Method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste

Through the extraction, precipitation, calcination and nitriding of rare earth waste, rare earth iron nitrogen magnetic powder is prepared, which solves the problem of rare earth waste recycling, improves resource utilization and reduces production costs, and promotes the recycling of rare earth resources and the magnetic powder. Market competitiveness.

CN118942824APending Publication Date: 2024-11-12PEKING UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411221058.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The waste generated by rare earth waste during processing cannot be effectively recycled, resulting in low reuse of rare earth resources and high production costs.

Method used

Through the extraction, precipitation, calcination, reduction heat treatment and nitriding of rare earth waste, high-purity rare earth iron nitrogen magnetic powder is prepared, which expands the application direction of rare earth waste and reduces production costs.

Benefits of technology

It improves the utilization rate of rare earth resources, reduces the production cost of rare earth iron nitrogen magnetic powder, makes the prepared rare earth iron nitrogen magnetic powder have better market competitiveness, and promotes the recycling of rare earth resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942824A_ABST
    Figure CN118942824A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste, and belongs to the technical field of rare earth waste recovery. The method comprises the following steps: firstly, extracting the rare earth waste to obtain a rare earth chloride solution, then mixing the rare earth chloride solution with a precipitant, carrying out precipitation treatment and solid-liquid separation to obtain a rare earth precipitate, calcining to obtain a rare earth oxide, mixing the rare earth oxide with iron powder and CaH2 / Ca, carrying out reduction heat treatment to obtain rare earth iron alloy powder, and sequentially carrying out nitriding treatment and post-treatment to obtain the rare earth iron alloy powder. The rare earth iron nitrogen magnetic powder is obtained. According to the method, on one hand, the problem of rare earth waste recycling is solved, the application direction of the rare earth waste is expanded, recycling of rare earth resources is promoted, on the other hand, the rare earth-iron-nitrogen magnetic powder material can be obtained, meanwhile, the production cost of the rare earth-iron-nitrogen magnetic powder is reduced, and the prepared rare earth-iron-nitrogen magnetic powder has higher market competitiveness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rare earth waste recycling, and in particular to a method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste. Background Art

[0002] Rare earth elements, due to their excellent optical, electrical, magnetic and other physical properties, can be combined with other materials to form new materials with different properties and a wide variety of varieties, achieving incomparable quality and performance of traditional materials. They have been widely used in high-tech fields such as permanent magnetic materials, new energy materials, luminescent materials, and catalytic materials. The waste generated during the preparation and processing of these new rare earth materials and the waste generated by long-term use have become secondary resources for the extraction of rare earth and other non-ferrous metal elements. The recycling of rare earth secondary resources is an urgent requirement and inevitable choice for the sustainable development of rare earths. Through waste recycling, the reuse rate of rare earths can be increased. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste. The method provided by the present invention utilizes rare earth waste to separate rare earth chlorides and then prepares high-purity rare earth iron nitrogen magnetic powder, which not only improves the utilization rate of rare earth resources but also reduces the production cost of rare earth iron nitrogen magnetic powder.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste, comprising the following steps:

[0006] 1) extracting rare earth waste to obtain a rare earth chloride solution;

[0007] 2) mixing the rare earth chloride solution obtained in step 1) with a precipitant, performing precipitation treatment and solid-liquid separation to obtain a rare earth precipitate;

[0008] 3) calcining the rare earth precipitate obtained in step 2) to obtain rare earth oxides;

[0009] 4) In an inert atmosphere, the rare earth oxide obtained in step 3) is mixed with iron powder and CaH2 / Ca, and subjected to reduction heat treatment to obtain rare earth iron alloy powder;

[0010] 5) In a nitrogen atmosphere, the rare earth iron alloy powder obtained in step 4) is subjected to nitridation treatment and post-treatment to obtain rare earth iron nitrogen magnetic powder.

[0011] Preferably, the extractant used for extraction in step 1) is one or more of P350, P204, P507, and cyclohexane acid, and the extraction is performed 2 to 8 times.

[0012] Preferably, the rare earth chloride in step 1) is one or more of the chlorides of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium.

[0013] Preferably, the precipitant in step 2) is at least one of oxalic acid, ammonium carbonate and sodium carbonate, and the rare earth precipitate is at least one of rare earth oxalate and rare earth carbonate.

[0014] Preferably, the particle size of the iron powder in step 4) is 0.1-20 μm.

[0015] Preferably, in step 4), the mass ratio of rare earth oxide, iron powder and CaH2 / Ca is (10-100):100:(10-100).

[0016] Preferably, the temperature of the reduction heat treatment in step 4) is 900-1100° C., and the time of the reduction heat treatment is 1-10 h.

[0017] Preferably, the temperature of the nitriding treatment in step 5) is 350-550° C., and the time of the nitriding treatment is 6-48 hours:

[0018] Preferably, the post-treatment in step 5) further comprises: washing, drying and grinding the product of the nitridation treatment in sequence to obtain rare earth iron nitrogen magnetic powder.

[0019] Preferably, the rare earth in the rare earth iron nitrogen magnetic powder in step 5) is one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium.

[0020] The present invention provides a method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste, firstly extracting the rare earth waste to obtain a rare earth chloride solution, then mixing it with a precipitant, performing precipitation treatment and solid-liquid separation to obtain a rare earth precipitate, calcining to obtain a rare earth oxide, then mixing it with iron powder and CaH2 / Ca, performing reduction heat treatment to obtain a rare earth iron alloy powder, and sequentially performing nitridation treatment and post-treatment to obtain a rare earth iron nitrogen magnetic powder. The method provided by the present invention, on the one hand, solves the problem of recycling rare earth waste, expands the application direction of rare earth waste, and promotes the recycling of rare earth resources, on the other hand, can obtain rare earth iron nitrogen magnetic powder materials, while reducing the production cost of rare earth iron nitrogen magnetic powder, so that the prepared rare earth iron nitrogen magnetic powder has more market competitiveness. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a magnetic property curve of the samarium iron nitrogen magnetic powder prepared in Example 1;

[0022] Figure 2 is a scanning electron microscope image of the samarium iron nitrogen magnetic powder before ball milling in Example 1;

[0023] Figure 3 This is a magnetic property curve of the samarium iron nitrogen magnetic powder prepared in Example 2;

[0024] Figure 4 is a scanning electron microscope image of the samarium iron nitrogen magnetic powder before ball milling in Example 2;

[0025] Figure 5 This is a magnetic property curve diagram of the samarium iron nitrogen magnetic powder prepared in Example 3;

[0026] Figure 6 is a scanning electron microscope image of the samarium iron nitrogen magnetic powder before ball milling in Example 3;

[0027] Figure 7 This is the XRD pattern of the samarium iron nitrogen magnetic powder prepared in Examples 1 to 3. DETAILED DESCRIPTION

[0028] The present invention provides a method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste, comprising the following steps:

[0029] 1) extracting rare earth waste to obtain a rare earth chloride solution;

[0030] 2) mixing the rare earth chloride solution obtained in step 1) with a precipitant, performing precipitation treatment and solid-liquid separation to obtain a rare earth precipitate;

[0031] 3) calcining the rare earth precipitate obtained in step 2) to obtain rare earth oxides;

[0032] 4) In an inert atmosphere, the rare earth oxide obtained in step 3) is mixed with iron powder and CaH2 / Ca, and subjected to reduction heat treatment to obtain rare earth iron alloy powder;

[0033] 5) In a nitrogen atmosphere, the rare earth iron alloy powder obtained in step 4) is subjected to nitridation treatment and post-treatment to obtain rare earth iron nitrogen magnetic powder.

[0034] In the present invention, unless otherwise specified, the raw materials used are conventional commercial products in the art.

[0035] The invention extracts rare earth waste to obtain rare earth chloride solution.

[0036] In the present invention, the extractant used for the extraction is one or more of P350, P204, P507, and cyclohexane acid, and the number of extractions is 2 to 8 times.

[0037] In the present invention, the rare earth chloride is preferably one or more of the chlorides of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium.

[0038] After obtaining the rare earth chloride solution, the present invention mixes the rare earth chloride solution with a precipitant, performs precipitation treatment and solid-liquid separation, and obtains a rare earth precipitate.

[0039] In the present invention, the precipitant is preferably at least one of oxalic acid, ammonium carbonate and sodium carbonate. The present invention has no special restrictions on the precipitation treatment, and it is sufficient to completely convert the rare earth chloride into a rare earth precipitate. In the present invention, the precipitation treatment is preferably stirred at room temperature for 1 to 24 hours. The present invention has no special restrictions on the method of solid-liquid separation, and the technical solutions well known in the art can be used.

[0040] In the present invention, the rare earth precipitate is preferably at least one of rare earth oxalate and rare earth carbonate.

[0041] After obtaining the rare earth precipitate, the present invention calcines the rare earth precipitate to obtain rare earth oxides.

[0042] In the present invention, the calcination is preferably carried out in air; the calcination temperature is preferably 1000-1200° C.; and the calcination time is preferably 1-10 h.

[0043] After obtaining the rare earth oxide, the present invention mixes the rare earth oxide with iron powder and CaH2 / Ca in an inert atmosphere, and performs reduction heat treatment to obtain rare earth iron alloy powder.

[0044] In the present invention, the inert atmosphere is preferably at least one of a hydrogen atmosphere and an argon atmosphere.

[0045] In the present invention, the particle size of the iron powder is preferably 0.1-20 μm, more preferably 0.5-10 μm. The present invention controls the particle size of the iron powder within the above range so that the iron powder fully participates in the reaction and ensures that the prepared product has better magnetic properties. In the present invention, the mass ratio of the rare earth oxide, iron powder and CaH2 / Ca is preferably (10-100):100:(10-100), more preferably (20-90):100:(20-90). The present invention controls the mass ratio of rare earth oxide, iron powder and CaH2 / Ca within the above range to ensure that the prepared rare earth iron nitrogen magnetic powder has better magnetic properties. In the present invention, the temperature of the reduction heat treatment is preferably 900-1100°C, more preferably 950-1050°C; the time of the reduction heat treatment is preferably 1-10h, more preferably 2-8h. The present invention controls the temperature and time of the reduction heat treatment within the above range to ensure that the reaction is fully carried out.

[0046] After obtaining the rare earth iron alloy powder, the present invention performs nitridation treatment and post-treatment on the rare earth iron alloy powder in a nitrogen atmosphere to obtain rare earth iron nitrogen magnetic powder.

[0047] In the present invention, the temperature of the nitriding treatment is preferably 350-530°C, more preferably 400-500°C; the time of the nitriding treatment is preferably 6-48h, more preferably 10-40h. The present invention controls the temperature and time of the nitriding treatment within the above range to ensure that the rare earth iron alloy can be completely transformed into rare earth iron nitrogen magnetic powder.

[0048] After the nitriding treatment is completed, the present invention preferably sequentially washes, dries and grinds the product of the nitriding treatment to obtain rare earth iron nitrogen magnetic powder.

[0049] In the present invention, the reagent used for washing is preferably a methanol solution of ammonium acetate; the concentration of ammonium acetate in the methanol solution of ammonium acetate is preferably 0.5% vol to 10% vol. In the present invention, the drying method is preferably vacuum drying. The present invention has no special restrictions on the temperature and time of vacuum drying, and the residual reagent can be removed by using technical solutions well known in the art. The present invention has no special restrictions on the grinding method, and the rare earth iron nitrogen magnetic powder of the target particle size can be obtained by using technical solutions well known in the art. In the present invention, the grinding method is preferably: the dried product and the alcohol solution are mixed and ball milled, the liquid is drained after the ball milling, and the rare earth iron nitrogen magnetic powder is obtained after drying. The present invention has no special restrictions on the ball milling method, and the rare earth iron nitrogen magnetic powder of the target particle size can be obtained by using technical solutions well known in the art.

[0050] In the present invention, the rare earth in the rare earth iron nitrogen magnetic powder is preferably one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium.

[0051] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] Example 1

[0053] A method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste, the steps are as follows:

[0054] 1) Using P350 as an extractant, extracting the rare earth waste 5 times to obtain a samarium chloride solution;

[0055] 2) mixing the samarium chloride solution obtained in step 1) with oxalic acid, performing a precipitation treatment at room temperature under stirring for 4 hours, and obtaining a samarium oxalate precipitate by solid-liquid separation;

[0056] 3) calcining the dilute samarium oxalate precipitate obtained in step 2) at 1100° C. for 4 hours to obtain samarium oxide powder;

[0057] 4) In an argon atmosphere, the samarium oxide powder obtained in step 3) is mixed with iron powder and Ca particles having a particle size of 1 μm, and subjected to reduction heat treatment at 1000° C. for 4 h to obtain a rare earth iron alloy powder;

[0058] The mass ratio of the rare earth oxide, iron powder and Ca particles is 80:100:60;

[0059] 5) In a nitrogen atmosphere, the rare earth iron alloy powder obtained in step 4) is subjected to nitriding treatment at 430° C. for 24 h, and then the nitriding product powder is washed in a 3% vol ammonium acetate methanol solution to a pH of 7, and then vacuum dried, and then mixed with an alcohol solution and ball milled for 3 h. After ball milling, the liquid is drained and dried to obtain samarium iron nitrogen magnetic powder.

[0060] The samarium iron nitrogen magnetic powder prepared in Example 1 was uniformly mixed with paraffin wax and oriented in a 5T magnetic field. The magnetic properties of the sample were measured in a 3T field using a vibrating sample magnetometer. The magnetic property curve of the samarium iron nitrogen prepared in Example 1 is as follows: Figure 1 The scanning electron microscope image of the samarium iron nitrogen magnetic powder prepared in Example 1 is as shown. Figure 2 As shown. Figure 1 and Figure 2 It can be seen that the samarium iron nitrogen magnetic powder prepared in Example 1 exhibits the microscopic morphology characteristics of rounded particles and has excellent magnetic properties.

[0061] Example 2

[0062] A method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste, the steps are as follows:

[0063] 1) Using P350 as an extractant, extracting the rare earth waste 5 times to obtain a samarium chloride solution;

[0064] 2) mixing the samarium chloride solution obtained in step 1) with ammonium carbonate, performing a precipitation treatment at room temperature under stirring for 4 hours, and obtaining a samarium carbonate precipitate by solid-liquid separation;

[0065] 3) calcining the samarium carbonate precipitate obtained in step 2) at 1000° C. for 4 hours to obtain samarium oxide powder;

[0066] 4) In an argon atmosphere, the samarium oxide powder obtained in step 3) is mixed with iron powder with a particle size of 5 μm and Ca particles, and subjected to reduction heat treatment at 1000° C. for 4 h to obtain a rare earth iron alloy powder;

[0067] The mass ratio of the rare earth oxide, iron powder and Ca particles is 80:100:60;

[0068] 5) In a nitrogen atmosphere, the rare earth iron alloy powder obtained in step 4) is subjected to nitriding treatment at 460° C. for 24 h, and then the nitriding product powder is washed in a 3% vol ammonium acetate methanol solution to a pH of 7, and then vacuum dried, and then mixed with an alcohol solution and ball milled for 3 h. After ball milling, the liquid is drained and dried to obtain samarium iron nitrogen magnetic powder.

[0069] The samarium iron nitrogen magnetic powder prepared in Example 2 was uniformly mixed with paraffin wax and oriented in a 5T magnetic field. The magnetic properties of the sample were measured using a vibrating sample magnetometer in a 3T field. The magnetic property curve of the samarium iron nitrogen prepared in Example 2 is as follows: Figure 3 The scanning electron microscope image of the samarium iron nitrogen magnetic powder prepared in Example 2 is as shown. Figure 4 As shown. Figure 3 and 4 It can be seen that the samarium iron nitrogen magnetic powder prepared in Example 2 exhibits the microscopic morphology characteristics of rounded particles and has excellent magnetic properties.

[0070] Example 3

[0071] A method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste, the steps are as follows:

[0072] 1) Using P350 as an extractant, extracting the rare earth waste 5 times to obtain a samarium chloride solution;

[0073] 2) mixing the samarium chloride solution obtained in step 1) with sodium carbonate, performing a precipitation treatment at room temperature under stirring for 4 hours, and obtaining a samarium carbonate precipitate by solid-liquid separation;

[0074] 3) calcining the samarium carbonate precipitate obtained in step 2) at 1000° C. for 4 hours to obtain samarium oxide powder;

[0075] 4) In an argon atmosphere, the samarium oxide powder obtained in step 3) is mixed with iron powder with a particle size of 10 μm and Ca particles, and subjected to reduction heat treatment at 1000° C. for 4 h to obtain a rare earth iron alloy powder;

[0076] The mass ratio of the rare earth oxide, iron powder and Ca particles is 80:100:60;

[0077] 5) In a nitrogen atmosphere, the rare earth iron alloy powder obtained in step 4) is subjected to nitriding treatment at 460° C. for 24 h, and then the nitriding product powder is washed in a 3% vol ammonium acetate methanol solution to a pH of 7, and then vacuum dried, and then mixed with an alcohol solution and ball milled for 3 h. After ball milling, the liquid is drained and dried to obtain samarium iron nitrogen magnetic powder.

[0078] The samarium iron nitrogen magnetic powder prepared in Example 3 was uniformly mixed with paraffin wax and oriented in a 5T magnetic field. The magnetic properties of the sample were measured in a 3T field using a vibrating sample magnetometer. The magnetic property curve of the samarium iron nitrogen prepared in Example 3 can be obtained based on the measurement data as shown in the following figure: Figure 5 The scanning electron microscope image of the samarium iron nitrogen magnetic powder prepared in Example 3 is as shown. Figure 6 As shown. Figure 5 and 6 It can be seen that the samarium iron nitrogen magnetic powder prepared in Example 3 exhibits the microscopic morphology characteristics of rounded particles and has excellent magnetic properties.

[0079] The XRD patterns of the samarium iron nitrogen magnetic powders prepared in Examples 1 to 3 were obtained by X-ray diffractometer. Figure 7 As shown, according to Figure 7 It can be seen that the samarium iron nitrogen magnetic powders prepared in Examples 1 to 3 all have a good "Th2Zn17 type" structure.

[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing rare earth iron nitrogen magnetic powder based on rare earth waste, characterized in that: The following steps are involved: 1) extracting rare earth waste to obtain a rare earth chloride solution; 2) mixing the rare earth chloride solution obtained in step 1) with a precipitant, performing precipitation treatment and solid-liquid separation to obtain a rare earth precipitate; 3) calcining the rare earth precipitate obtained in step 2) to obtain rare earth oxides; 4) In an inert atmosphere, the rare earth oxide obtained in step 3) is mixed with iron powder and CaH2 / Ca, and subjected to reduction heat treatment to obtain rare earth iron alloy powder; 5) In a nitrogen atmosphere, the rare earth iron alloy powder obtained in step 4) is subjected to nitridation treatment and post-treatment to obtain rare earth iron nitrogen magnetic powder.

2. The method according to claim 1, characterized in that The extractant used for extraction in step 1) is one or more of P350, P204, P507, and cyclohexane acid, and the number of extractions is 2 to 8 times.

3. The method according to claim 1, characterized in that: The rare earth chloride in step 1) is one or more of the chlorides of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium.

4. The method according to claim 1, characterized in that: The precipitant in step 2) is at least one of oxalic acid, ammonium carbonate and sodium carbonate, and the rare earth precipitate is at least one of rare earth oxalate and rare earth carbonate.

5. The method according to claim 1, characterized in that The particle size of the iron powder in step 4) is 0.1-20 μm.

6. The method according to claim 1, characterized in that In the step 4), the mass ratio of rare earth oxide, iron powder and CaH2 / Ca is (10-100):100:(10-100).

7. The method according to claim 1, characterized in that The temperature of the reduction heat treatment in step 4) is 900-1100° C., and the time of the reduction heat treatment is 1-10 hours.

8. The method according to claim 1, characterized in that: The temperature of the nitriding treatment in step 5) is 350-550° C., and the time of the nitriding treatment is 6-48 hours.

9. The method according to claim 1, characterized in that: The post-treatment in step 5) further comprises: washing, drying and grinding the product of the nitridation treatment in sequence to obtain rare earth iron nitrogen magnetic powder.

10. The method according to claim 1, characterized in that The rare earth in the rare earth iron nitrogen magnetic powder in step 5) is one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium.