High-heat-dissipation wear-resistant transparent conductive film and preparation method thereof

By adding specific ingredients to the aqueous solution of ethylenediaminetetraacetic acid and ultrasonic cleaning, coating and high-temperature treatment, C/MgZnO:Al transparent conductive composite film was prepared, which solved the problem of insufficient toxicity and conductivity of the existing ZnO film, and realized the High heat dissipation, wear-resistant, non-toxic and low-cost transparent conductive film.

CN118942795APending Publication Date: 2024-11-12方宇航
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410995680.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Among the existing transparent conductive film materials, the In element used in the In2O3:Sn(ITO) film is expensive and rare, and the ZnO film prepared by the sol-gel method has problems of toxicity and insufficient conductivity.

Method used

The C/MgZnO:Al transparent conductive composite film is prepared by adding zinc acetate, magnesium acetate, alumina and glucose to the aqueous solution of ethylenediaminetetraacetic acid, and the C/MgZnO:Al transparent conductive composite film is prepared by ultrasonic cleaning, coating, vacuum high-temperature treatment and high-temperature annealing, forming a multi-layer Structure to improve conductivity and wear resistance.

Benefits of technology

It realizes transparent conductive films with high heat dissipation, wear resistance, non-toxicity and low cost, which improves the conductive performance and service life, while reducing the toxicity and pollution risks of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-heat-dissipation wear-resistant transparent conductive film and a preparation method thereof, and relates to the technical field of conductive film materials. Zinc acetate is utilized to inhibit solid phase diffusion and improve the film quality, then aluminum oxide is used for replacing Zn crystal lattices, the carrier concentration is increased, the resistance is reduced, and magnesium acetate is combined to increase the forbidden band width of the film, so that the film has higher visible light transmittance; glucose is used as a carbon source, is decomposed at a high temperature and uniformly coats the surfaces of metal ions, so that better conductivity is obtained; wherein water is used as a solvent, diethylamine tetraacetic acid is used as a complexing agent, and ammonia water is used for preparing gel. The high-heat-dissipation wear-resistant transparent conductive film prepared by the invention has the effects of high durability, efficient conductivity, no toxicity and no pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conductive film materials, in particular to a high-heat dissipation, wear-resistant, transparent conductive film and a preparation method thereof. Background Art

[0002] Transparent conductive films have been widely used in recent years as electrode materials for solar cells, displays, gas sensors, etc. At present, the most widely used transparent conductive film is In2O3:Sn (ITO) film, but its raw material In is an expensive and rare element, which limits its practical application potential. Recently, it has been found that ZnO film has the characteristics of high transmittance and low resistance comparable to ITO film, and the raw materials are abundant and low-priced, and it is expected to become an ideal material to replace ITO. However, most of the ZnO films currently prepared by the sol-gel method use organic solvents, which can easily cause harm to the body if not properly protected, and there are also many limitations on conductivity and service life. Based on this, how to invent a durable, efficient, non-toxic, high heat dissipation and wear-resistant transparent conductive film is particularly important. Summary of the invention

[0003] The object of the present invention is to provide a high heat dissipation wear-resistant transparent conductive film and a preparation method thereof, so as to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing a high heat dissipation wear-resistant transparent conductive film, comprising the following steps:

[0005] (1) After wiping the substrate clean, ultrasonically clean it in acetone solution, anhydrous ethanol and deionized water for 10-20 minutes in sequence, and finally rinse it with deionized water and dry it in an oven for later use;

[0006] (2) placing 30 to 90 parts of ethylenediaminetetraacetic acid aqueous solution in a container, adding 0.5 to 3 parts of zinc acetate, 0.2 to 1.2 parts of magnesium acetate, 0.03 to 0.24 parts of aluminum oxide, and 0.5 to 2 parts of glucose to prepare a solution, adding ammonia aqueous solution dropwise while stirring until the pH value reaches 6 to 8, and continuing to stir at 60 to 80° C. for 2 to 4 hours to obtain a viscous colloidal liquid;

[0007] (3) immersing the pretreated substrate into the sol prepared in (2) to uniformly coat the substrate, leaving it to stand for 1 to 2 hours, and then placing it in a vacuum furnace at 300 to 400° C. for 0.5 to 1 hour before taking it out;

[0008] (4) repeating step (3) to prepare a multilayer composite film;

[0009] (5) The obtained composite film is placed in a tubular furnace for high temperature annealing at 300-500° C. to obtain a highly heat-dissipating, wear-resistant, transparent conductive film.

[0010] Furthermore, in step (1), the substrate comprises polymer, glass, ceramic or metal.

[0011] Furthermore, the preparation method of the ethylenediaminetetraacetic acid aqueous solution in step (2) is: adding 0.5-1.5 parts of NaOH or KOH solution to 1 part of ethylenediaminetetraacetic acid, then adding water to a pH value of 7-9, and stirring until completely dissolved.

[0012] Furthermore, the concentration of the NaOH or KOH solution is 5-15M.

[0013] Furthermore, in step (2), glucose can be replaced by one or more of other organic carbon sources, such as citric acid, vitamin C, polydopamine, sugars, polyvinyl alcohol, tannic acid, resorcinol-formaldehyde resin, polyethylene glycol, asphalt, polypyrrole, polyvinyl pyrrolidone, anthracene and aniline.

[0014] Furthermore, the dropping speed of the ammonia water in step (2) is 0.1-0.5 mL / min, and the stirring speed is 600-1400 rpm.

[0015] Furthermore, in step (3), the coating is performed by immersing for 1-3 minutes and then pulling at a speed of 5 mm / min.

[0016] Furthermore, the vacuum degree in step (3) is 1×10 -4 ~7×10 -4 Pa.

[0017] Furthermore, the final thickness of the film formed by repeating the step (4) is 150-600 nm, and the optimal thickness is 400 nm.

[0018] Furthermore, the specific operation of the high temperature annealing treatment in step (5) is as follows: heating to 300-500°C at a rate of 13°C / min and maintaining for 12 hours; the protective gas is an inert gas.

[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0020] The present invention prepares a C / MgZnO:Al transparent conductive composite film with a multilayer structure through the steps of configuring into sol, coating, drying, vacuum annealing, etc., so as to achieve the effects of high durability, good conductivity, low cost, non-toxicity and no pollution.

[0021] First, water is used as solvent to reduce costs, zinc acetate is added to inhibit solid phase diffusion and improve film quality, and magnesium acetate is added to increase the bandgap of the film to have a higher visible light transmittance. Aluminum oxide is then added to replace the Zn lattice to increase the carrier concentration and reduce resistance. Glucose is then added as a carbon source and coated on the surface of the metal ions after high temperature decomposition to obtain better conductivity. After mixing evenly, a metal ion mixture is obtained, and ethylenediaminetetraacetic acid is used as a complexing agent to react with Zn 2+ Mg 2+ ,Al 3+ Effectively combine, and finally add ammonia water to buffer the pH value to 6-8 to promote the subsequent gel formation, which has better stability, and stir at a constant temperature for 2-4 hours to obtain a viscous gel.

[0022] Secondly, the sol is evenly plated on the substrate and left to dry to avoid cracking of the film. Then, the residual solvent on the substrate is evaporated through vacuum high temperature pretreatment, so that the hydrolysis intermediate decomposes to form ZnO nuclei. At this time, the carbon source gradually decomposes to form C in an oxygen-free environment, which is evenly coated on the formed grains to optimize the film strength. After repeating the treatment 3-5 times, a multilayer structure is formed, a three-dimensional conductive network of carbon is constructed, the transmission speed of carriers in the film is enhanced, and the conductivity of the composite film material is improved. Finally, high-temperature annealing further increases the ZnO grains, reduces the pores of the porous film, densifies the shrinkage, and enhances the strength of the film. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail. The various index tests of the high heat dissipation and wear-resistant transparent conductive films prepared in the following examples are all carried out with reference to GBT26598-2011.

[0025] Example 1

[0026] (1) After wiping the ceramic sheet clean, ultrasonically clean it in acetone solution, anhydrous ethanol and deionized water for 10 min in sequence, and finally rinse it with deionized water and dry it in an oven for later use;

[0027] (2) adding 0.5 parts of 5M NaOH solution to 1 part of ethylenediaminetetraacetic acid, adding water to a pH value of 7, and stirring until completely dissolved to obtain an ethylenediaminetetraacetic acid aqueous solution;

[0028] (3) 30 parts of ethylenediaminetetraacetic acid aqueous solution were placed in a container, 0.5 parts of zinc acetate, 0.2 parts of magnesium acetate, 0.03 parts of aluminum oxide, and 0.5 parts of glucose were added to prepare a solution, and an ammonia solution was added dropwise at a rate of 0.1 mL / min under a stirring speed of 600 rpm until the pH value reached 6, and the stirring was continued at 60° C. for 2 h to obtain a viscous colloidal liquid;

[0029] (4) The pretreated ceramic sheet was immersed in the sol prepared in (3) for 1 min and then pulled up at a speed of 5 mm / min. After standing for 1 h, it was placed in a vacuum furnace and vacuumed at 1×10 -4 Pa, 300℃ for 0.5h and then taken out;

[0030] (5) repeating step (4) to prepare a 150 nm thick multilayer composite film;

[0031] (6) The obtained composite film is placed in a tubular furnace and heated to 300° C. at a rate of 13° C. / min under argon protection and maintained for 12 h to obtain a high heat dissipation and wear-resistant transparent conductive film.

[0032] Example 2

[0033] (1) After wiping the glass slide clean, ultrasonically clean it in acetone solution, anhydrous ethanol and deionized water for 10 min in sequence, and finally rinse it with deionized water and dry it in an oven for later use;

[0034] (2) adding 1 part of 10M NaOH solution to 1 part of ethylenediaminetetraacetic acid, adding water to a pH value of 8, and stirring until completely dissolved to obtain an ethylenediaminetetraacetic acid aqueous solution;

[0035] (3) 60 parts of ethylenediaminetetraacetic acid aqueous solution were placed in a container, 1.75 parts of zinc acetate, 0.7 parts of magnesium acetate, 0.14 parts of aluminum oxide, and 1.25 parts of glucose were added to prepare a solution, and an ammonia solution was added dropwise at a rate of 0.3 mL / min under a stirring speed of 1000 rpm until the pH value reached 7, and stirring was continued at 70° C. for 3 h to obtain a viscous colloidal liquid;

[0036] (4) The pretreated glass sheet was immersed in the sol prepared in (3) for 2 min and then pulled up at a speed of 5 mm / min. After standing for 1.5 h, it was placed in a vacuum furnace and heated at a vacuum degree of 4 × 10 -4 Pa, 350℃ for 0.75h and then taken out;

[0037] (5) repeating step (4) to prepare a 400 nm thick multilayer composite film;

[0038] (6) The obtained composite film is placed in a tubular furnace and heated to 400°C at a rate of 13°C / min under nitrogen protection and maintained for 12 hours to obtain a high heat dissipation and wear-resistant transparent conductive film.

[0039] Example 3

[0040] (1) After wiping the polyethylene sheet clean, ultrasonically clean it in acetone solution, anhydrous ethanol and deionized water for 10 min in sequence, and finally rinse it with deionized water and dry it in an oven for later use;

[0041] (2) adding 1.5 parts of 15M NaOH solution to 1 part of ethylenediaminetetraacetic acid, adding water to a pH value of 9, and stirring until completely dissolved to obtain an ethylenediaminetetraacetic acid aqueous solution;

[0042] (3) 90 parts of ethylenediaminetetraacetic acid aqueous solution were placed in a container, 3 parts of zinc acetate, 0.7 parts of magnesium acetate, 0.24 parts of aluminum oxide, and 2 parts of glucose were added to prepare a solution, and an ammonia solution was added dropwise at a rate of 0.5 mL / min under a stirring speed of 1500 rpm until the pH value reached 8, and the stirring was continued at 70° C. for 4 h to obtain a viscous colloidal liquid;

[0043] (4) The pretreated polyethylene sheet was immersed in the sol prepared in (3) for 3 min and then pulled up at a speed of 5 mm / min. After standing for 2 h, it was placed in a vacuum furnace and heated at a vacuum degree of 7×10 -4 Pa, treated at 400℃ for 1h and then taken out;

[0044] (5) repeating step (4) to prepare a 600 nm thick multilayer composite film;

[0045] (6) The obtained composite film is placed in a tubular furnace and heated to 500° C. at a rate of 13° C. / min under nitrogen protection and maintained for 12 h to obtain a high heat dissipation and wear-resistant transparent conductive film.

[0046] Comparative Example 1

[0047] The difference between Comparative Example 1 and Example 2 is only the difference in step (3), and step (3) is modified as follows: 60 parts of ethylenediaminetetraacetic acid aqueous solution are placed in a container, 1.75 parts of zinc acetate, 0.7 parts of magnesium acetate, and 0.14 parts of aluminum oxide are added to prepare a solution, and an ammonia solution is added dropwise at a rate of 0.3 mL / min to a pH value of 7 under a stirring speed of 1000 rpm, and stirring is continued at 70° C. for 3 h to obtain a viscous colloidal liquid. The remaining preparation steps are the same as those in Example 2.

[0048] Comparative Example 2

[0049] The difference between Comparative Example 2 and Example 2 is only the difference in step (3), and step (3) is modified as follows: 60 parts of ethylenediaminetetraacetic acid aqueous solution are placed in a container, 1.75 parts of zinc acetate, 0.7 parts of magnesium acetate, and 1.25 parts of glucose are added to prepare a solution, and an ammonia solution is added dropwise at a rate of 0.3 mL / min to a pH value of 7 under a stirring speed of 1000 rpm, and stirring is continued at 70° C. for 3 h to obtain a viscous colloidal liquid. The remaining preparation steps are the same as those in Example 2.

[0050] Comparative Example 3

[0051] The difference between Comparative Example 3 and Example 2 is only the difference in step (3), and step (3) is modified as follows: 60 parts of ethylenediaminetetraacetic acid aqueous solution are placed in a container, 1.75 parts of zinc acetate, 0.14 parts of aluminum oxide, and 1.25 parts of glucose are added to prepare a solution, and an ammonia aqueous solution is added dropwise at a rate of 0.3 mL / min to a pH value of 7 under a stirring speed of 1000 rpm, and stirring is continued at 70° C. for 3 h to obtain a viscous colloidal liquid. The remaining preparation steps are the same as those in Example 2.

[0052] Comparative Example 4

[0053] The difference between Comparative Example 4 and Example 2 is only the difference in step (3), and step (3) is modified as follows: 60 parts of ethylenediaminetetraacetic acid aqueous solution are placed in a container, 0.7 parts of magnesium acetate, 0.14 parts of aluminum oxide, and 1.25 parts of glucose are added to prepare a solution, and an ammonia solution is added dropwise at a rate of 0.3 mL / min to a pH value of 7 under a stirring speed of 1000 rpm, and stirring is continued at 70° C. for 3 h to obtain a viscous colloidal liquid. The remaining preparation steps are the same as those in Example 2.

[0054] Comparative Example 5

[0055] The difference between Comparative Example 5 and Example 2 is only the difference in step (5), in which step (5) is modified as follows: step (4) is not repeated. The remaining preparation steps are the same as those in Example 2.

[0056] Comparative Example 6

[0057] The difference between Comparative Example 6 and Example 2 is only the difference in step (4), which is modified as follows: immersing the pretreated glass sheet in the sol prepared in (3) for 2 minutes, then pulling it at a speed of 5 mm / min and letting it stand for 1.5 hours. The remaining preparation steps are the same as those in Example 2.

[0058] Comparative Example 7

[0059] The difference between Comparative Example 7 and Example 2 is that there is no step (6). The remaining preparation steps are the same as those of Example 2.

[0060] Effect example

[0061] Table 1 below shows the performance analysis results of the high heat dissipation and wear-resistant transparent conductive films of Examples 1 to 3 of the present invention and Comparative Examples 1 to 7.

[0062] Average light transmittance (%) <![CDATA[Resistivity (10 -3 Ω·cm)]]> Film firmness Example 1 90.9 2.31 whole Example 2 89.3 2.01 whole Example 3 87.4 2.17 whole Comparative Example 1 86.5 3.43 whole Comparative Example 2 84.2 3.05 whole Comparative Example 3 80.7 4.62 whole Comparative Example 4 87.1 5.80 Obvious scratches Comparative Example 5 88.5 3.19 whole Comparative Example 6 87.2 3.26 Shedding Comparative Example 7 87.6 2.77 Obvious scratches, peeling

[0063] From the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 1, it can be found that the present invention utilizes glucose, which is uniformly coated on the surface of metal ions after high temperature decomposition, thereby increasing the mobility between electrons and showing better conductivity; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 2, it can be found that the lattice of Zn is successfully replaced by aluminum oxide, the carrier concentration is increased, and the resistance is significantly reduced; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 3, it can be found that the addition of magnesium acetate increases the band gap of the film and obtains better visible light transmittance; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 4, it can be found that the addition of zinc acetate reduces solid phase diffusion and effectively improves the service life of the material. From the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 5, it can be found that repeated coating can form a multilayer structure, build a three-dimensional conductive network of carbon, and improve the conductivity of the film material. From the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 6, it can be found that the high temperature pretreatment can remove the residual solvent on the substrate, avoid cracking of the film during subsequent annealing, and enhance the firmness of the film. At the same time, the carbon source is fully decomposed and evenly coated outside the grains, thereby improving the conductivity. From the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 7, it can be found that the high temperature annealing densifies and shrinks the material, and the strength is significantly improved.

[0064] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a high heat dissipation wear-resistant transparent conductive film, characterized in that: The method comprises the following preparation steps: (1) After wiping the substrate clean, ultrasonically clean it in acetone solution, anhydrous ethanol and deionized water for 10-20 minutes in sequence, and finally rinse it with deionized water and dry it in an oven for later use; (2) placing 30 to 90 parts of ethylenediaminetetraacetic acid aqueous solution in a container, adding 0.5 to 3 parts of zinc acetate, 0.2 to 1.2 parts of magnesium acetate, 0.03 to 0.24 parts of aluminum oxide, and 0.5 to 2 parts of glucose to prepare a solution, adding ammonia aqueous solution dropwise while stirring until the pH value reaches 6 to 8, and continuing to stir at 60 to 80° C. for 2 to 4 hours to obtain a viscous colloidal liquid; (3) immersing the pretreated substrate into the sol prepared in (2) to uniformly coat the substrate, leaving it to stand for 1 to 2 hours, and then placing it in a vacuum furnace at 300 to 400° C. for 0.5 to 1 hour before taking it out; (4) repeating step (3) to prepare a multilayer composite film; (5) The obtained composite film is placed in a tubular furnace for high temperature annealing at 300-500° C. to obtain a highly heat-dissipating, wear-resistant, transparent conductive film.

2. The method for preparing a high heat dissipation wear-resistant transparent conductive film according to claim 1, characterized in that: In the step (1), the substrate comprises polymer, glass, ceramic or metal.

3. The method for preparing a high heat dissipation wear-resistant transparent conductive film according to claim 1, characterized in that: The preparation method of the ethylenediaminetetraacetic acid aqueous solution in step (2) is: add 0.5-1.5 parts of NaOH or KOH solution to 1 part of ethylenediaminetetraacetic acid, then add water to a pH value of 7-9, and stir until it is completely dissolved.

4. The method for preparing a high heat dissipation wear-resistant transparent conductive film according to claim 3, characterized in that: The concentration of the NaOH or KOH solution is 5-15M.

5. The method for preparing a highly heat-dissipating and wear-resistant transparent conductive film according to claim 1, characterized in that: In the step (2), glucose can be replaced by one or more of other organic carbon sources, such as citric acid, vitamin C, polydopamine, sugars, polyvinyl alcohol, tannic acid, resorcinol-formaldehyde resin, polyethylene glycol, asphalt, polypyrrole, polyvinyl pyrrolidone, anthracene and aniline.

6. The method for preparing a high heat dissipation wear-resistant transparent conductive film according to claim 1, characterized in that: The dropping speed of the ammonia water in the step (2) is 0.1-0.5 mL / min, and the stirring speed is 600-1400 rpm.

7. The method for preparing a highly heat-dissipating and wear-resistant transparent conductive film according to claim 1, characterized in that: The coating in step (3) is performed by immersing for 1-3 minutes and then pulling at a speed of 5 mm / min.

8. The method for preparing a highly heat dissipating and wear-resistant transparent conductive film according to claim 1, characterized in that: The vacuum degree of step (3) is 1×10 -4 ~7×10 -4 Pa.

9. The method for preparing a highly heat-dissipating and wear-resistant transparent conductive film according to claim 1, characterized in that: The final thickness of the film produced by repeating the step (4) is 150-600 nm, and the optimal thickness is 400 nm.

10. The method for preparing a highly heat-dissipating, wear-resistant, transparent conductive film according to claim 1, characterized in that: The specific operation of the high temperature annealing treatment in step (5) is as follows: heating to 300-500° C. at a rate of 13° C. / min and maintaining for 12 hours; the protective gas is an inert gas.

Citation Information

Patent Citations

  • Dielectric-constant adjustable houghite-like membrane and preparation method thereof

    CN101538018A

  • Method needing no vacuum process to prepare organic polymer solar cell

    CN101661994A

  • Preparation method for resistivity regulation and control of aluminum-doped zinc oxide transparent conducting film

    CN102412018A

  • Organic solar cell based on multilayer magnesium- and aluminium-doped zinc oxide composite film serving as electron transfer layer

    CN108198939A

  • Compound oxide sintered compact, oxide transparent conductive film, and method for producing the same