Low-reflection optical lens and processing technology thereof

By forming an imidazole amino ion liquid interpolation and nano-bilayer coating on the optical lens, the problems of environmental pollution, high cost and insufficient self-repair capabilities in the improvement of low reflection and high transmission performance of existing optical lenses are solved, and the problem of insufficient environmental pollution, high cost and self-repair capabilities in the improvement of low reflection and high transmission performance is achieved. The lens has low reflection, enhanced transparency, anti-fog and anti-fog properties, and gives it the ability to repair itself at room temperature, extending its service life.

CN118938363AActive Publication Date: 2024-11-12XINGLANG OPTICAL TECH (JIANGSU) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410994597.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

While improving low reflection and high transmission performance, existing optical lenses have problems such as environmental pollution, high equipment costs, insufficient bonding between layers and layers and inability to self-repair. They cannot be repaired quickly during mechanical damage, which affects the optical imaging equipment. use.

Method used

The optical lens substrate is etched by fluorine-free etching liquid to form a double layer of hydroxide containing an imidazole amino ion liquid intercalation as a wear-resistant layer, and a nano-bilayer coating is constructed on it, including an anti-reflective layer and a protective layer. , imidazole amino ion liquid composite double-layer mesoporous nanosilicon dioxide, form a gradient of refractive index, enhancing the wear resistance, anti-fog properties and self-healing ability of the lens.

Benefits of technology

It realizes the low reflection, transparency, anti-fog and anti-fog properties of optical lenses, and at the same time gives them the ability to repair their daily temperature, extending the service life of the lenses and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959786850000101
    Figure BDA0004959786850000101
  • Figure BDA0004959786850000111
    Figure BDA0004959786850000111
Patent Text Reader

Abstract

The invention relates to the technical field of optical imaging equipment, in particular to a low-reflection optical lens and a processing technology thereof.Inorganic glass or organic glass is adopted as a lens substrate, ethylene diamine tetraacetic acid disodium and ethylene diamine tetraacetic acid tetrasodium are compounded to serve as a fluoride-free etching solution for etching, and the low-reflection optical lens is obtained. Then double-layer hydroxide containing imidazole amino ionic liquid intercalation is formed on the pretreated substrate to serve as a wear-resistant layer, and a nano double-layer coating is constructed on the wear-resistant layer to form gradient refractive index, so that the optical lens has anti-reflection and anti-fogging properties, and meanwhile, the optical lens is endowed with an antifouling self-repairing surface; the method comprises the following steps: synthesizing 1-methyl-3-n-alkyl brominated imidazole ionic liquid by using brominated n-butane and N-methylimidazole, and then replacing with amino acid aspartic acid to obtain imidazole amino ionic liquid; imidazole amino ionic liquid composite double-layer mesoporous nano silicon dioxide is introduced into the antireflection layer and the protective layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optical imaging equipment, and in particular to a low-reflection optical lens and a processing technology thereof. Background Art

[0002] With the advancement of technology and the rise of various smart devices, the requirements for optical lenses are becoming increasingly stringent, especially for the low reflectivity, anti-fog and wear resistance of optical lenses. For example, they must have a low reflectivity in the visible light wavelength range to avoid ghosting, glare and other problems in imaging.

[0003] In order to improve the low reflection and high transmittance optical performance of optical lenses in the existing market, anti-reflection films are usually prepared on the surface. Traditional methods include hydrofluoric acid solution etching, magnetron sputtering oxide layer film stacking, etc. However, the use of hydrofluoric acid can easily cause environmental pollution, and the equipment of magnetron sputtering is relatively expensive and costly. At the same time, the bonding force between the formed layers is insufficient. At the same time, the optical lenses commonly used in optical imaging equipment in the existing market cannot self-repair at room temperature in a short time when they encounter mechanical damage such as scratches, which in turn affects the use of optical imaging equipment. Summary of the invention

[0004] The purpose of the present invention is to provide a low-reflection optical lens and a processing technology thereof to solve the problems in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A processing technology for low-reflection optical lenses comprises the following steps:

[0007] S1: polishing, rinsing, ultrasonically cleaning the lens substrate in sequence, drying and setting aside; placing the lens substrate in an etching solution, etching at a constant temperature, taking it out and cleaning and drying it to obtain a pre-treated substrate;

[0008] S2: In situ synthesis of a double hydroxide layer containing an imidazolium amino ionic liquid intercalation layer on the pretreated substrate to obtain a wear-resistant layer;

[0009] S3: mixing imidazole amino ionic liquid composite double-layer mesoporous nano-silica, ultrapure water, and anhydrous ethanol, and ultrasonically stirring to obtain a silica slurry; coating the silica slurry on the wear-resistant layer, and drying to obtain an anti-reflection layer;

[0010] S4: Prepare a protective coating using a self-healing prepolymer, imidazole amino ionic liquid composite double-layer mesoporous nano-silica, and N,N-dimethylformamide; apply the protective coating on the anti-reflection layer, cure it to form a protective layer, and obtain a low-reflection optical lens.

[0011] Furthermore, deionized water is used as the solvent: the composition of the etching solution is: 0.2 mol / L disodium ethylenediaminetetraacetate, 0.34 mol / L tetrasodium ethylenediaminetetraacetate, and the pH is 7-8.

[0012] Furthermore, the lens substrate is one of organic glass and inorganic glass.

[0013] Furthermore, the working conditions of the constant temperature etching are: 175-180° C. for 6-7 hours.

[0014] Furthermore, the preparation of the wear-resistant layer includes the following steps: mixing zinc nitrate hexahydrate, aluminum nitrate nonahydrate, urea, and deionized water, placing a pretreated substrate therein, keeping warm at 90-95°C for 22-24 hours, adding imidazole amino ionic liquid, continuing stirring for 1-2 hours, centrifuging, washing, and drying, forming a double-layer hydroxide containing an imidazole amino ionic liquid intercalation layer on the pretreated substrate to obtain a wear-resistant layer.

[0015] Furthermore, the mass volume ratio of the self-healing prepolymer, the imidazole amino ionic liquid composite double-layer mesoporous nano-silica, and N,N-dimethylformamide in the protective coating is 4g:2g:17mL.

[0016] Furthermore, the preparation of the imidazole amino ionic liquid includes the following steps: mixing n-butane bromide and N-methylimidazole under a nitrogen atmosphere, stirring at 75-80° C. for 6-8 hours, cooling to 25° C., extracting with ethyl acetate, rotary evaporation, and drying to obtain 1-methyl-3-n-alkyl imidazole bromide ionic liquid; mixing 1-methyl-3-n-alkyl imidazole bromide ionic liquid, aspartic acid, and potassium hydroxide, keeping warm at 60-70° C. for 3-5 hours, rotary evaporation, adding anhydrous ethanol, suction filtration, filtering, rotary evaporation, and washing to obtain the imidazole amino ionic liquid.

[0017] Furthermore, the preparation of the imidazole amino ionic liquid composite double-layer mesoporous nano-silica comprises the following steps:

[0018] (1) Hexadecyltrimethylammonium bromide, sodium salicylate and deionized water are mixed, kept at 50-60° C. for 15-20 minutes, triethylamine is added, stirring is continued for 5-10 minutes, the temperature is raised to 80° C., tetraethyl silicate and 1,2-bis(triethoxysilyl)ethane are added, the temperature is kept at 10-12 hours, centrifuged, washed with anhydrous ethanol for 3-5 times, and dried to obtain dendritic silica;

[0019] (2) mixing hexadecyltrimethylammonium bromide, sodium salicylate and deionized water, keeping the mixture at 50-60°C for 15-20 minutes, adding triethylamine, continuing stirring for 5-10 minutes, adding the mixture of dendritic silica and deionized water and heating it to 80°C, adding tetraethyl silicate and 1,2-bis(triethoxysilyl)ethane, keeping the mixture for 10-12 hours, centrifuging, washing with anhydrous ethanol for 3-5 times, and drying to obtain double-layer dendritic nanosilica;

[0020] (3) Mixing the double-layer dendritic nano-silica with a sodium carbonate solution, ultrasonically dispersing, keeping warm at 60° C. for 3-6 hours, centrifuging and washing with anhydrous ethanol, adding imidazole amino ionic liquid, and ultrasonically stirring to obtain imidazole amino ionic liquid composite double-layer mesoporous nano-silica.

[0021] Furthermore, the preparation of the self-healing prepolymer comprises the following steps:

[0022] 1) Under a nitrogen atmosphere, dimethylaminoethyl methacrylate and acetone are mixed, and a mixed solution of 1,3-propane sultone, 4-methoxyphenol and acetone is added, and the mixture is kept in a dark place at 18-25° C. for 44-48 hours, precipitated with ice acetone, filtered, dried, precipitated with ice ether, and dried to obtain methacrylic acid sulfobetaine;

[0023] 2) 1H,1H-perfluorooctyl methacrylate, methacrylic acid sulfobetaine, 2,2'-azobisisobutyronitrile and dimethyl sulfoxide are mixed, frozen with liquid nitrogen, and naturally melted at 18-25°C, and the operation is repeated 3-5 times. Under nitrogen protection, the mixture is kept warm at 70-75°C for 44-48 hours, and then dropped into ultrapure water to precipitate, separated, washed and dried to obtain a self-healing prepolymer.

[0024] Furthermore, the mass ratio of 1H,1H-perfluorooctyl methacrylate to methacrylic acid sulfobetaine is 3.16:0.21.

[0025] Beneficial effects of the present invention:

[0026] The present invention provides a low-reflection optical lens and a processing technology thereof. Inorganic glass or organic glass is used as a lens substrate, and a fluorine-free etching solution is used for etching. Then, a double-layer hydroxide containing an imidazole amino ion liquid intercalation layer is formed on the pretreated substrate as a wear-resistant layer. A nano double-layer coating is constructed on the wear-resistant layer to form a refractive index gradient, so that the optical lens has both anti-reflection and anti-fogging properties, and at the same time, an anti-fouling and self-repairing surface is given to the optical lens.

[0027] Disodium ethylenediaminetetraacetate and tetrasodium ethylenediaminetetraacetate, which have strong complexing ability, are compounded as a fluorine-free etching solution. By controlling the process parameters, a pre-treated substrate with a loose and porous surface is obtained, which reduces the reflectivity of the lens substrate and facilitates the subsequent in-situ formation of a double hydroxide layer containing an imidazole amino ionic liquid intercalation layer as a wear-resistant layer on the pre-treated substrate.

[0028] In order to improve the wear resistance of optical lenses and reduce the reflectivity of lenses, the present invention uses urea as a precipitant, zinc nitrate and aluminum nitrate as raw materials, and imidazole amino ionic liquid as an intercalation agent to in-situ form an aluminum zinc hydroxide nanosheet layer containing imidazole amino ionic liquid intercalation on a pretreated substrate, thereby improving the wear resistance of the lens and enhancing the anti-reflection effect of the lens; 1-methyl-3-n-alkyl brominated imidazole ionic liquid is synthesized with n-butane bromide and N-methylimidazole, and then replaced with amino acid aspartic acid to obtain imidazole amino ionic liquid, and the imidazole amino ionic liquid is introduced into the wear-resistant layer, which not only synergistically improves the wear resistance of the wear-resistant layer, but also improves the bonding force between the wear-resistant layer and the subsequent nano-coating, thereby further improving the corrosion and anti-fouling properties of the lens and extending the service life of the lens.

[0029] Construct a nano double-film coating on the wear-resistant layer, including an anti-reflection layer and a protective layer. By adjusting the raw materials, the anti-reflection and anti-fogging properties of the optical lens are enhanced, and the optical lens is given an anti-fouling self-repairing surface, so that it can complete self-repair at room temperature when it encounters mechanical scratches, effectively improving the scratch resistance and anti-fouling properties of the optical lens;

[0030] Imidazole amino ionic liquid composite double-layer mesoporous nano-silica is introduced into both the anti-reflection layer and the protective layer, hexadecyltrimethylammonium bromide and sodium salicylate are used as composite soft templates, and the concentration gradient is constructed by utilizing the difference in the hydrolysis and condensation speeds of 1,2-bis(triethoxysilyl)ethane and ethyl orthosilicate, and then the inorganic components are selectively etched to obtain double-layer mesoporous nano-silica, and its unique and rich pore and cavity structure is composited with imidazole amino ionic liquid to give the optical lens high transmittance and low reflectivity;

[0031] In order to give optical lenses a self-repairing and antifouling surface, the zwitterionic monomer methacrylic acid sulfobetaine was synthesized using dimethylaminoethyl methacrylate and 1,3-propane sultone as raw materials. Methacrylic acid sulfobetaine was used as a hydrophilic monomer and was free radical copolymerized with 1H,1H-perfluorooctyl methacrylate as a hydrophobic monomer to obtain a self-repairing prepolymer. Imidazolyl amino ionic liquid composite double-layer mesoporous nano-silica was added to prepare a self-repairing protective coating. The introduction of imidazolyl amino ionic liquid composite double-layer mesoporous nano-silica can effectively improve the mechanical properties of the coating and reduce the Tg value. The ion-dipole interaction is formed between the more electronegative F atoms in the self-repairing prepolymer and the imidazolyl cations of the imidazolyl amino ionic liquid composite double-layer mesoporous nano-silica, thereby giving the protective layer excellent room temperature intrinsic self-repairing ability. At the same time, the introduction of imidazolyl amino ionic liquid composite double-layer mesoporous nano-silica can effectively improve the water resistance and anti-fogging properties of the protective layer, thereby extending the service life of the optical lens. DETAILED DESCRIPTION

[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] It should be noted that if the embodiments of the present invention involve directional indications such as up, down, left, right, front, back, etc., the directional indication is only used to explain a specific posture such as the relative position relationship between the components, the movement status, etc. If the specific posture changes, the directional indication will also change accordingly. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.

[0034] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0035] Embodiment 1: A processing technology for low-reflection optical lenses, comprising the following steps:

[0036] S1: polishing, rinsing, ultrasonically cleaning the lens substrate in sequence, drying and setting aside; placing the lens substrate in an etching solution, etching at a constant temperature, taking it out and cleaning and drying it to obtain a pre-treated substrate;

[0037] Deionized water was used as the solvent: the composition of the etching solution was: 0.2 mol / L disodium ethylenediaminetetraacetate, 0.34 mol / L tetrasodium ethylenediaminetetraacetate, pH 7; the working conditions of constant temperature etching were: 175°C for 7 hours;

[0038] S2: In situ synthesizing a double-layer hydroxide containing an imidazolium amino ionic liquid intercalation layer on the pretreated substrate to obtain a wear-resistant layer, the preparation comprising the following steps:

[0039] 3mmol zinc nitrate hexahydrate, 1mmol aluminum nitrate nonahydrate, 18mmol urea, and 20mL deionized water were mixed, 1g of the pretreated substrate was placed in it, and the mixture was kept at 90°C for 24h, 0.1g of imidazole amino ionic liquid was added, and the mixture was stirred for 1h, centrifuged, washed, and dried to form a double-layer hydroxide containing an imidazole amino ionic liquid intercalation layer on the pretreated substrate to obtain a wear-resistant layer;

[0040] The preparation of imidazole amino ionic liquid comprises the following steps: in a nitrogen atmosphere, 0.8 mmol of n-butyl bromide and 1 mmol of 2-methylimidazole are mixed, stirred at 75°C for 8 hours, cooled to 25°C, extracted with ethyl acetate, rotary evaporated, and dried to obtain 1-methyl-3-n-alkyl brominated imidazole ionic liquid; 1 mmol of 1-methyl-3-n-alkyl brominated imidazole ionic liquid, 1 mmol of aspartic acid, and 100 mL of 0.05 mol / L potassium hydroxide are mixed, kept warm at 60°C for 5 hours, rotary evaporated, 20 mL of anhydrous ethanol is added, suction filtered, filtered, rotary evaporated, and washed to obtain the imidazole amino ionic liquid.

[0041] S3: 2 g of imidazole amino ionic liquid composite double-layer mesoporous nano-silica, 20 mL of ultrapure water, and 20 mL of anhydrous ethanol were mixed and ultrasonically stirred to obtain a silica slurry; the silica slurry was coated on the wear-resistant layer and dried to obtain an anti-reflection layer;

[0042] The preparation of imidazole amino ionic liquid composite double-layer mesoporous nano-silica comprises the following steps:

[0043] (1) 0.5 mol of hexadecyltrimethylammonium bromide, 0.4 mol of sodium salicylate, and 10 mL of deionized water were mixed, kept at 50° C. for 20 min, 2 mL of triethylamine was added, stirring was continued for 5 min, the temperature was raised to 80° C., 1 mL of tetraethyl silicate and 1 mL of 1,2-bis(triethoxysilyl)ethane were added, the temperature was kept for 10 h, centrifuged, washed with anhydrous ethanol for 3-5 times, and dried to obtain dendritic silica;

[0044] (2) 0.5 mol hexadecyltrimethylammonium bromide, 0.4 mol sodium salicylate, and 10 mL deionized water were mixed, kept at 50°C for 20 min, 2 mL triethylamine was added, stirring was continued for 5 min, the mixture of dendritic silica and deionized water was added and heated to 80°C, 1 mL tetraethyl silicate and 1 mL 1,2-bis(triethoxysilyl)ethane were added, kept warm for 10 h, centrifuged, washed with anhydrous ethanol 3 times, and dried to obtain double-layer dendritic nanosilica;

[0045] (3) 1 g of double-layer dendritic nano-silica was mixed with 100 mL of 0.4 mol / L sodium carbonate solution, ultrasonically dispersed, kept at 60° C. for 3 h, centrifuged and washed with anhydrous ethanol, 0.2 g of imidazole amino ionic liquid was added, and ultrasonically stirred to obtain imidazole amino ionic liquid composite double-layer mesoporous nano-silica;

[0046] S4: Prepare a protective coating using 4 g of self-repairing prepolymer, 2 g of imidazole amino ionic liquid composite double-layer mesoporous nano-silica, and 17 mL of N,N-dimethylformamide; apply the protective coating on the anti-reflection layer, cure it to form a protective layer, and obtain a low-reflection optical lens;

[0047] The preparation of the self-healing prepolymer includes the following steps:

[0048] 1) Under a nitrogen atmosphere, 1 g of dimethylaminoethyl methacrylate and 20 mL of acetone were mixed, and a mixture of 0.73 g of 1,3-propane sultone, 2 mg of 4-methoxyphenol, and 10 mL of acetone was added, and the mixture was kept in the dark at 18° C. for 48 h, and precipitated with ice acetone, filtered, and dried, and precipitated with ice ether and dried to obtain methacrylic acid sulfobetaine;

[0049] 2) 3.16 g 1H,1H-methacrylate perfluorooctyl ester, 0.21 g methacrylate sulfobetaine, 40 mg 2,2'-azobisisobutyronitrile, and 18 mL dimethyl sulfoxide were mixed, frozen with liquid nitrogen, and naturally thawed at 18°C. The operation was repeated 3 times, and the mixture was kept warm at 70°C for 48 h under nitrogen protection, and then dropped into ultrapure water to precipitate, separated, washed, and dried to obtain a self-healing prepolymer.

[0050] Embodiment 2: A processing technology for a low-reflection optical lens, comprising the following steps:

[0051] S1: polishing, rinsing, ultrasonically cleaning the lens substrate in sequence, drying and setting aside; placing the lens substrate in an etching solution, etching at a constant temperature, taking it out and cleaning and drying it to obtain a pre-treated substrate;

[0052] Deionized water was used as the solvent: the composition of the etching solution was: 0.2 mol / L disodium ethylenediaminetetraacetate, 0.34 mol / L tetrasodium ethylenediaminetetraacetate, pH 7.5; the working conditions of constant temperature etching were: 178°C for 6.5 hours;

[0053] S2: In situ synthesizing a double-layer hydroxide containing an imidazolium amino ionic liquid intercalation layer on the pretreated substrate to obtain a wear-resistant layer, the preparation comprising the following steps:

[0054] 3mmol zinc nitrate hexahydrate, 1mmol aluminum nitrate nonahydrate, 18mmol urea, and 20mL deionized water were mixed, 1g of the pretreated substrate was placed in it, and the mixture was kept at 93°C for 23h, 0.1g of imidazole amino ionic liquid was added, and the mixture was stirred for 1.5h, centrifuged, washed, and dried to form a double-layer hydroxide containing an imidazole amino ionic liquid intercalation layer on the pretreated substrate to obtain a wear-resistant layer;

[0055] The preparation of imidazole amino ionic liquid comprises the following steps: in a nitrogen atmosphere, 0.8 mmol of n-butyl bromide and 1 mmol of 2-methylimidazole are mixed, stirred at 78° C. for 7 hours, cooled to 25° C., extracted with ethyl acetate, rotary evaporated, and dried to obtain 1-methyl-3-n-alkyl brominated imidazole ionic liquid; 1 mmol of 1-methyl-3-n-alkyl brominated imidazole ionic liquid, 1 mmol of aspartic acid, and 100 mL of 0.05 mol / L potassium hydroxide are mixed, kept warm at 65° C. for 4 hours, rotary evaporated, 20 mL of anhydrous ethanol is added, suction filtered, filtered, rotary evaporated, and washed to obtain imidazole amino ionic liquid;

[0056] S3: 2 g of imidazole amino ionic liquid composite double-layer mesoporous nano-silica, 20 mL of ultrapure water, and 20 mL of anhydrous ethanol were mixed and ultrasonically stirred to obtain a silica slurry; the silica slurry was coated on the wear-resistant layer and dried to obtain an anti-reflection layer;

[0057] The preparation of imidazole amino ionic liquid composite double-layer mesoporous nano-silica comprises the following steps:

[0058] (1) 0.5 mol hexadecyltrimethylammonium bromide, 0.4 mol sodium salicylate, and 10 mL deionized water were mixed, kept at 55° C. for 18 min, 2 mL triethylamine was added, stirring was continued for 8 min, the temperature was raised to 80° C., 1 mL tetraethyl silicate and 1 mL 1,2-bis(triethoxysilyl)ethane were added, the temperature was kept for 10-12 h, centrifuged, washed with anhydrous ethanol 4 times, and dried to obtain dendritic silica;

[0059] (2) 0.5 mol hexadecyltrimethylammonium bromide, 0.4 mol sodium salicylate, and 10 mL deionized water were mixed, kept at 55°C for 18 min, 2 mL triethylamine was added, stirring was continued for 8 min, the mixture of dendritic silica and deionized water was added and heated to 80°C, 1 mL tetraethyl silicate and 1 mL 1,2-bis(triethoxysilyl)ethane were added, kept warm for 11 h, centrifuged, washed with anhydrous ethanol 4 times, and dried to obtain double-layer dendritic nanosilica;

[0060] (3) 1 g of double-layer dendritic nano-silica was mixed with 100 mL of 0.4 mol / L sodium carbonate solution, ultrasonically dispersed, kept at 60° C. for 4 h, centrifuged and washed with anhydrous ethanol, 0.2 g of imidazole amino ionic liquid was added, and ultrasonically stirred to obtain imidazole amino ionic liquid composite double-layer mesoporous nano-silica;

[0061] S4: Prepare a protective coating using 4 g of self-repairing prepolymer, 2 g of imidazole amino ionic liquid composite double-layer mesoporous nano-silica, and 17 mL of N,N-dimethylformamide; apply the protective coating on the anti-reflection layer, cure it to form a protective layer, and obtain a low-reflection optical lens;

[0062] The preparation of the self-healing prepolymer includes the following steps:

[0063] 1) Under a nitrogen atmosphere, 1 g of dimethylaminoethyl methacrylate and 20 mL of acetone were mixed, and a mixture of 0.73 g of 1,3-propane sultone, 2 mg of 4-methoxyphenol, and 10 mL of acetone was added, and the mixture was kept in a dark place at 20° C. for 45 h, and precipitated with ice acetone, filtered, and dried, and precipitated with ice ether, and dried to obtain methacrylic acid sulfobetaine;

[0064] 2) 3.16 g 1H,1H-methacrylate perfluorooctyl ester, 0.21 g methacrylate sulfobetaine, 40 mg 2,2'-azobisisobutyronitrile, and 18 mL dimethyl sulfoxide were mixed, frozen with liquid nitrogen, and naturally thawed at 20°C. The operation was repeated 4 times, and the mixture was kept warm at 72°C for 46 h under nitrogen protection, and then dropped into ultrapure water to precipitate, separated, washed, and dried to obtain a self-healing prepolymer.

[0065] Embodiment 3: A processing technology for low-reflection optical lenses, comprising the following steps:

[0066] S1: polishing, rinsing, ultrasonically cleaning the lens substrate in sequence, drying and setting aside; placing the lens substrate in an etching solution, etching at a constant temperature, taking it out and cleaning and drying it to obtain a pre-treated substrate;

[0067] Deionized water was used as the solvent: the composition of the etching solution was: 0.2 mol / L disodium ethylenediaminetetraacetate, 0.34 mol / L tetrasodium ethylenediaminetetraacetate, pH 8; the working conditions of constant temperature etching were: 180°C for 6 hours;

[0068] S2: In situ synthesizing a double-layer hydroxide containing an imidazolium amino ionic liquid intercalation layer on the pretreated substrate to obtain a wear-resistant layer, the preparation comprising the following steps:

[0069] 3mmol zinc nitrate hexahydrate, 1mmol aluminum nitrate nonahydrate, 18mmol urea, and 20mL deionized water were mixed, 1g of the pretreated substrate was placed in it, and the mixture was kept at 95°C for 22h, 0.1g of imidazole amino ionic liquid was added, and the mixture was stirred for 2h, centrifuged, washed, and dried to form a double-layer hydroxide containing an imidazole amino ionic liquid intercalation layer on the pretreated substrate to obtain a wear-resistant layer;

[0070] The preparation of the imidazole amino ionic liquid comprises the following steps: in a nitrogen atmosphere, 0.8 mmol of n-butyl bromide and 1 mmol of 2-methylimidazole are mixed, stirred at 80° C. for 6 hours, cooled to 25° C., extracted with ethyl acetate, rotary evaporated, and dried to obtain 1-methyl-3-n-alkyl brominated imidazole ionic liquid; 1 mmol of 1-methyl-3-n-alkyl brominated imidazole ionic liquid, 1 mmol of aspartic acid, and 100 mL of 0.05 mol / L potassium hydroxide are mixed, kept warm at 70° C. for 3 hours, rotary evaporated, 20 mL of anhydrous ethanol is added, suction filtered, filtered, rotary evaporated, and washed to obtain the imidazole amino ionic liquid;

[0071] S3: 2 g of imidazole amino ionic liquid composite double-layer mesoporous nano-silica, 20 mL of ultrapure water, and 20 mL of anhydrous ethanol were mixed and ultrasonically stirred to obtain a silica slurry; the silica slurry was coated on the wear-resistant layer and dried to obtain an anti-reflection layer;

[0072] The preparation of imidazole amino ionic liquid composite double-layer mesoporous nano-silica comprises the following steps:

[0073] (1) 0.5 mol of hexadecyltrimethylammonium bromide, 0.4 mol of sodium salicylate, and 10 mL of deionized water were mixed, kept at 60°C for 15 min, 2 mL of triethylamine was added, stirring was continued for 10 min, the temperature was raised to 80°C, 1 mL of tetraethyl silicate and 1 mL of 1,2-bis(triethoxysilyl)ethane were added, the temperature was kept for 12 h, centrifuged, washed with anhydrous ethanol 5 times, and dried to obtain dendritic silica;

[0074] (2) 0.5 mol hexadecyltrimethylammonium bromide, 0.4 mol sodium salicylate, and 10 mL deionized water were mixed, kept at 60°C for 15 min, 2 mL triethylamine was added, stirring was continued for 10 min, the mixture of dendritic silica and deionized water was added and heated to 80°C, 1 mL tetraethyl silicate and 1 mL 1,2-bis(triethoxysilyl)ethane were added, kept warm for 12 h, centrifuged, washed with anhydrous ethanol 5 times, and dried to obtain double-layer dendritic nanosilica;

[0075] (3) 1 g of double-layer dendritic nano-silica was mixed with 100 mL of 0.4 mol / L sodium carbonate solution, ultrasonically dispersed, kept at 60° C. for 6 h, centrifuged and washed with anhydrous ethanol, 0.2 g of imidazole amino ionic liquid was added, and ultrasonically stirred to obtain imidazole amino ionic liquid composite double-layer mesoporous nano-silica;

[0076] S4: Prepare a protective coating using 4 g of self-repairing prepolymer, 2 g of imidazole amino ionic liquid composite double-layer mesoporous nano-silica, and 17 mL of N,N-dimethylformamide; apply the protective coating on the anti-reflection layer, cure it to form a protective layer, and obtain a low-reflection optical lens;

[0077] The preparation of the self-healing prepolymer includes the following steps:

[0078] 1) Under a nitrogen atmosphere, 1 g of dimethylaminoethyl methacrylate and 20 mL of acetone were mixed, and a mixture of 0.73 g of 1,3-propane sultone, 2 mg of 4-methoxyphenol, and 10 mL of acetone was added, and the mixture was kept in the dark at 25° C. for 44 h, and precipitated with ice acetone, filtered, and dried, and precipitated with ice ether and dried to obtain methacrylic acid sulfobetaine;

[0079] 2) 3.16 g 1H,1H-methacrylate perfluorooctyl ester, 0.21 g methacrylate sulfobetaine, 40 mg 2,2'-azobisisobutyronitrile, and 18 mL dimethyl sulfoxide were mixed, frozen with liquid nitrogen, and naturally thawed at 25°C. The operation was repeated 5 times, and the mixture was kept warm at 75°C for 44 h under nitrogen protection, and then dropped into ultrapure water to precipitate, separated, washed, and dried to obtain a self-healing prepolymer.

[0080] Comparative Example 1: Example 3 was used as the control group, without etching, and other processes were normal.

[0081] Comparative Example 2: Taking Example 3 as the control group, the imidazolium amino ionic liquid was replaced by 1-methyl-3-n-alkyl imidazolium bromide ionic liquid, and the other processes were normal.

[0082] Comparative Example 3: Example 3 was used as a control group, in which imidazole amino ionic liquid was not prepared, and other processes were normal.

[0083] Comparative Example 4: Taking Example 3 as the control group, the imidazole amino ionic liquid composite double-layer mesoporous nano-silica was replaced by silicon dioxide (S433678: Aladdin reagent), and the other processes were normal.

[0084] Comparative Example 5: Example 3 was used as the control group, no self-repairing prepolymer was prepared, and other processes were normal.

[0085] Comparative Example 6: Example 3 was used as the control group, no wear-resistant layer was prepared, and other processes were normal.

[0086] In the above embodiments and comparative examples, the wear-resistant layer is 50 nm, the anti-reflection layer is 100 nm, and the protective layer is 200 nm.

[0087] The sources of raw materials used in the above examples and comparative examples are:

[0088] The lens substrate is aluminosilicate tempered glass 7418 (0.7mm): Corning, USA; disodium ethylenediaminetetraacetic acid E116431, tetrasodium ethylenediaminetetraacetic acid T161517, zinc nitrate hexahydrate Z111703, aluminum nitrate nonahydrate A110781, urea U111897, n-butane bromide B105250, 2-methylimidazole M104839, aspartic acid A163270, hexadecyltrimethylammonium bromide H108983, sodium salicylate S104176, triethylamine T103285, tetraethyl silicate T1 10596, 1,2-bis(triethoxysilyl)ethane W132160, N,N-dimethylformamide D111999, dimethylaminoethyl methacrylate D111129, 1,3-propanesultone P105652, 4-methoxyphenol M170858, 1H,1H-perfluorooctyl methacrylate H477322, 2,2'-azobisisobutyronitrile A104255, dimethyl sulfoxide D432337; ethyl acetate, potassium hydroxide, anhydrous ethanol, sodium carbonate, acetone, analytical grade: Sinopharm Group reagents.

[0089] Performance Test:

[0090] Performance tests were performed on Examples 1-3 and Comparative Examples 1-6;

[0091] Light transmittance: measure the average transmittance in the 300-800nm ​​band; Self-repairing property: scratch a 100nm long and 100nm deep scratch on the surface, keep it at 30℃ for 24h, measure the light transmittance before and after the scratch test, and characterize the self-repairing property, which is recorded as the self-repairing rate; Anti-fogging property: place the lens substrate and the sample vertically on a semiconductor cold table, and place them in a box with an ultrasonic humidifier that can generate fog. The working temperature is 25℃ and the humidity is 75%. The transmittance after 5min of atomization is tested. The transmittance of the lens substrate after 5min of atomization is 86%. The difference between the transmittance of the sample and the lens substrate after atomization characterizes the anti-fogging property. A value greater than 9 is excellent, 5-9 is qualified, and a value less than 5 is unqualified; Friction resistance: wrap a 2kg weight with a dust-free cloth, rub it back and forth on the sample surface 500 times, compare the transmittance ratio before and after friction and characterize it. The results are shown in Table 1;

[0092] Table 1

[0093]

[0094]

[0095] The present invention provides a low-reflection optical lens and a processing technology thereof. Inorganic glass or organic glass is used as a lens substrate, and a fluorine-free etching solution is used for etching. Then, a double-layer hydroxide containing an imidazole amino ion liquid intercalation layer is formed on the pretreated substrate as a wear-resistant layer. A nano double-layer coating is constructed on the wear-resistant layer to form a refractive index gradient, so that the optical lens has both anti-reflection and anti-fogging properties, and at the same time, an anti-fouling and self-repairing surface is given to the optical lens.

[0096] Comparing Example 3 with Comparative Example 1, disodium ethylenediaminetetraacetate and tetrasodium ethylenediaminetetraacetate having strong complexing ability are compounded as fluorine-free etching solution, and by controlling process parameters, a loose and porous pre-treated substrate is obtained. While reducing the reflectivity of the lens substrate, it facilitates the subsequent in-situ formation of a double hydroxide layer containing an imidazole amino ionic liquid intercalation layer on the pre-treated substrate as a wear-resistant layer, thereby improving various performances of the lens.

[0097] Example 3 is compared with Comparative Examples 2 and 3. 1-Methyl-3-n-alkyl imidazolium bromide ionic liquid is synthesized with n-butane bromide and N-methylimidazole, and then replaced with amino acid aspartic acid to obtain imidazolium amino ionic liquid. The imidazolium amino ionic liquid is introduced into the wear-resistant layer, which not only synergistically improves the wear resistance of the wear-resistant layer, but also improves the bonding strength between the wear-resistant layer and the subsequent nano-coating, thereby further improving the corrosion and anti-fouling properties of the lens and extending the service life of the lens; ion-dipole interactions are formed between the more electronegative F atoms in the self-repairing prepolymer and the imidazolium cations of the imidazolium amino ionic liquid composite double-layer mesoporous nano-silica, thereby giving the protective layer excellent room temperature intrinsic self-repairing ability; at the same time, the introduction of the imidazolium amino ionic liquid composite double-layer mesoporous nano-silica can effectively improve the water resistance and anti-fogging properties of the protective layer, thereby extending the service life of the optical lens.

[0098] Comparing Example 3 with Comparative Example 4, imidazole amino ionic liquid composite double-layer mesoporous nano-silica is introduced into both the anti-reflection layer and the protective layer, hexadecyltrimethylammonium bromide and sodium salicylate are used as composite soft templates, and the concentration gradient is constructed by utilizing the difference in the hydrolysis condensation rate of 1,2-bis(triethoxysilyl)ethane and ethyl orthosilicate, and then the inorganic component is selectively etched to obtain double-layer mesoporous nano-silica, and its unique and rich pore and cavity structure is utilized to composite with imidazole amino ionic liquid to give the optical lens high transmittance and low reflectivity;

[0099] Example 3 is compared with Comparative Example 5. In order to give the optical lens a self-repairing and anti-fouling surface, dimethylaminoethyl methacrylate and 1,3-propane sultone are used as raw materials to synthesize the zwitterionic monomer methacrylic acid sulfonate betaine, and methacrylic acid sulfonate betaine is used as a hydrophilic monomer and is free radical-copolymerized with 1H,1H-methacrylate perfluorooctyl ester as a hydrophobic monomer to obtain a self-repairing prepolymer, and imidazole amino ionic liquid composite double-layer mesoporous nano-silica is added to prepare a self-repairing protective coating. The introduction of imidazole amino ionic liquid composite double-layer mesoporous nano-silica can effectively improve the mechanical properties of the coating and reduce the Tg value, wherein the F atoms with higher electronegativity in the self-repairing prepolymer and the imidazole cations of the imidazole amino ionic liquid composite double-layer mesoporous nano-silica form ion-dipole interactions, thereby giving the protective layer excellent room temperature intrinsic self-repairing ability; at the same time, the introduction of imidazole amino ionic liquid composite double-layer mesoporous nano-silica can effectively improve the water resistance and anti-fog properties of the protective layer, thereby extending the service life of the optical lens.

[0100] Example 3 is compared with Comparative Example 6. In order to improve the wear resistance of the optical lens and reduce the reflectivity of the lens, the present invention uses urea as a precipitant, zinc nitrate and aluminum nitrate as raw materials, and imidazole amino ionic liquid as an intercalating agent to in situ form an aluminum zinc hydroxide nanosheet layer containing imidazole amino ionic liquid intercalation on a pretreated substrate, thereby improving the wear resistance of the lens while enhancing the anti-reflection and anti-transmission effects of the lens.

[0101] Comparing Example 3 with Comparative Example 1, a nanometer double film-forming coating is constructed on the wear-resistant layer, including an anti-reflection layer and a protective layer. By adjusting the raw materials, the anti-reflection and anti-fogging properties of the optical lens are enhanced, and the anti-fouling and self-repairing surface of the optical lens is given, so that the optical lens can complete self-repair at room temperature when it encounters mechanical scratches, effectively improving the scratch resistance and anti-fouling properties of the optical lens, thereby extending the service life of the optical lens;

[0102] The above descriptions are only embodiments of the present invention and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the present invention specification under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A processing technology for low-reflection optical lenses, characterized in that: The following steps are involved: S1: polishing, rinsing, ultrasonically cleaning the lens substrate in sequence, drying and setting aside; placing the lens substrate in an etching solution, etching at a constant temperature, taking it out and cleaning and drying it to obtain a pre-treated substrate; S2: In situ synthesis of a double hydroxide layer containing an imidazolium amino ionic liquid intercalation layer on the pretreated substrate to obtain a wear-resistant layer; S3: mixing imidazole amino ionic liquid composite double-layer mesoporous nano-silica, ultrapure water, and anhydrous ethanol, and ultrasonically stirring to obtain a silica slurry; coating the silica slurry on the wear-resistant layer, and drying to obtain an anti-reflection layer; S4: Prepare a protective coating using a self-healing prepolymer, imidazole amino ionic liquid composite double-layer mesoporous nano-silica, and N,N-dimethylformamide; apply the protective coating on the anti-reflection layer, cure it to form a protective layer, and obtain a low-reflection optical lens.

2. The processing technology of a low-reflection optical lens according to claim 1, characterized in that: Deionized water is used as the solvent: the composition of the etching solution is: 0.2 mol / L disodium ethylenediaminetetraacetate, 0.34 mol / L tetrasodium ethylenediaminetetraacetate, and the pH is 7-8.

3. The processing technology of a low-reflection optical lens according to claim 1, characterized in that: The working conditions of constant temperature etching are: 175-180℃ for 6-7h.

4. The processing technology of a low-reflection optical lens according to claim 1, characterized in that: Preparation of wear-resistant layer The method comprises the following steps: mixing zinc nitrate hexahydrate, aluminum nitrate nonahydrate, urea and deionized water, placing a pretreated substrate therein, keeping the temperature at 90-95°C for 22-24 hours, adding imidazole amino ionic liquid, continuing stirring for 1-2 hours, centrifuging, washing and drying, forming a double-layer hydroxide containing an imidazole amino ionic liquid intercalation layer on the pretreated substrate, and obtaining a wear-resistant layer.

5. The processing technology of a low-reflection optical lens according to claim 1, characterized in that: In the protective coating, the mass volume ratio of the self-healing prepolymer, the imidazole amino ionic liquid composite double-layer mesoporous nano-silica, and N,N-dimethylformamide is 4g:2g:17mL.

6. The processing technology of a low-reflection optical lens according to claim 1, characterized in that: The preparation of imidazole amino ionic liquid comprises the following steps: mixing n-butane bromide and N-methyl imidazole under nitrogen atmosphere, stirring at 75-80 DEG C for 6-8 hours, cooling to 25 DEG C, extracting with ethyl acetate, rotary evaporation and drying to obtain 1-methyl-3-n-alkyl imidazole bromide ionic liquid; mixing 1-methyl-3-n-alkyl imidazole bromide ionic liquid, aspartic acid and potassium hydroxide, keeping warm at 60-70 DEG C for 3-5 hours, rotary evaporation, adding anhydrous ethanol, suction filtration, filtering, rotary evaporation and washing to obtain imidazole amino ionic liquid.

7. The processing technology of a low-reflection optical lens according to claim 1, characterized in that: The preparation of imidazole amino ionic liquid composite double-layer mesoporous nano-silica comprises the following steps: (1) Hexadecyltrimethylammonium bromide, sodium salicylate and deionized water are mixed, kept at 50-60° C. for 15-20 minutes, triethylamine is added, stirring is continued for 5-10 minutes, the temperature is raised to 80° C., tetraethyl silicate and 1,2-bis(triethoxysilyl)ethane are added, the temperature is kept at 10-12 hours, centrifuged, washed with anhydrous ethanol for 3-5 times, and dried to obtain dendritic silica; (2) mixing hexadecyltrimethylammonium bromide, sodium salicylate and deionized water, keeping the mixture at 50-60°C for 15-20 minutes, adding triethylamine, continuing stirring for 5-10 minutes, adding the mixture of dendritic silica and deionized water and heating it to 80°C, adding tetraethyl silicate and 1,2-bis(triethoxysilyl)ethane, keeping the mixture for 10-12 hours, centrifuging, washing with anhydrous ethanol for 3-5 times, and drying to obtain double-layer dendritic nanosilica; (3) Mixing the double-layer dendritic nano-silica with a sodium carbonate solution, ultrasonically dispersing, keeping warm at 60° C. for 3-6 hours, centrifuging and washing with anhydrous ethanol, adding imidazole amino ionic liquid, and ultrasonically stirring to obtain imidazole amino ionic liquid composite double-layer mesoporous nano-silica.

8. The processing technology of a low-reflection optical lens according to claim 1, characterized in that: The preparation of the self-healing prepolymer includes the following steps: 1) Under a nitrogen atmosphere, dimethylaminoethyl methacrylate and acetone are mixed, and a mixed solution of 1,3-propane sultone, 4-methoxyphenol and acetone is added, and the mixture is kept in a dark place at 18-25° C. for 44-48 hours, precipitated with ice acetone, filtered, dried, precipitated with ice ether, and dried to obtain methacrylic acid sulfobetaine; 2) 1H,1H-perfluorooctyl methacrylate, methacrylic acid sulfobetaine, 2,2'-azobisisobutyronitrile and dimethyl sulfoxide are mixed, frozen with liquid nitrogen, and naturally melted at 18-25°C, and the operation is repeated 3-5 times. Under nitrogen protection, the mixture is kept warm at 70-75°C for 44-48 hours, and then dropped into ultrapure water to precipitate, separated, washed and dried to obtain a self-healing prepolymer.

9. The processing technology of a low-reflection optical lens according to claim 8, characterized in that: The mass ratio of 1H,1H-perfluorooctyl methacrylate and methacrylate sulfobetaine is 3.16:0.

21.

10. A low-reflection optical lens, characterized in that: The invention is prepared by any one of the processing techniques of claims 1 to 9.

Citation Information

Patent Citations

  • Superhydrophobic self-healing intelligent nano-coating and preparation method thereof

    CN105524497A

  • Preparation method of zinc selenide nano hollow sphere double-layer graded-index antireflection film

    CN110133764A

  • Self-repairing resin, preparation method and application thereof, and preparation method of self-repairing optical film

    CN113667054A

  • Self-healing coating optical lens and manufacturing method thereof

    KR101483043B1

  • Optical Elements with Gradient Structure

    US20100321784A1