Production process for preparing copper-chromium-zirconium contact wire by up-drawing method

The melting furnace and inert gas vortex protection process connected through the undercurrent channel solve the problems of high equipment investment and high energy consumption in the preparation of copper-chromium-zirconium contact wires, and realize the continuous preparation of large roll weight and long-size copper-chromium-zirconium contact wires. , simplify the process flow and improve performance and composition uniformity.

CN118942794APending Publication Date: 2024-11-12FUJIKURA HENGTONG AERIAL CABLE SYST
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410994436.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing copper chromium zirconium contact line preparation process has problems such as high equipment investment, large energy consumption, complex process and uneven composition in the production of large coil weights and long sizes, which is difficult to meet the performance requirements of high-speed railway contact line.

Method used

The melting furnace, transition furnace and insulation furnace connected to the undercurrent channel are adopted to realize the continuous preparation of copper-chromium-zirconium alloy through the inert gas vortex protection process, simplify the process flow and reduce costs.

Benefits of technology

The continuous preparation of large roll weight and long-size copper-chromium zirconium contact wires is realized, the process flow is simplified, the cost is reduced, the composition uniformity and performance is improved, oxygen is avoided, and the yield of zirconium is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942794A_ABST
    Figure CN118942794A_ABST
Patent Text Reader

Abstract

The invention discloses a production process for preparing a copper-chromium-zirconium contact wire by an up-drawing method, which comprises the following steps of: adding cathode copper into a melting furnace for melting, and sequentially adding copper-chromium, copper-magnesium and copper-zirconium intermediate alloys to obtain a copper alloy melt; the copper alloy melt is buffered by the transition furnace and then enters a heat preservation furnace for up-drawing continuous casting of a copper-chromium-zirconium blank rod; and the copper-chromium-zirconium blank rod is subjected to extrusion, water seal solid solution, annealing and drawing to obtain the copper-chromium-zirconium contact wire. Charcoal covers the melts of the melting furnace and the transition furnace, graphite flakes cover the melts of the heat preservation furnace, and inert gas protection devices are arranged at furnace mouths of the melting furnace, the transition furnace and the heat preservation furnace to form inert gas vortexes at the furnace mouths. The copper-chromium-zirconium contact wire is prepared by adopting an up-drawing method, the process is simple, the flow is short, the cost is low, and continuous preparation of the copper-chromium-zirconium contact wire with large coil weight and long size can be realized; inert gas vortexes are manufactured at the furnace mouth, so that oxygen is prevented from entering in the feeding and up-drawing process, and the yield of the zirconium element is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper-chromium-zirconium contact wires, and in particular to a production process for preparing copper-chromium-zirconium contact wires by an up-drawing method. Background Art

[0002] With the development of science and technology, the operating speed of high-speed railways is expected to increase to more than 400 kilometers per hour in the future. The performance of the existing Cu-Ag, Cu-Sn and Cu-Mg contact wires is difficult to meet the requirements, so it is necessary to use copper-chromium-zirconium alloy contact wires with high strength and high conductivity. For copper-chromium-zirconium contact wires, the current mainstream preparation processes are: vacuum casting-rolling-drawing method, vacuum vertical semi-continuous casting-hot processing blanking-drawing method, vacuum casting-water seal extrusion-drawing method.

[0003] For the vacuum melting-rolling-drawing method, the equipment investment required for this process is relatively low, so it is more suitable for small-scale and small-batch wire manufacturing. However, it is difficult to achieve continuous large-scale production of large coil weights and long wires. In addition, the ingots produced by this process have problems such as uneven composition and loose structure. These problems are difficult to be completely solved in the subsequent cold working process, which ultimately affects the overall performance of the wire products.

[0004] For the vacuum vertical semi-continuous casting-hot processing billet-drawing method, when manufacturing heavy coils and long-distance wires, it is necessary to rely on large vacuum melting furnaces and hot processing facilities, while the energy consumption is high and the metal loss during the processing is also large. After the hot processing is completed, the surface pickling treatment is also required, which not only increases the complexity of the process flow, but also puts great pressure on the environment.

[0005] For the vacuum melting-water seal extrusion-drawing method, the two steps of extrusion molding and solution quenching are combined into one, simplifying the production process of copper-chromium-zirconium alloy contact wire. However, when producing heavy coils and long-sized wires, this technology also requires the use of large vacuum melting furnaces and large water seal extruders, which not only means a higher initial investment, but also comes with greater energy consumption and higher process control difficulty.

[0006] For a single contact wire with a length greater than 1500 meters, the cross-sectional area is 150mm 2 For example, a copper alloy contact wire weighing about 2 tons needs to be prepared. At the same time, in order to ensure the performance of the contact wire, its composition must be kept uniform over the entire length, so it is of great significance to develop a low-cost and efficient preparation and processing technology for high-performance copper-chromium-zirconium alloy contact wire. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a production process for preparing copper-chromium-zirconium contact wire by the upward drawing method, which adopts a melting furnace, a transition furnace and a holding furnace connected by a submerged flow channel, and creates an inert gas vortex at the furnace mouth to avoid the entry of oxygen during the feeding process. The process has low cost and can realize the continuous preparation of large coil weight and long-sized copper-chromium-zirconium contact wire.

[0008] In order to solve the above technical problems, the present invention provides a production process for preparing copper-chromium-zirconium contact wire by an up-drawing method, comprising the following steps:

[0009] S1, adding cathode copper to a melting furnace and heating it to 1145-1300° C. to melt, adding a copper-chromium master alloy to the melting furnace, and after the copper-chromium master alloy is melted, sequentially adding copper-magnesium and copper-zirconium master alloys to the melting furnace to obtain a copper alloy melt;

[0010] S2, the copper alloy melt enters the transition furnace for buffering through the first submerged flow channel, and then enters the holding furnace through the second submerged flow channel to be drawn into the continuous casting copper-chromium-zirconium blank rod;

[0011] S3, the copper-chromium-zirconium blank rod is extruded, water-sealed solid solution, annealed, and drawn to obtain a copper-chromium-zirconium contact wire;

[0012] The melt in the melting furnace and transition furnace is covered with charcoal, and the melt in the holding furnace is covered with graphite flakes. An inert gas protection device is arranged at the furnace mouth of the melting furnace, transition furnace and holding furnace to form an inert gas vortex at the furnace mouth.

[0013] The present invention completes the continuous addition and melting of copper plates and intermediate alloys through a melting furnace. In the melting channel area, the charge is melted and continuously tumbles in the channel. The melted copper alloy melt flows to the transition furnace and the holding furnace in sequence through the undercurrent channel between the two furnaces. The transition furnace buffers the melt flow impact in the melting furnace to prevent the melt from directly entering the holding furnace, which causes the copper liquid level to fluctuate violently due to the addition of charge to the melting furnace. The holding furnace controls the temperature of the copper liquid in the furnace, and at the same time, the copper alloy liquid is continuously solidified and crystallized into a wire rod through a crystallizer. The circulation of copper liquid between the three furnaces is controlled by the undercurrent channel, so that the continuous preparation of large coil weight and long-sized copper-chromium-zirconium contact wire can be achieved. Charcoal is covered in the melting furnace and the transition furnace, and graphite flakes are covered in the holding furnace. Charcoal is burned while the melting furnace is added to reduce the entry of oxygen. The holding furnace isolates the air through the graphite flakes, and an inert gas vortex is created above the furnace mouths of the three furnace bodies to further reduce the entry of oxygen.

[0014] The invention adds copper-magnesium and copper-zirconium master alloys, which are lower in price than copper-magnesium-zirconium master alloys, and are more convenient to control the content of each component (Mg content, Cr content and Zr content) in the copper liquid; in the invention, the Zr element is introduced through the Cu-Zr alloy, but Zr is easily burned by reacting with oxygen; the invention firstly adds the Cu-Mg master alloy to consume a part of the oxygen in the copper liquid, and then adds the Cu-Zr master alloy to reduce the burning of the Zr element, thereby improving the recovery rate of Zr.

[0015] Furthermore, the inert gas protection device includes a plurality of jet pipes, which are connected to an inert gas source, the outlets of the jet pipes are located at the furnace mouth and the outlets of all the jet pipes are uniformly bent in a clockwise or counterclockwise direction so that the ejected gas forms a clockwise or counterclockwise vortex, and the angle of the jet pipe after bending is 110°-130°.

[0016] Furthermore, the air injection pipe is a stainless steel pipe.

[0017] Furthermore, the mass percentage of magnesium in the copper-magnesium master alloy is 15wt%-20wt%, the mass percentage of chromium in the copper-chromium master alloy is 6wt%-10wt%, and the mass percentage of zirconium in the copper-zirconium master alloy is 12wt%-20wt%.

[0018] Furthermore, the copper-magnesium, copper-chromium and copper-zirconium master alloys are all added to the melting furnace in a copper foil wrapping manner. The copper foil wrapping manner is convenient for feeding, and for the copper-magnesium master alloy, the flash of magnesium is temporarily delayed by the copper foil wrapping.

[0019] Furthermore, the components of the copper-chromium-zirconium contact wire and their mass percentages are: 0.1wt% to 1.5wt% Cr, 0.02wt% to 0.2wt% Zr, impurities <0.15wt%, and the balance is copper.

[0020] Furthermore, the casting speed of the upward continuous casting is 450-550 mm / min, and the diameter of the blank rod is 20-25 mm.

[0021] Furthermore, during the upward continuous casting process, the alloy composition is detected regularly and alloy compensation is performed when necessary.

[0022] Furthermore, the extrusion temperature is 500-550° C., and the diameter of the blank rod after extrusion is 25-28 mm.

[0023] Furthermore, the water-sealed solid solution treatment is specifically as follows: the extruded blank rod is heated to 900-950° C. and kept warm for 1-2 hours, and then placed in water at 20-30° C. for 30-60 minutes.

[0024] Furthermore, the annealing temperature is 400-500° C., and the annealing time is 2-4 hours.

[0025] Furthermore, the drawing passes are 5 times, the processing rate of each pass is 15-30%, and the total processing rate is 60-70%.

[0026] Furthermore, the first drawing pass is a round die, and the next four drawing passes are slotted heteromorphic dies.

[0027] Beneficial effects of the present invention:

[0028] The present invention adopts the up-drawing method to prepare the copper-chromium-zirconium contact wire. Compared with vacuum melting, the process is simple, the flow is short, the cost is low, and the continuous preparation of large coil weight and long-sized copper-chromium-zirconium contact wire can be achieved.

[0029] The present invention creates an inert gas vortex at the furnace mouth to avoid the entry of oxygen during the feeding and upward drawing processes. At the same time, copper-magnesium alloy is added in advance to consume part of the oxygen in the copper liquid, thereby improving the recovery rate of the zirconium element. Compared with the copper-magnesium-zirconium master alloy, the addition of copper-magnesium and copper-zirconium master alloy has low cost and is convenient for controlling the alloy composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a production device for preparing copper-chromium-zirconium contact wire by the up-drawing method of the present invention;

[0031] Figure 2 It is a schematic structural diagram of a melting furnace, a transition furnace and a holding furnace of the present invention;

[0032] Figure 3 This is a schematic diagram of the jet pipe bending;

[0033] Explanation of the numbers in the figure: 1. melting furnace, 2. transition furnace, 3. holding furnace, 4. heating coil, 5. first undercurrent channel, 6. second undercurrent channel, 7. charcoal, 8. graphite flakes, 9. jet pipe, 10. melt. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0035] This embodiment relates to a production process for preparing a copper-chromium-zirconium contact wire by an up-drawing method, comprising the following steps:

[0036] S1. Add cathode copper into a melting furnace and heat it to 1145-1300°C for melting, add a copper-magnesium master alloy into the melting furnace, and after the copper-magnesium master alloy is melted, add copper-chromium and copper-zirconium master alloys into the melting furnace in sequence to obtain a copper alloy melt; S2. The copper alloy melt enters a transition furnace for buffering through a first undercurrent channel, and then enters a holding furnace through a second undercurrent channel to be drawn into a continuous casting copper-chromium-zirconium blank rod; S3. The copper-chromium-zirconium blank rod is extruded, water-sealed for solid solution, annealed, and drawn to obtain a copper-chromium-zirconium contact wire.

[0037] Preferably, the mass percentage of magnesium in the copper-magnesium master alloy is 15wt% to 20wt%, the mass percentage of chromium in the copper-chromium master alloy is 6wt% to 10wt%, and the mass percentage of zirconium in the copper-zirconium master alloy is 12wt% to 20wt%; the copper-magnesium, copper-chromium, and copper-zirconium master alloys are all added to the melting furnace in the form of copper foil wrapping. The components and mass percentages of the copper-chromium-zirconium contact wire are: 0.1wt% to 1.5wt% Cr, 0.02wt% to 0.2wt% Zr, impurities <0.15wt%, and the balance is copper.

[0038] Preferably, the casting speed of the upward continuous casting is 450-550mm / min, the diameter of the blank rod is 20-25mm, and during the upward continuous casting, the alloy composition is regularly detected and alloy compensation is performed when necessary; the extrusion temperature is 500-550℃, and the diameter of the blank rod after extrusion is 25-28mm; the water seal solution treatment is specifically as follows: the extruded blank rod is heated to 900-950℃ and kept warm for 1-2h, and then placed in water at 20-30℃ for 30-60min; the annealing temperature is 400-500℃, and the annealing time is 2-4h; the drawing passes are 5 times, the processing rate of each pass is 15-30%, and the total processing rate is 60-70%.

[0039] The production equipment used in the production process of preparing copper-chromium-zirconium contact wire by the up-drawing method in this embodiment is as follows: Figure 1 and Figure 2 As shown, it includes a melting furnace 1, a transition furnace 2 and a holding furnace 3. A heating coil 4 is arranged at the bottom of each furnace body. A first undercurrent channel 5 is arranged between the melting furnace 1 and the transition furnace 2. A second undercurrent channel 6 is arranged between the transition furnace 2 and the holding furnace 3. Charcoal 7 is covered above the melt 10 of the melting furnace 1 and the transition furnace 2. Charcoal 7 is added to the melting furnace 1. Figure 2As shown by the arrow, continuous casting is conducted on the holding furnace 3, and the melt 10 of the holding furnace 3 is covered with graphite flakes 8. Inert gas protection devices are provided at the furnace openings of the melting furnace 1, transition furnace 2, and holding furnace 3 to form an inert gas vortex at the furnace openings. The inert gas protection devices include a plurality of jet pipes 9, which are connected to an inert gas source (not marked in the figure). The outlets of the jet pipes 9 are located at the furnace opening, and the outlets of all the jet pipes 9 are uniformly bent in a clockwise or counterclockwise direction so that the ejected gas forms a clockwise or counterclockwise vortex as shown in FIG. Figure 1 As shown by the arrow, the angle of the jet pipe 9 after bending is θ=120°. Figure 3 As shown, the air injection pipe is a stainless steel pipe.

[0040] Example 1

[0041] This embodiment 1 relates to a production process for preparing a copper-chromium-zirconium contact wire by an up-drawing method, using the above Figure 1 The production equipment in the production process includes the following steps:

[0042] (1) adding high-purity cathode copper to the melting furnace in the upper lead furnace for smelting at a smelting temperature of 1245° C. covering the surface of the melting furnace and the transition furnace with dried charcoal, and covering the surface of the holding furnace with graphite flakes. At the same time, turning on the argon gas injection device at the furnace mouth to form an argon gas vortex at the furnace mouth to isolate the entry of oxygen during the feeding and upper lead;

[0043] (2) adding a Cu-6wt% Cr master alloy until it is completely melted, and then sequentially adding a Cu-20wt% Mg and a Cu-12wt% Zr master alloy, stirring and then standing for a period of time to keep the temperature, measuring the Cr and Zr alloy compositions and adjusting them to not less than 0.2wt% Cr and 0.02wt% Zr, and adjusting the Mg content to not more than 0.2wt%, with the remainder being Cu and some unavoidable impurities;

[0044] (3) After being buffered in the transition furnace, the melt enters the holding furnace, and the crystallizer is inserted into the copper liquid in the holding furnace at a depth of 40 mm. The solution temperature is maintained at about 1200° C. and the upper drawing and pulling out is started at a speed of 450 mm / min. During the pulling process, the alloy composition is measured every half an hour, and the Cu-20wt% Mg and Cu-12wt% Zr master alloys are compensated on time to obtain an upper drawing rod blank with a diameter of 20 mm;

[0045] (4) After preheating the extrusion tooling die at 550°C for 2 hours in advance, the upper rod blank is continuously extruded to obtain an extruded rod with a rod diameter of 25.5 mm. The extruded rod is heated to 950°C and kept warm for 1 hour, then placed in 25°C water for water seal solution treatment, and then annealed at 400°C for 2 hours to obtain an annealed billet;

[0046] (5) The annealed billet is continuously drawn for 5 times to finally obtain a copper-chromium-zirconium contact wire.

[0047] The copper-chromium-zirconium contact wire prepared in Example 1 was subjected to a performance test. The tensile strength of the copper-chromium-zirconium contact wire was 581 MPa, and the electrical conductivity was 79% IACS.

[0048] In summary, the present invention adopts the upward drawing method to prepare copper-chromium-zirconium contact wire. Compared with vacuum smelting, the process is simple, the process is short, and the cost is low. It can also realize the continuous preparation of large coil weight and long-sized copper-chromium-zirconium contact wires. The copper-chromium-zirconium contact wires have excellent tensile strength and conductivity. By creating an inert gas vortex at the furnace mouth, the entry of oxygen during the feeding and upward drawing process is avoided. At the same time, copper-magnesium alloy is added in advance to consume part of the oxygen in the copper liquid, thereby increasing the yield of zirconium element. Compared with copper-magnesium-zirconium intermediate alloy, adding copper-magnesium and copper-zirconium intermediate alloy is low in cost and convenient for controlling the alloy composition.

[0049] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A production process for preparing copper-chromium-zirconium contact wire by up-drawing method, characterized in that: The steps include: S1, adding cathode copper to a melting furnace and heating it to 1145-1300° C. to melt, adding a copper-chromium master alloy to the melting furnace, and after the copper-chromium master alloy is melted, sequentially adding copper-magnesium and copper-zirconium master alloys to the melting furnace to obtain a copper alloy melt; S2, the copper alloy melt enters the transition furnace for buffering through the first submerged flow channel, and then enters the holding furnace through the second submerged flow channel to be drawn into the continuous casting copper-chromium-zirconium blank rod; S3, the copper-chromium-zirconium blank rod is extruded, water-sealed solid solution, annealed, and drawn to obtain a copper-chromium-zirconium contact wire; The melt in the melting furnace and transition furnace is covered with charcoal, and the melt in the holding furnace is covered with graphite flakes. An inert gas protection device is arranged at the furnace mouth of the melting furnace, transition furnace and holding furnace to form an inert gas vortex at the furnace mouth.

2. The production process for preparing copper-chromium-zirconium contact wire by the up-drawing method according to claim 1, characterized in that: The inert gas protection device comprises a plurality of jet pipes, wherein the jet pipes are connected to an inert gas source, outlets of the jet pipes are located at the furnace mouth and outlets of all the jet pipes are uniformly bent in a clockwise or counterclockwise direction, and the angle of the jet pipes after bending is 110°-130°.

3. The production process for preparing copper-chromium-zirconium contact wire by the up-drawing method according to claim 1, characterized in that: The mass percentage of magnesium in the copper-magnesium master alloy is 15wt%-20wt%, the mass percentage of chromium in the copper-chromium master alloy is 6wt%-10wt%, and the mass percentage of zirconium in the copper-zirconium master alloy is 12wt%-20wt%.

4. The production process for preparing copper-chromium-zirconium contact wire by the up-drawing method according to claim 1, characterized in that: The copper-magnesium, copper-chromium and copper-zirconium master alloys are all added to the melting furnace in a copper foil-wrapped manner.

5. The production process for preparing copper-chromium-zirconium contact wire by up-drawing method according to claim 1, characterized in that: The components of the copper-chromium-zirconium contact wire and their mass percentages are: 0.1wt%-1.5wt% Cr, 0.02wt%-0.2wt% Zr, impurities <0.15wt%, and the balance is copper.

6. The production process for preparing copper-chromium-zirconium contact wire by up-drawing method according to claim 1, characterized in that: The casting speed of the upward continuous casting is 450-550 mm / min, and the diameter of the blank rod is 20-25 mm.

7. The production process for preparing copper-chromium-zirconium contact wire by up-drawing method according to claim 1, characterized in that: The extrusion temperature is 500-550° C., and the diameter of the blank rod after extrusion is 25-28 mm.

8. The production process for preparing copper-chromium-zirconium contact wire by up-drawing method according to claim 1, characterized in that: The water-sealed solid solution method is specifically as follows: the extruded blank rod is heated to 900-950° C. and kept warm for 1-2 hours, and then placed in water at 20-30° C. for 30-60 minutes.

9. The production process for preparing copper-chromium-zirconium contact wire by up-drawing method according to claim 1, characterized in that: The annealing temperature is 400-500° C., and the annealing time is 2-4 hours.

10. The production process for preparing copper-chromium-zirconium contact wire by up-drawing method according to claim 1, characterized in that: The drawing passes are 5 times, the processing rate of each pass is 15-30%, and the total processing rate is 60-70%.

Citation Information

Cited By

  • Cu-Cr-X alloy contact wire and preparation method thereof

    CN120866686A