Square-core silica optical fiber for laser transmission, preparation method of square-core silica optical fiber and optical fiber laser
By designing the structure and preparation method of square core quartz fiber, the problems of uneven beam superposition and local energy loss in fiber lasers are solved, spot homogenization and stable laser energy transmission are achieved, and it is suitable for applications in multiple fields.
Patent Information
- Application Number
- CN202411116833.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
In existing fiber lasers, circular core fibers are prone to cause uneven beam superposition and local energy loss when combined, affecting the uniformity and efficiency of laser energy transmission.
The square core quartz fiber is used to prepare a square core quartz fiber with high geometric accuracy through the core layer, inner cladding, outer cladding and coating structure concentrically arranged from the inside to the outside, combined with specific deposition and assembly processes. Realize spot homogenization and stable laser energy transmission.
It realizes the homogenization of the light beam, improves the transmission efficiency and stability of laser energy, and is suitable for the fields of national defense, scientific research, industry and medical beauty.
Smart Images

Figure CN118938387A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of energy transmission optical fibers, and in particular relates to a square core quartz optical fiber for laser transmission and a preparation method thereof, and an optical fiber laser. Background Art
[0002] With the rapid development of fiber lasers in the fields of national defense, scientific research, industry, medical cosmetology, etc., the power and uniformity of their output beams have become the focus of attention at home and abroad. Compared with other lasers, fiber lasers mainly use glass optical fibers doped with rare earth elements such as ytterbium, erbium, and thulium as gain media, which have the advantages of high power, low energy consumption, simple structure, and low cost. In addition, through the fiber beam combining device, multiple lasers can be combined and output to meet the use requirements of different powers, with high flexibility. The energy of fiber lasers is mainly output through energy transmission optical fibers. Such optical fibers are usually composed of concentric circles with different refractive indices on the end faces. When the laser is transmitted in the optical fiber, the energy is Gaussian distributed. This mode distribution is prone to energy concentration and local damage in the region, thereby reducing its own transmission efficiency and uniformity, affecting the processing quality of the product.
[0003] In response to the problems of uneven beam superposition and local energy loss caused by this type of circular core optical fiber during beam combining, the researchers proposed the design of square core quartz energy transfer fiber, which can not only shape the output light mode of the laser and output a homogenized square flat-top optical mode field with high coupling efficiency, but also can be tightly stacked when the beams are combined at the end, thereby improving the energy density of the beam and meeting the needs of high-quality laser processing.
[0004] However, unlike circular core optical fiber, which can obtain different refractive index layers by direct deposition in a tube in one step, square core optical fiber usually needs to be polished multiple times due to its special structure of square or square core; then a concentric circular fluorine-doped layer of a specific thickness is deposited on the inner wall of the circular base tube through the in-tube deposition process, and the fluorine-doped layer is polished into a square inner hole matching the core rod; the existing hole-cutting process is to directly hollow out the circular hole into a square structure, or directly divide the circular base tube on which the fluorine-doped layer is deposited into two halves and then fine-process the fluorine-doped layer into a square groove, and finally directly splice and assemble the two semicircular base tubes with square grooves with the square core rod. However, the above process is relatively complicated, has high requirements for cold machine processing accuracy, and is prone to introduce defects in the process, resulting in high local heat during laser energy transmission and fiber damage.
[0005] Therefore, it is urgent to develop a square-core quartz optical fiber for laser transmission that can achieve light spot homogenization and stable transmission of laser energy. Summary of the invention
[0006] The invention provides a square core quartz optical fiber for laser transmission, which is used to solve the problems of uneven beam superposition, local energy loss and the like in the prior art.
[0007] The invention provides a method for preparing a square core quartz optical fiber for laser transmission. The preparation method is simple and can prepare the square core quartz optical fiber for laser transmission with homogenized light spot and stable transmission of laser energy.
[0008] The present invention provides a fiber laser, comprising a fiber laser body and the square-core quartz fiber for laser transmission connected to the fiber laser body or the square-core quartz fiber for laser transmission prepared by the preparation method.
[0009] In a first aspect, the present invention provides a square core quartz optical fiber for laser transmission, wherein the square core quartz optical fiber for laser transmission comprises a core layer, an inner cladding layer, an outer cladding layer and a coating layer which are concentrically arranged in sequence from the inside to the outside;
[0010] On a cross section perpendicular to the extension direction of the square core quartz optical fiber for laser transmission, the cross section of the core layer is in a square shape, the cross section of the inner cladding is in a square ring shape, and the cross section of the outer cladding is in a circular ring shape with a square through hole;
[0011] The verticality of the edge of the core layer is not greater than 1°, the concentricity of the core layer and the inner cladding is not greater than 0.25 μm; the difference in the side length of the core layer is not greater than 0.25 μm; and the corner radius of the core layer is not greater than 1.25 μm.
[0012] Furthermore, the numerical aperture of the square-core quartz optical fiber for laser transmission is 0.06-0.22.
[0013] Further, a first difference between the refractive index of the core layer and the refractive index of the outer cladding layer is 0 to 0.7%; and / or,
[0014] A second difference between the refractive index of the inner cladding and the refractive index of the outer cladding is -0.5 to -1.2%.
[0015] Furthermore, on a cross section perpendicular to the extension direction of the square core quartz optical fiber for laser transmission, the side length of the core layer is 20 to 600 μm; and / or,
[0016] The thickness of the inner cladding is 1 to 50 μm; and / or,
[0017] The outer radius of the outer cladding is 60-1000 μm.
[0018] Further, the core layer comprises silicon dioxide; and / or,
[0019] The hydroxyl content of the core layer is not more than 1 ppm; and / or,
[0020] The inner cladding comprises fluorine-doped silicon dioxide; and / or,
[0021] The outer cladding includes silicon dioxide.
[0022] Furthermore, the core layer also includes germanium oxide.
[0023] Furthermore, the coating layer includes an inner coating layer and an outer coating layer which are concentrically arranged in sequence; the inner coating layer is close to the outer coating layer;
[0024] The inner coating layer includes a polyacrylic acid resin having a refractive index of 1.36 to 1.42, and the outer coating layer includes a polyacrylic acid resin having a refractive index of 1.49 to 1.51.
[0025] In a second aspect, the present invention provides a method for preparing the square core quartz optical fiber for laser transmission according to the first aspect, characterized in that it comprises the following steps:
[0026] (1) performing a first deposition process on the outer wall of a square target rod to form a loose circular square core-shell layer, and after extracting the square target rod, degassing and sintering the loose circular square core-shell layer to obtain an outer cladding precursor;
[0027] (2) performing a second deposition process on the inner wall of the outer cladding precursor to form an inner cladding precursor, thereby obtaining a circular square core substrate tube;
[0028] (3) assembling the square core rod and the circular square core base tube into a rod-enclosed manner, and then performing a drawing process to obtain an optical fiber precursor;
[0029] (4) forming a coating layer on the outer wall of the optical fiber precursor to obtain the square core silica optical fiber for laser transmission.
[0030] Further, a first deposition treatment is performed on the outer wall of the square target rod by vapor axial deposition or external vapor deposition to form the loose circular square core shell layer with a thickness of not less than 60 mm, and after the square target rod is extracted, the loose circular square core shell layer is degassed and sintered to obtain the outer cladding precursor with an outer diameter of 30 to 45 mm; and / or,
[0031] Performing a second deposition process on the inner wall of the outer cladding precursor by chemical vapor deposition or plasma vapor deposition to form the inner cladding precursor with a thickness of 1.5 to 5 mm; and / or,
[0032] The rod assembly process adopts vertical assembly, and the gap between the outer wall of the square core rod and the inner wall of the circular square core base tube is 0.5-1.5 mm; and / or,
[0033] The square target rod is at least one of aluminum oxide, zirconium oxide, and aluminum nitride; the surface roughness of the square target rod is not greater than 0.6 μm; and / or,
[0034] The square core rod has a hydroxyl content of no greater than 1 ppm and a surface roughness of no greater than 0.3 μm.
[0035] In a third aspect, the present invention provides a fiber laser, comprising a fiber laser body and the square-core quartz fiber for laser transmission described in the first aspect or the square-core quartz fiber for laser transmission prepared by the preparation method described in the second aspect connected to the fiber laser body.
[0036] The invention provides a square core quartz optical fiber for laser transmission, which comprises a core layer, an inner cladding layer, an outer cladding layer and a coating layer which are concentrically sleeved in sequence from the inside to the outside; on a cross section perpendicular to the extension direction of the square core quartz optical fiber for laser transmission, the cross section of the core layer is in a square shape, the cross section of the inner cladding layer is in a square ring shape, and the cross section of the outer cladding layer is in a circular ring shape with a square through hole; and by further limiting the verticality of the edge of the square core quartz optical fiber for laser transmission, the concentricity of the core layer and the inner cladding layer, the difference in the side length of the core layer, and the corner radius of the core layer, the square core quartz optical fiber for laser transmission with high geometric accuracy and uniform components can be obtained, the light spot can be homogenized, and the laser energy can be stably transmitted, which is conducive to wide application in the fields of national defense, scientific research, industry, medical cosmetology, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 Schematic diagram of the cross section and refractive index of a square core quartz optical fiber for laser transmission in one embodiment of the present invention;
[0038] Figure 2 Schematic diagram of the corner radius of the core layer;
[0039] Figure 3 Schematic diagram of a method for preparing a square core quartz optical fiber for laser transmission in one embodiment of the present invention.
[0040] Description of reference numerals:
[0041] 110: core layer;
[0042] 210: inner cladding;
[0043] 310: outer layer;
[0044] 1: Square target stick;
[0045] 2: Loose round square core shell;
[0046] 3: Flame blowtorch;
[0047] 4: outer cladding precursor;
[0048] 5: inner cladding precursor;
[0049] 6: Square mandrel. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] In a first aspect, the present invention provides a square core quartz optical fiber for laser transmission. Figure 1 Schematic diagram of the cross section and refractive index of a square core quartz optical fiber for laser transmission in one embodiment of the present invention; Figure 1 As shown, the square core quartz optical fiber for laser transmission includes a core layer 110, an inner cladding layer 210, an outer cladding layer 310 and a coating layer (not shown in the figure) which are concentrically arranged from the inside to the outside;
[0052] On a cross section perpendicular to the extension direction of the square core quartz optical fiber for laser transmission, the cross section of the core layer is in a square shape, the cross section of the inner cladding is in a square ring shape, and the cross section of the outer cladding is in a circular ring shape with a square through hole;
[0053] The verticality of the edge of the core layer is not greater than 1°, the concentricity of the core layer and the inner cladding is not greater than 0.25μm; the difference in the side length of the core layer is greater than 0.25μm; the corner radius of the core layer is not greater than 1.25μm.
[0054] The verticality of the edge of the core layer refers to the difference between the angles of the adjacent edges of the square core minus 90°, which can be obtained by high-magnification optical microscope testing;
[0055] The concentricity of the core layer and the inner cladding refers to the distance between the symmetrical center points of the cross-sectional shapes of the core layer 110 and the outer cladding 310, which can be obtained by testing with an optical microscope or a single-mode optical fiber geometry tester (such as PK2400 equipment);
[0056] The core length difference refers to the difference in the length of opposite sides in the square core, which is usually obtained by optical microscope or single-mode fiber geometry tester (such as PK2400 equipment);
[0057] Figure 2 is a schematic diagram of the corner radius of the core layer, such as Figure 2 As shown, the corner radius r of the core layer refers to the distance between the intersection point and the tangent point of the tangent lines of adjacent sides.
[0058] In the related art, the energy transfer optical fiber includes a core layer and a cladding layer, and the cladding layer is arranged around the core layer. The cross-sectional shape of the core layer is circular, and the cross-sectional shape of the cladding layer is circular. However, the energy of the light beam output by this energy transfer optical fiber presents a Gaussian distribution. When cutting materials, the Gaussian beam with highly concentrated energy can easily damage the cut plate, causing the expansion of the cutting heat affected zone, and then causing metal residues to splash and damage the laser output lens. For this reason, high-power lasers use different methods to forward the laser beam excited by the active optical fiber, so that the laser output through the energy transfer optical fiber is transformed from the original Gaussian beam to a flat-top beam, thereby improving the cutting quality of the high-power laser.
[0059] In order to solve the above problems, the present invention provides a square core quartz optical fiber for laser transmission with a square core and a circular shape, comprising a core layer, an inner cladding layer, an outer cladding layer and a coating layer which are concentrically arranged in sequence from the inside to the outside; on a cross section perpendicular to the extension direction of the square core quartz optical fiber for laser transmission, the cross section of the core layer is in a square shape, the cross section of the inner cladding layer is in a square ring shape, and the cross section of the outer cladding layer is in a circular ring shape with a square through hole; and by further limiting the verticality of the edge of the square core quartz optical fiber for laser transmission, the concentricity of the core layer and the inner cladding layer, the difference in the side length of the core layer, and the corner radius of the core layer, a square core quartz optical fiber for laser transmission with high geometric accuracy and uniform components can be obtained, which can realize light spot homogenization and stable transmission of laser energy, and is conducive to wide application in the fields of national defense, scientific research, industry, medical cosmetology, etc.
[0060] Furthermore, the numerical aperture of the square core quartz optical fiber for laser transmission is 0.06 to 0.22.
[0061] The numerical aperture of square core quartz optical fiber for laser transmission is an important parameter to measure its light receiving ability. It determines the maximum angle of light that the optical fiber can receive and has an impact on the efficiency and distance of optical fiber light transmission. The numerical aperture NA calculation formula is as follows:
[0062]
[0063] Where na is the refractive index of the core layer, and nb is the refractive index of the cladding layer.
[0064] Limiting the numerical aperture of square-core quartz optical fiber for laser transmission can further optimize the performance of the optical fiber in a specific application, ensuring that it can effectively transmit optical signals while meeting other system requirements such as coupling efficiency, transmission distance and bandwidth, and can further achieve spot homogenization and stable transmission of laser energy.
[0065] In a specific embodiment, a first difference Δn0 between the refractive index of the core layer and the refractive index of the outer cladding layer is 0 to 0.7%; a second difference Δn1 between the refractive index of the inner cladding layer and the refractive index of the outer cladding layer is -0.5 to -1.2%.
[0066] Among them, the first difference refers to the value Δn0 obtained by subtracting the refractive index of the outer cladding from the refractive index of the core layer, and the second difference refers to the value Δn1 obtained by subtracting the refractive index of the outer cladding from the refractive index of the inner cladding; by further limiting the difference between the refractive index of the core layer and the refractive index of the outer cladding, and the refractive index of the inner cladding and the refractive index of the outer cladding, better light spot homogenization and stable transmission of laser energy can be achieved.
[0067] Specifically, the refractive index profile of square-core silica optical fiber for laser transmission is a step-type distribution.
[0068] It should be noted that if Figure 1 As shown, on a cross section perpendicular to the extension direction of the square core quartz optical fiber for laser transmission, the side length R1 of the core layer is 20 to 600 μm;
[0069] The thickness R2 of the inner cladding is 1 to 50 μm;
[0070] The outer radius R3 of the outer cladding is 60 to 1000 μm.
[0071] By further limiting the side length R1 of the core layer, the thickness R2 of the inner cladding layer, and the outer radius R3 of the outer cladding layer, the homogenization effect of the square core quartz optical fiber for laser transmission on the light beam can be further improved, and the energy transmission is more stable.
[0072] In one embodiment, the core layer comprises silicon dioxide; the hydroxyl content of the core layer is no more than 1 ppm; the inner cladding layer comprises fluorine-doped silicon dioxide; and the outer cladding layer comprises silicon dioxide.
[0073] By limiting the material composition of the core layer, the inner cladding layer and the outer cladding layer, it is helpful to further reduce the loss of laser energy during transmission, and it is possible to further homogenize the light spot and stably transmit the laser energy.
[0074] In another embodiment, the core layer further comprises germanium oxide.
[0075] The inventors have found that when the core layer also includes germanium oxide, it is beneficial for the core layer to achieve a positive refractive index, which can further homogenize the light spot and stably transmit the laser energy.
[0076] Optionally, the coating layer includes an inner coating and an outer coating which are concentrically arranged in sequence; the inner coating is close to the outer cladding; the inner coating includes a polyacrylic acid resin with a refractive index of 1.36 to 1.42, and the outer coating includes a polyacrylic acid resin with a refractive index of 1.49 to 1.51.
[0077] The inventors have found that providing a concentrically arranged inner coating and outer coating outside the outer cladding can protect the optical fiber from mechanical damage, maintain the optical fiber's geometric shape and optical properties, thereby further improving the transmission performance of the optical fiber and reducing signal attenuation and distortion.
[0078] The refractive index of the polyacrylic acid resin of the inner coating layer can be further limited to 1.37 to 1.4.
[0079] In a second aspect, the present invention provides a method for preparing the square core quartz optical fiber for laser transmission according to the first aspect. Figure 3 FIG. 1 is a schematic diagram of a method for preparing a square core quartz optical fiber for laser transmission according to an embodiment of the present invention. Figure 3 As shown, the following steps are included:
[0080] (1) performing a first deposition process on the outer wall of the square target rod 1 to form a loose circular square core shell layer 2, and after the square target rod 1 is extracted, degassing and sintering the loose circular square core shell layer 2 to obtain an outer cladding precursor 4;
[0081] (2) performing a second deposition process on the inner wall of the outer cladding precursor 4 to form an inner cladding precursor 5, thereby obtaining a circular square core substrate tube;
[0082] (3) The square core rod 6 and the round square core base tube are assembled into a rod, and then drawn to obtain an optical fiber precursor;
[0083] (4) A coating layer is formed on the outer wall of the optical fiber precursor to obtain a square core silica optical fiber for laser transmission.
[0084] The preparation method provided by the present invention utilizes a square target rod to directly deposit thereon to obtain a loose circular square core shell layer, degassing and sintering to obtain an outer cladding precursor, and then depositing in the outer cladding precursor to obtain a circular square core base tube, and directly assembling and drawing the square core rod and the circular square core base tube to obtain an optical fiber precursor with high geometric accuracy, and after forming a coating layer, a square core quartz optical fiber for laser transmission can be obtained. The preparation method is simple and easy to implement, and can obtain a square core quartz optical fiber for laser transmission with homogenized light spots and stable transmission of laser energy.
[0085] The present invention does not limit the specific process parameters in the preparation method;
[0086] Optionally, in step (1), the square target rod 1 is mounted on a lathe, and reaction gases SiCl4, H2 and O2 are introduced through a flame torch 3, and a first deposition treatment is performed at a deposition rate of not less than 10 g / min, and the torch is moved back and forth to deposit layer by layer to form a loose circular square core shell layer 2, and after the square target rod 1 is extracted, the loose circular square core shell layer 2 is placed in a sintering furnace for degassing and sintering to obtain an outer cladding precursor 4;
[0087] In step (3), a circular SiO2 mother rod is first prepared by vapor axial deposition (VAD) or external vapor deposition (OVD) process, wherein the hydroxyl content of the mother rod is less than 1ppm, and the mother rod is extended to a diameter of 16 to 30mm, and a square core rod 6 is obtained by cold working and grinding process, and then the polished square core rod 6 and the circular square core substrate are pickled to remove interface impurities and defects, and then the sleeve rod assembly process is performed, and the sleeve rod assembly process adopts a vertical assembly method, which can effectively reduce interface scratches; the assembled sleeve rod is drawn, the drawing temperature is 1800 to 2200°C, the drawing speed is 5 to 20m / min, and the outer diameter of the optical fiber precursor after drawing is not more than 1.5mm;
[0088] In step (4), the inner coating layer adopts a low-refractive-index polyacrylic resin coating, and the outer coating layer adopts a high-refractive-index polyacrylic resin. After being cured by ultraviolet or LED, a square-core quartz optical fiber for laser transmission is obtained.
[0089] In a specific embodiment, a first deposition process is performed on the outer wall of the square target rod by vapor axial deposition or external vapor deposition to form a loose circular square core shell layer with a thickness of not less than 60 mm, and after the square target rod is extracted, the loose circular square core shell layer is degassed and sintered to obtain an outer cladding precursor with an outer diameter of 30 to 45 mm;
[0090] Performing a second deposition process on the inner wall of the outer cladding precursor by chemical vapor deposition (MCVD) or plasma vapor deposition (PCVD) to form an inner cladding precursor with a thickness of 1.5 to 5 mm;
[0091] The rod assembly process adopts vertical assembly, and the gap between the outer wall of the square core rod and the inner wall of the round square core base tube is 0.5-1.5mm;
[0092] The square target rod is at least one of aluminum oxide, zirconium oxide, and aluminum nitride; the surface roughness of the square target rod is not greater than 0.6 μm;
[0093] The hydroxyl content of the square core rod is not greater than 1 ppm, and the surface roughness is not greater than 0.3 μm.
[0094] In a third aspect, the present invention provides a fiber laser, comprising a fiber laser body and the square-core quartz fiber for laser transmission of the first aspect or the square-core quartz fiber for laser transmission prepared by the preparation method of the second aspect connected to the fiber laser body.
[0095] Hereinafter, a square core quartz optical fiber for laser transmission provided by the present invention is introduced in detail through specific embodiments.
[0096] Example 1
[0097] The method for preparing square core quartz optical fiber for laser transmission comprises the following steps:
[0098] (1) A square target rod is mounted on a VAD lathe, and reaction gases SiCl4, H2 and O2 are introduced through a flame torch, and a first deposition process is performed at a deposition rate of 10 g / min. The torch is moved back and forth to deposit layer by layer to form a loose circular square core shell layer. After the target rod is withdrawn, the loose circular square core shell layer is placed in a sintering furnace for degassing and sintering to obtain an outer cladding precursor with an outer diameter of 35 mm and an inner hole diameter of 12.9 mm; wherein the outer cladding precursor comprises high-purity quartz glass, and the surface roughness of the square target rod is 0.3 μm but not more than 0.6 μm;
[0099] (2) performing a second deposition process on the inner wall of the outer cladding precursor by a PCVD process to form an inner cladding precursor with a thickness of 0.266 mm, thereby obtaining a circular square core substrate tube; wherein the inner cladding precursor comprises fluorine-doped silica;
[0100] (3) a circular SiO2 mother rod is first prepared by a vapor axial deposition (VAD) or an outside vapor deposition (OVD) process, wherein the hydroxyl content of the mother rod is 0.8 ppm, the mother rod is extended to a diameter of 16 to 30 mm, and a square core rod with a side length of 8 mm is obtained by a cold working and grinding process; wherein the square core rod comprises 97% silicon oxide and 3% germanium oxide, and the surface roughness of the square core rod is 0.2 μm and not more than 0.3 μm;
[0101] (4) The polished square core rod and the round square core base tube are pickled to remove interface impurities and defects, and then the sleeve rod assembly process is performed. The sleeve rod assembly process adopts a vertical assembly method, and the gap between the outer wall of the square core rod and the inner wall of the round square core base tube is 1 mm; the assembled sleeve rod is drawn, the drawing temperature is 1950° C., the drawing speed is 20 m / min, and the outer diameter of the optical fiber precursor after drawing is 125 μm;
[0102] (5) A coating layer is formed on the outer wall of the optical fiber precursor, wherein the inner coating layer comprises a polyacrylic acid resin with a refractive index of 1.37 and the outer coating layer comprises a polyacrylic acid resin with a refractive index of 1.51, thereby obtaining a square core quartz optical fiber for laser transmission.
[0103] Example 2
[0104] The method for preparing square core quartz optical fiber for laser transmission comprises the following steps:
[0105] (1) A square target rod is mounted on an OVD lathe, and reaction gases SiCl4, H2 and O2 are introduced through a flame torch to perform a first deposition process at a deposition rate of 10 g / min. The torch is moved back and forth to deposit layer by layer to form a loose circular square core shell layer. After the target rod is removed, the loose circular square core shell layer is placed in a sintering furnace for degassing and sintering to obtain an outer cladding precursor with an outer diameter of 35 mm and an inner hole diameter of 18.9 mm; wherein the outer cladding precursor comprises high-purity quartz glass;
[0106] (2) performing a second deposition process on the inner wall of the outer cladding precursor by a PCVD process to form an inner cladding precursor with a thickness of 1.55 mm, thereby obtaining a circular square core substrate tube; wherein the inner cladding precursor comprises fluorine-doped silica;
[0107] (3) a circular SiO2 mother rod prepared by a vapor axial deposition (VAD) or an outside vapor deposition (OVD) process, wherein the hydroxyl content of the mother rod is 0.8 ppm, the mother rod is extended to a diameter of 16 to 30 mm, and a square core rod with a side length of 14 mm is obtained by a cold working and grinding process; wherein the square core rod comprises silicon dioxide;
[0108] (4) The polished square core rod and the round square core base tube are pickled to remove interface impurities and defects, and then the sleeve rod assembly process is performed. The sleeve rod assembly process adopts a vertical assembly method, and the assembled sleeve rod is drawn. The drawing temperature is 1980° C., the drawing speed is 10 m / min, and the outer diameter of the optical fiber precursor after drawing is 600 μm;
[0109] (5) A coating layer is formed on the outer wall of the optical fiber precursor, wherein the inner coating layer comprises a polyacrylic acid resin with a refractive index of 1.37 and the outer coating layer comprises a polyacrylic acid resin with a refractive index of 1.51, thereby obtaining a square core quartz optical fiber for laser transmission.
[0110] Example 3
[0111] The method for preparing square core quartz optical fiber for laser transmission comprises the following steps:
[0112] (1) A square target rod is mounted on a VAD lathe, and reaction gases SiCl4, H2 and O2 are introduced through a flame torch. A first deposition process is performed at a deposition rate of 10 g / min. The torch is moved back and forth to deposit layer by layer to form a loose circular square core shell layer. After the target rod is removed, the loose circular square core shell layer is placed in a sintering furnace for degassing and sintering to obtain an outer cladding precursor with an outer diameter of 35 mm and an inner hole diameter of 20.7 mm; wherein the outer cladding precursor comprises high-purity quartz glass;
[0113] (2) performing a second deposition process on the inner wall of the outer cladding precursor by a PCVD process to form an inner cladding precursor with a thickness of 0.37 mm, thereby obtaining a circular square core substrate tube; wherein the inner cladding precursor comprises fluorine-doped silica;
[0114] (3) a circular SiO2 mother rod prepared by a vapor axial deposition (VAD) or an outside vapor deposition (OVD) process, wherein the hydroxyl content of the mother rod is 0.8 ppm, the mother rod is extended to a diameter of 16 to 30 mm, and a square core rod with a side length of 12 mm is obtained by a cold working and grinding process; wherein the square core rod comprises silicon dioxide;
[0115] (4) The polished square core rod and the round square core base tube are pickled to remove interface impurities and defects, and then the sleeve rod assembly process is performed. The sleeve rod assembly process adopts a vertical assembly method, and the assembled sleeve rod is drawn. The drawing temperature is 2040° C., the drawing speed is 8 m / min, and the outer diameter of the optical fiber precursor after drawing is 600 μm;
[0116] (5) A coating layer is formed on the outer wall of the optical fiber precursor, wherein the inner coating layer comprises a polyacrylic acid resin with a refractive index of 1.37 and the outer coating layer comprises a polyacrylic acid resin with a refractive index of 1.51, thereby obtaining a square core quartz optical fiber for laser transmission.
[0117] Comparative Example 1
[0118] The difference between this comparative example and Example 2 is that in step (2), a capillary tube with a diameter of 1.55 mm is used to fill one circle along the inner wall of the outer cladding precursor to obtain a circular square core substrate tube.
[0119] Test Example 1
[0120] The square core quartz optical fibers for laser transmission prepared in the above embodiments and comparative examples were tested for their limb perpendicularity, concentricity of the core layer and the inner cladding (referred to as core-cladding concentricity), core layer side length difference (referred to as square core side length difference), and core layer corner radius r. The typical attenuation value at a wavelength of 1550 nm was tested by OTDR (optical time domain reflectometer). The test results are shown in Table 1.
[0121] Table 1
[0122]
[0123]
[0124] The invention provides a square core quartz optical fiber for laser transmission, which comprises a core layer, an inner cladding layer, an outer cladding layer and a coating layer which are concentrically sleeved in sequence from the inside to the outside. On a cross section perpendicular to the extension direction of the square core quartz optical fiber for laser transmission, the cross section of the core layer is in a square shape, the cross section of the inner cladding layer is in a square ring shape, and the cross section of the outer cladding layer is in a ring shape with a square through hole. By further limiting the verticality of the edge of the square core quartz optical fiber for laser transmission, the concentricity of the core layer and the inner cladding layer, the difference in the side length of the core layer, and the corner radius of the core layer, the square core quartz optical fiber for laser transmission with high geometric accuracy and uniform components can be obtained, and light spot homogenization and stable transmission of laser energy can be achieved, which is conducive to wide application in the fields of national defense, scientific research, industry, medical cosmetology, etc.
[0125] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A square core quartz optical fiber for laser transmission, It is characterized in that It includes a core layer, an inner cladding layer, an outer cladding layer and a coating layer which are concentrically arranged from the inside to the outside; On a cross section perpendicular to the extension direction of the square core quartz optical fiber for laser transmission, the cross section of the core layer is in a square shape, the cross section of the inner cladding is in a square ring shape, and the cross section of the outer cladding is in a circular ring shape with a square through hole; The verticality of the edge of the core layer is not greater than 1°, the concentricity of the core layer and the inner cladding is not greater than 0.25 μm; the difference in the side length of the core layer is not greater than 0.25 μm; and the corner radius of the core layer is not greater than 1.25 μm.
2. The square core quartz optical fiber for laser transmission according to claim 1, It is characterized in that The numerical aperture of the square core quartz optical fiber for laser transmission is 0.06-0.
22.
3. The square core quartz optical fiber for laser transmission according to claim 1 or 2, It is characterized in that A first difference between the refractive index of the core layer and the refractive index of the outer cladding layer is 0 to 0.7%; and / or, A second difference between the refractive index of the inner cladding and the refractive index of the outer cladding is -0.5 to -1.2%.
4. The square core quartz optical fiber for laser transmission according to any one of claims 1 to 3, It is characterized in that On a cross section perpendicular to the extending direction of the square core quartz optical fiber for laser transmission, the side length of the core layer is 20 to 600 μm; and / or, The thickness of the inner cladding is 1 to 50 μm; and / or, The outer radius of the outer cladding is 60-1000 μm.
5. The square core quartz optical fiber for laser transmission according to any one of claims 1 to 4, It is characterized in that The core layer comprises silicon dioxide; and / or, The hydroxyl content of the core layer is not more than 1 ppm; and / or, The inner cladding comprises fluorine-doped silicon dioxide; and / or, The outer cladding includes silicon dioxide.
6. The square core quartz optical fiber for laser transmission according to any one of claim 5, It is characterized in that The core layer also includes germanium oxide.
7. The square core quartz optical fiber for laser transmission according to any one of claims 1 to 6, It is characterized in that The coating layer comprises an inner coating layer and an outer coating layer which are concentrically arranged in sequence; the inner coating layer is close to the outer coating layer; The inner coating layer includes a polyacrylic acid resin having a refractive index of 1.36 to 1.42, and the outer coating layer includes a polyacrylic acid resin having a refractive index of 1.49 to 1.
51.
8. A method for preparing the square core quartz optical fiber for laser transmission according to any one of claims 1 to 7, It is characterized in that The following steps are involved: (1) performing a first deposition process on the outer wall of a square target rod to form a loose circular square core-shell layer, and after extracting the square target rod, degassing and sintering the loose circular square core-shell layer to obtain an outer cladding precursor; (2) performing a second deposition process on the inner wall of the outer cladding precursor to form an inner cladding precursor, thereby obtaining a circular square core substrate tube; (3) assembling the square core rod and the circular square core base tube into a rod-enclosed manner, and then performing a drawing process to obtain an optical fiber precursor; (4) forming a coating layer on the outer wall of the optical fiber precursor to obtain the square core silica optical fiber for laser transmission.
9. The preparation method according to claim 8, It is characterized in that A first deposition process is performed on the outer wall of the square target rod by vapor axial deposition or external vapor deposition to form the loose circular square core shell layer with a thickness of not less than 60 mm, and after the square target rod is extracted, the loose circular square core shell layer is degassed and sintered to obtain the outer cladding precursor with an outer diameter of 30 to 45 mm; and / or, Performing a second deposition process on the inner wall of the outer cladding precursor by chemical vapor deposition or plasma vapor deposition to form the inner cladding precursor with a thickness of 1.5 to 5 mm; and / or, The rod assembly process adopts vertical assembly, and the gap between the outer wall of the square core rod and the inner wall of the circular square core base tube is 0.5-1.5 mm; and / or, The square target rod is at least one of aluminum oxide, zirconium oxide, and aluminum nitride; the surface roughness of the square target rod is not greater than 0.6 μm; and / or, The square core rod has a hydroxyl content of no greater than 1 ppm and a surface roughness of no greater than 0.3 μm.
10. A fiber laser, It is characterized in that The invention comprises a fiber laser body and a square core quartz optical fiber for laser transmission as claimed in any one of claims 1 to 7 or a square core quartz optical fiber for laser transmission prepared by the preparation method as claimed in any one of claims 8 to 9 connected to the fiber laser body.
Citation Information
Patent Citations
Square core optical fiber and preparation method thereof
CN108975675A
Energy homogenizing optical fiber and preparation method thereof
CN111983748A
Preparation method of square energy-transmitting optical fiber preform and optical fiber preform
CN118270974A
Optical fiber and mode scrambler provided therewith
WO2009104350A1
Cited By
Square-core quartz fiber for laser transmission and preparation method therefor, and fiber laser
WO2026036680A1