium dioxide three-dimensional inverse opal structure is 5800nm;
[0187] (3) immersing the glass substrate loaded with the titanium dioxide three-dimensional inverse opal structure obtained in step (2) in a solution of silver nanospheres (diameter 45 nm) with a concentration of 1.5 mg / mL, and controlling the ratio of the weight of the silver nanospheres in the silver nanosphere solution to the area of the spin-coated coating surface to be 0.5 mg / cm 2 , and then put it into an oven at 70°C for 4 hours for drying. After the solvent evaporates completely, the silver nanospheres are loaded on the titanium dioxide three-dimensional inverse opal structure;
[0188] (4) placing the substrate obtained in step (3) in an ethanol solution of thiol (n-propyl mercaptan) (the concentration of n-propyl mercaptan is 10 - 2 mol / L) for 30 min, then washed and dried;
[0189] Wherein, the preparation method of the solution containing titanium dioxide precursor is the same as that in Example 1;
[0190] The silver nanosphere solution is obtained by treating a commercially available silver nanosphere solution.
[0191] Example 9
[0192] The composite SERS substrate S9 based on titanium dioxide and metal nanoparticles was prepared. The specific process is as follows:
[0193] (1) providing a glass sheet as a glass substrate;
[0194] A polystyrene microsphere (diameter 700nm) suspension (polystyrene content 20 wt%) was ultrasonically treated for 15 minutes, fully mixed, and placed in a beaker. A glass substrate was then vertically inserted and immersed in the polystyrene microsphere suspension, and then placed in a 40°C oven for drying for 6 hours. After the solution evaporated completely, polystyrene three-dimensional photonic crystal microspheres were densely stacked on the glass substrate; wherein the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the spin-coated coating surface was 4 g / cm 2 ;
[0195] (2) A solution containing a titanium dioxide precursor (di(2-hydroxypropionic acid) diammonium dihydroxide titanium) was added dropwise onto the substrate obtained in step (1), and the ratio of the weight of the titanium element in the solution containing the titanium dioxide precursor to the area of the spin-coated coating surface was controlled to be 1.3 g / cm2 , spin-coated at 1500r / min for 2min, then placed in an oven and dried at 80°C for 3h, taken out and placed in a muffle furnace for calcination at 450°C for 6h, to obtain a glass substrate loaded with a three-dimensional inverse opal structure of titanium dioxide, the pore size of the three-dimensional inverse opal structure of titanium dioxide is 700nm, and the thickness of titanium dioxide is 4900nm;
[0196] (3) immersing the glass substrate loaded with the titanium dioxide three-dimensional inverse opal structure obtained in step (2) in a metal nanoparticle solution, wherein the metal nanoparticles are gold nanospheres (with a diameter of 45 nm) and silver nanospheres (with a diameter of 45 nm), with concentrations of 1.0 mg / mL and 1.2 mg / mL, respectively, and controlling the ratio of the weight of the metal nanoparticles in the metal nanoparticle solution to the area of the spin-coated coating surface to be 0.8 mg / cm 2 , and then put it into an oven at 70°C for 4 hours for drying. After the solvent evaporates completely, the metal nanoparticles are loaded on the three-dimensional inverse opal structure of titanium dioxide;
[0197] (4) placing the substrate obtained in step (3) in an ethanol solution of thiol (n-propyl mercaptan) (the concentration of n-propyl mercaptan is 10 - 2 mol / L) for 30 min, and then washed and dried to obtain a composite SERS substrate S9;
[0198] Wherein, the preparation method of the solution containing titanium dioxide precursor is the same as that in Example 1;
[0199] The metal nanoparticles are obtained by treating a commercially available gold nanosphere solution and a silver nanosphere solution.
[0200] Example 10
[0201] The method described in Example 8 is used, except that in step (4), the thiol used is n-hexylthiol, to obtain a composite SERS substrate S10 based on titanium dioxide and metal nanoparticles.
[0202] Comparative Example 1
[0203] The method described in Example 1 is used for implementation, except that in step (1), the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the spin-coated coating surface is controlled to be 0.8 g / cm 2 The obtained titanium dioxide three-dimensional inverse opal structure has a pore size of 700nm and a thickness of 1400nm.
[0204] Comparative Example 2
[0205] The method described in Example 1 was used, except that in step (3), the diameter of the gold nanospheres used was 10 nm, and the ratio of the weight of the gold nanospheres in the gold nanosphere solution to the area of the spin-coated coating surface was controlled to be 0.09 mg / cm 2 .
[0206] Comparative Example 3
[0207] The method described in Example 1 is followed, except that step (4) is not performed.
[0208] Test Example 1
[0209] The product obtained in step (2) in Example 1 and the composite SERS substrate S1 were characterized by SEM. The results were as follows: Figure 2 and 3 shown.
[0210] As can be seen from the figure, the method described in the present invention can form a typical titanium dioxide three-dimensional inverse opal structure with uniform pore size; and the metal nanoparticles can be evenly distributed on the surface of the three-dimensional inverse opal structure.
[0211] Test Example 2
[0212] The performance of the products prepared in the examples and comparative examples was tested. The test process was as follows: 5 uL, 10 -4 mol / L phenanthrene ethanol solution was dripped onto the substrate to be tested. After the solvent evaporated, the substrate was tested using a Horiba Xplus microscope confocal Raman spectrometer. The laser wavelength was 785nm, the power was 10mW, the filter transmittance was 1%, the integration time was 20s, and the integration times were 2. -1 Taking the strength at as an example, the strength results are shown in Table 1.
[0213] Table 1
[0214] serial number strength serial number strength Example 1 5469 Example 7 5023 Example 2 5219 Example 8 5448 Example 3 5487 Example 9 5341 Example 4 5312 Example 10 5219 Example 5 5491 Comparative Example 1 4538 Example 6 5292 Comparative Example 2 4187 Comparative Example 3 4357
[0215] It can be seen from Table 1 that the composite SERS substrate based on titanium dioxide and metal nanoparticles of the present invention can be applied to surface enhanced Raman detection and has good signal amplification capability.
[0216] Test Example 3
[0217] The concentration of phenanthrene was set to 10 -8 mol / L、10 -7 mol / L、10 -6 mol / L、10 -5 mol / L、10 -4 mol / L、10- 3 mol / L and 10 -2 mol / L standard solution, the standard solution was dripped onto 7 composite SERS substrates prepared according to the method described in Example 1, and after the solvent was evaporated, SERS detection was performed using a Raman spectrometer. The corresponding Raman signal is shown in the figure below. Figure 4 As shown in the figure, it can be seen that the characteristic peaks of phenanthrene molecules are mainly 406cm -1 、545cm -1 、706cm -1 、1031cm -1 、1353cm -1 、1430cm -1 、1604cm -1 It can be seen from the intensity of the characteristic peak that as the concentration gradually decreases, the intensity of the characteristic peak also gradually decreases, indicating that the composite SERS substrate of the present invention can achieve a -8 Qualitative detection of phenanthrene molecules at mol / L.
[0218] Further, in order to achieve quantitative detection of phenanthrene, according to the attached Figure 4 For the data in, 706cm is selected -1 The intensity of the characteristic peak at is taken as the ordinate, and the logarithm of the concentration is taken as the abscissa. Figure 5 From the attached Figure 5 It can be seen that the intensity of the characteristic peak and the logarithm of the concentration show a good functional relationship, the characteristic peak intensity y = 170x 3 +3423x 2 +23204x+53949,R 2 = 0.996, x is the logarithm of the concentration. Based on this mathematical relationship, 706 cm -1 After measuring the intensity of the characteristic peak, the concentration of the solution can be calculated, thereby achieving quantitative detection of phenanthrene molecules.
[0219] The concentration of phenanthrene molecules was prepared to be 10 -3 mol / L、10 -4.5 mol / L、10 -5.8 mol / L aqueous solution was used as the test solution, and three composite SERS substrates prepared according to the method described in Example 1 were prepared. Then the above solution was dripped onto the composite SERS substrate. After the solvent evaporated, the Raman spectrum was tested and the 706 cm -1 The intensity of the characteristic peak at , is substituted into the relationship to calculate the concentration. The measured results are compared with the theoretical values of the test solution, and the results are shown in Table 2.
[0220] Table 2
[0221] Theoretical value Characteristic peak intensity Detection value error <![CDATA[10 -3 mol / L]]> 10338 <![CDATA[10 -3.03 mol / L]]> 6.70% <![CDATA[10 -4.5 mol / L]]> 3466 <![CDATA[10 -4.46 mol / L]]> 9.60% <![CDATA[10 -5.8 mol / L]]> 1364 <![CDATA[10 -5.77 mol / L]]> 7.20%
[0222] From the results in Table 2, it can be seen that the composite SERS substrate based on titanium dioxide and metal nanoparticles of the present invention can accurately detect the concentration of phenanthrene molecules.
[0223] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A composite SERS substrate based on titanium dioxide and metal nanoparticles, characterized in that: include: A substrate, a titanium dioxide three-dimensional inverse opal structure supported on the substrate, metal nanoparticles supported on the surface of the titanium dioxide three-dimensional inverse opal structure, and thiol modified on the metal nanoparticles; The size of the metal nanoparticles is 30-300 nm; The thickness of the titanium dioxide three-dimensional inverse opal structure is ≥3000 nm.
2. The composite SERS substrate based on titanium dioxide and metal nanoparticles according to claim 1, characterized in that: The pore size of the titanium dioxide three-dimensional inverse opal structure is 200-1000nm.
3. The composite SERS substrate based on titanium dioxide and metal nanoparticles according to claim 1 or 2, characterized in that: The mercaptan is selected from one or more of n-propyl mercaptan, n-hexyl mercaptan and n-dodecyl mercaptan.
4. The composite SERS substrate based on titanium dioxide and metal nanoparticles according to any one of claims 1 to 3, characterized in that: The substrate is a glass substrate, a silicon substrate, a metal substrate or a polymer material substrate.
5. The composite SERS substrate based on titanium dioxide and metal nanoparticles according to claim 1, characterized in that: The metal nanoparticles are selected from one or more of gold nanoparticles, silver nanoparticles and copper nanoparticles.
6. A method for preparing a composite SERS substrate based on titanium dioxide and metal nanoparticles, characterized in that: The method comprises the following steps: (1) immersing the substrate in a polystyrene microsphere solution and then drying it; (2) spin coating a solution containing a titanium dioxide precursor onto the substrate obtained in step (1), and then drying and calcining the solution to obtain a substrate loaded with a titanium dioxide three-dimensional inverse opal structure; (3) immersing the substrate obtained in step (2) in a metal nanoparticle solution and then drying it; (4) placing the substrate obtained in step (3) in a thiol solution for immersion, taking it out, washing it and drying it; Wherein, the size of the metal nanoparticles is 30-300nm; The thickness of the titanium dioxide three-dimensional inverse opal structure is ≥3000nm.
7. The method according to claim 6, characterized in that In step (1), the diameter of the polystyrene microspheres is 200-1000 nm; Preferably, the concentration of polystyrene microspheres in the polystyrene microsphere solution is 10-40 wt %; Preferably, the ratio of the weight of the polystyrene microspheres in the polystyrene microsphere solution to the area of the coating surface to be spin-coated is 1-8 g / cm 2 .
8. The method according to claim 6 or 7, characterized in that: In step (1), the drying conditions include: temperature of 30-80°C and time of 2-8h.
9. The method according to claim 6, characterized in that In step (2), the ratio of the weight of titanium element in the solution containing titanium dioxide precursor to the area of the spin-coated coating surface is 0.2-2 mg / cm 2 ; Preferably, the titanium dioxide precursor is selected from one or more of di(2-hydroxypropionic acid)diammonium titanium dihydroxide, tetrabutyl titanate, isopropyl titanate and titanyl sulfate.
10. The method according to claim 6, characterized in that In step (2), the spin coating conditions include: a rotation speed of 600-6000 r / min and a time of 1-10 min.
11. The method according to any one of claims 6 to 10, characterized in that: In step (2), the drying conditions include: temperature of 40-120° C. and time of 0.2-5 h.
12. The method according to claim 6 or 11, characterized in that: In step (2), the calcination conditions include: temperature of 300-600° C. and time of 2-8 hours.
13. The method according to claim 6, characterized in that In step (3), the concentration of the metal nanoparticles in the metal nanoparticle solution is 0.1-2.5 mg / mL; Preferably, the ratio of the weight of the metal nanoparticles in the metal nanoparticle solution to the area of the spin-coated coating surface is 0.1-1 mg / cm 2 ; Preferably, the metal nanoparticles are selected from one or more of gold nanoparticles, silver nanoparticles and copper nanoparticles.
14. The method according to claim 6 or 13, characterized in that: In step (3), the drying conditions include: temperature of 50-100° C. and time of 1-10 h.
15. The method according to claim 6, characterized in that In step (4), the mercaptan is selected from one or more of n-propyl mercaptan, n-hexyl mercaptan and n-dodecyl mercaptan; Preferably, the concentration of thiol in the thiol-containing solution is 10 -1 -10 -4 mol / L.
16. The method according to claim 6 or 15, characterized in that In step (4), the soaking time is 10-45 minutes.
17. A composite SERS substrate based on titanium dioxide and metal nanoparticles prepared by the method of any one of claims 6 to 16.
18. Use of the composite SERS substrate based on titanium dioxide and metal nanoparticles according to any one of claims 1 to 5 or the composite SERS substrate based on titanium dioxide and metal nanoparticles according to claim 17 in the detection of polycyclic aromatic hydrocarbons.
19. The use according to claim 18, characterized in that The polycyclic aromatic hydrocarbons are selected from at least one of naphthalene, anthracene, phenanthrene, pyrene and benzopyrene; Preferably, the detection concentration of polycyclic aromatic hydrocarbons by the composite SERS substrate based on titanium dioxide and metal nanoparticles is ≥10 - 8 mol / L.
20. A method for detecting the concentration of polycyclic aromatic hydrocarbons in a solution, characterized in that: The solution to be tested is dripped onto the composite SERS substrate based on titanium dioxide and metal nanoparticles as claimed in claim 1 or claim 17, and SERS detection is performed using a Raman spectrometer.