Permanent magnet, device, method for manufacturing permanent magnet, and method for manufacturing permanent magnet powder
Through specific chemical composition and process processing, the SmFe12-type compound permanent magnet with ThMn12-type crystal structure is formed, which solves the problem of insufficient coercive force in the prior art, and achieves the effects of high coercive force and high saturation magnetization. It is suitable for A variety of electronic devices and sensor applications.
Patent Information
- Application Number
- CN202410468963.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-12-26
- Filing Date
- 2024-04-18
- Publication Date
- 2024-11-12
AI Technical Summary
The existing SmFe12-type compound permanent magnets have shortcomings in coercive forces, which are difficult to meet the demand for high coercive forces.
Using SmFe12-type compound with ThMn12-type square crystal structure, the preparation of melts with chemical formula (R1-xZrx)a(T1-y-zCuyMz)bBc is carried out for quenching, crushing and forming. , sintering and aging treatment to form permanent magnets with high coercive force.
Permanent magnets with high coercivity and high saturation magnetization are suitable for high temperature environments and are suitable for various electronic equipment and sensor applications.
Smart Images

Figure CN118942828A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a permanent magnet, a device, a method for manufacturing a permanent magnet, and a method for manufacturing permanent magnet powder. Background Art
[0002] A permanent magnet with high residual magnetization and high heat resistance is required. As a candidate for such a magnet material, ThMn 12 SmFe 12 The SmFe 12 The compounds have high saturation magnetization and high Curie temperature.
[0003] As a permanent magnet having excellent saturation magnetization and coercive force and improved temperature characteristics of coercive force, Japanese Patent Application Laid-Open No. 2001-189206 discloses a permanent magnet comprising a ThMn 12 It is an alloy of a hard magnetic phase and a non-magnetic phase with a tetragonal crystal structure.
[0004] As a magnetic material for improving saturation magnetization, Japanese Patent Publication No. 2018-125512 discloses a magnetic material having a specific composition, wherein the magnetic material comprises ThMn 12 The main phase is composed of type crystalline phase. Summary of the invention
[0005] In the presence of ThMn 12 SmFe 12 In the series of compounds, a higher coercivity is also required.
[0006] The present disclosure aims to solve the above-mentioned problems, and an object of the present disclosure is to provide a permanent magnet having high coercive force, a device, a method for producing a permanent magnet, and a method for producing permanent magnet powder.
[0007] The permanent magnet of the present disclosure has a composition represented by the following chemical formula (1):
[0008] Chemical formula (1): (R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c
[0009] Among them, R represents at least one selected from the rare earth elements, T represents at least one selected from the group consisting of Fe, Co and Ni, M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta and W, a, b and c respectively represent atomic %, x, y and z respectively represent the ratios of Zr, Cu and M, and satisfy the following conditions: 5≤a≤10, b=100-(a+c), 3≤c≤20, 0.01≤x≤0.5, 0.001≤y≤0.1, 0≤z≤0.1.
[0010] Furthermore, a device according to the present disclosure includes the permanent magnet.
[0011] In the method for producing a permanent magnet according to the present disclosure, a molten metal having a composition represented by the following chemical formula (1) is prepared.
[0012] Chemical formula (1): (R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c
[0013] Wherein, R represents at least one selected from the rare earth elements, T represents at least one selected from the group consisting of Fe, Co and Ni, M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta and W, a, b and c represent atomic %, x, y and z represent the ratio of Zr, Cu and M, respectively, and the following conditions are satisfied: 5≤a≤10, b=100-(a+c), 3≤c≤20, 0.01≤x≤0.5, 0.001≤y≤0.1, 0≤z≤0.1,
[0014] 50~10 7 The melt is quenched at 1000 K / sec to form an alloy, the alloy is crushed into powder, the powder is formed into a formed body, the formed body is sintered in a temperature range of 950°C to 1250°C to form a sintered body, the sintered body is aged in a temperature range of 700°C to 900°C, and then quenched.
[0015] In the method for producing permanent magnet powder according to the present disclosure, a molten metal having a composition represented by the following chemical formula (1) is prepared.
[0016] Chemical formula (1): (R 1-x Zr x ) a (T1-y-z Cu y M z ) b B c
[0017] Wherein, R represents at least one selected from the rare earth elements, T represents at least one selected from the group consisting of Fe, Co and Ni, M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta and W, a, b and c represent atomic %, x, y and z represent the ratio of Zr, Cu and M, respectively, and the following conditions are satisfied: 5≤a≤10, b=100-(a+c), 3≤c≤20, 0.01≤x≤0.5, 0.001≤y≤0.1, 0≤z≤0.1,
[0018] 50~10 7 The molten metal is rapidly cooled at 1000 K / sec to prepare an alloy, the alloy is crystallized at a temperature ranging from 700° C. to 900° C., and the alloy is pulverized into powder.
[0019] According to the present disclosure, it is possible to provide a permanent magnet having high coercive force, a device, a method for producing a permanent magnet, and a method for producing permanent magnet powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a diagram showing the correlation between the half-value width of the X-ray diffraction spectrum peak and the crystallite size of the permanent magnet according to the present embodiment.
[0021] Figure 2 : It is the X-ray diffraction spectrum of the permanent magnet of Example and Comparative Example.
[0022] Figure 3 It is a graph showing the dependency of the half width of the X-ray diffraction spectrum peak of the permanent magnet of the Example on the heat treatment temperature.
[0023] Figure 4 It is a graph showing magnetization curves of permanent magnets of Examples and Comparative Examples.
[0024] Figure 5 : It is the X-ray diffraction spectrum of the permanent magnet of Example and Comparative Example.
[0025] Figure 6 These are scanning transmission electron microscope images of the permanent magnets of the examples and comparative examples.
[0026] Figure 7 It is a graph showing magnetization curves of permanent magnets of Examples and Comparative Examples.
[0027] Figure 8This is a diagram showing a crystal growth model of the permanent magnet according to the present embodiment. DETAILED DESCRIPTION
[0028] Hereinafter, the permanent magnet, the manufacturing method and the device of this embodiment will be described. It should be noted that, unless otherwise specified, "to" indicating a numerical range includes the lower limit and the upper limit.
[0029] [Permanent magnet]
[0030] The permanent magnet according to the present embodiment has a composition represented by the following chemical formula (1):
[0031] Chemical formula (1): (R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c
[0032] in,
[0033] R represents at least one selected from rare earth elements,
[0034] T represents at least one selected from the group consisting of Fe, Co and Ni,
[0035] M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta and W,
[0036] a, b and c represent atomic %, x, y and z represent the ratio of Zr, Cu and M, respectively, and the following conditions are satisfied:
[0037] 5≤a≤10,
[0038] b = 100 - (a + c),
[0039] 3≤c≤20,
[0040] 0.01≤x≤0.5,
[0041] 0.001≤y≤0.1,
[0042] 0≤z≤0.1.
[0043] R in the chemical formula (1) represents a rare earth element. The rare earth elements involved in this embodiment are a general term for lanthanoid elements from La (lanthanum) to Lu (lutetium) and elements containing Sc (scandium) and Y (yttrium). R contains at least one element selected from the above rare earth elements. Since R is contained within a range where the ratio of R satisfies the above chemical formula (1), a permanent magnet with high magnetic anisotropy and high coercive force can be obtained. From the viewpoint of magnetic anisotropy and coercive force, R is preferably selected from Sm (samarium), Pr (praseodymium), Nd (neodymium), Ce (cerium), and La (lanthanum), and more preferably contains Sm. In addition, from the viewpoint of magnetic anisotropy and coercive force, in R, preferably 50 atomic % or more is Sm, preferably 80 atomic % or more is Sm, and more preferably R is substantially Sm.
[0044] The permanent magnet involved in this embodiment contains Zr in the range of R to Zr (zirconium) ratio (atomic %) of (1-x):x. Since Zr is contained in the above range, the content of M element described later can be suppressed, and ThMn 12 The ThMn type crystal structure is stabilized, and as a result, the saturation magnetization is improved. 12 From the viewpoint of stabilizing the type crystal structure, x may be 0.01 to 0.5, and from the viewpoint of magnetic anisotropy and coercive force, it is preferably 0.2 or less.
[0045] From ThMn 12 From the viewpoint of regarding the type crystal structure as the main phase, the total content ratio (a) of R and Zr relative to the entire permanent magnet according to the present embodiment is 5 to 10. From the viewpoint of improving magnetization, a is preferably 9 or less.
[0046] T in the chemical formula (1) represents at least one selected from the group consisting of Fe (iron), Co (cobalt) and Ni (nickel). Each element of T contributes to the magnetization of the permanent magnet. From the viewpoint of improving magnetization, T preferably contains Fe. In addition, from the viewpoint of increasing the Curie temperature and improving heat resistance, T preferably contains Co. From the viewpoint of improving magnetization, in T, preferably 50 atomic % or more is Fe, and preferably 60 atomic % or more is Fe. In addition, for example, when Fe and Co are used in combination, the ratio of Fe to Co (atomic %) is preferably 60:40 to 95:5, and more preferably 70:30 to 80:20. In the permanent magnet involved in this embodiment, the content ratio of T is represented by (1-yz).
[0047] From the viewpoint described later, the content ratio (Y) of Cu (copper) may be 0.001 to 0.1, and more preferably 0.005 to 0.05.
[0048] In the chemical formula (1), M represents at least one selected from the group consisting of C (carbon), N (nitrogen), Al (aluminum), Si (silicon), P (phosphorus), Ti (titanium), V (vanadium), Cr (chromium), Mn (manganese), Nb (niobium), Mo (molybdenum), Hf (hafnium), Ta (tantalum) and W (tungsten). Each element of M can increase the ThMn 12 The M content (z) may be 0 to 0.1, but it is not essential in the permanent magnet of the present embodiment.
[0049] The total content ratio (b) of T, Cu and M relative to the entire permanent magnet of this embodiment can be expressed as 100-(a+c). 12 From the viewpoint of regarding the type crystal structure as the main phase, b is 70 to 92. From the viewpoint of improving magnetization, b is preferably 75 or more, more preferably 77 or more.
[0050] In addition, the permanent magnet involved in this embodiment contains 3 to 20 atomic % of B (boron). Since B and Cu are contained within the above range, the crystallite size is reduced and the coercive force is increased. From the viewpoint of further increasing the coercive force, the B content ratio (c) is preferably 3 or more, and more preferably 5 or more. On the other hand, from the viewpoint of suppressing the decrease in saturation magnetization, the B content ratio (c) is preferably 20 or less, and more preferably 15 or less.
[0051] In addition, the permanent magnet involved in this embodiment may include a precipitate of a boride containing M in the chemical formula (1). For example, when the permanent magnet involved in this embodiment contains Ti as M, the permanent magnet may also contain a precipitate of titanium boride. It should be noted that the precipitate is not limited to borides. For example, when the permanent magnet involved in this embodiment contains Ti and C as M, the permanent magnet may also contain a carbide such as titanium carbide as a precipitate.
[0052] The boride or carbide precipitates contained in the permanent magnet according to the present embodiment are preferred because the finer the precipitates are, the smaller the grain size of the 1-12 phase can be. The average Feret diameter of the precipitates is preferably less than 20 nm.
[0053] Here, the Feret diameter is defined by the distance between two parallel lines circumscribed to the measurement object, and the maximum value thereof is referred to as the maximum Feret diameter. The Feret diameter and the maximum Feret diameter are obtained by analyzing an observation image obtained, for example, from a scanning electron microscope or a transmission electron microscope using image processing software. Therefore, the average Feret diameter of the precipitates is the average value of the maximum Feret diameters of the precipitates present in the observation field, and the average Feret diameter of the main phase grains is the average value of the maximum Feret diameters of the main phase grains present in the observation field.
[0054] The permanent magnet involved in the present embodiment may also contain inevitable impurities within the scope of achieving the effect of the present disclosure. The inevitable impurities are elements that are inevitably mixed from the raw materials or the manufacturing process, and are elements not included in the chemical formula (1) (elements other than R, T, M, Zr, Cu, and B). Specifically, O (oxygen), S (sulfur), Sn (tin), etc. can be cited, but are not limited to this. Relative to the total amount of the permanent magnet involved in the present embodiment, the proportion of inevitable impurities in the permanent magnet involved in the present embodiment is preferably less than 5 atomic %, more preferably less than 1 atomic %, and further preferably less than 0.1 atomic %.
[0055] The content ratio of each element in the permanent magnet according to the present embodiment can be measured using, for example, energy dispersive X-ray spectrometry (EDX: Energy dispersive X-ray spectrometry).
[0056] The permanent magnet according to the present embodiment satisfies the composition of the above chemical formula (1) and is a permanent magnet having: 12 The main phase of the 1-12 type crystal structure has a grain structure, and the grain boundary is a grain boundary. In addition, due to the presence of B and Cu, fine Cu is segregated in the grains, and the crystallite size of the 1-12 phase becomes smaller. Therefore, the permanent magnet involved in this embodiment has a ThMn 12 The type has excellent stability of crystal structure, saturation magnetization and heat resistance, and especially has high coercive force.
[0057] In addition, when the permanent magnet according to the present embodiment contains precipitates of boride or carbide, in the case where ThMn 12 In the main phase grains of the type crystal structure, the average Feret diameter (average grain diameter) is less than 100nm, and the coefficient of variation of the Feret diameter is preferably less than 0.4. Here, the coefficient of variation is an indicator of the size deviation of the grain diameter, and the coefficient of variation is obtained by dividing the standard deviation of the Feret diameter by the average Feret diameter.
[0058] Regarding the permanent magnet involved in the present embodiment, as an example, a permanent magnet having a coercive force (Hcj) exceeding 3.0 kOe can be obtained. In addition, regarding the permanent magnet involved in the present embodiment, as an example, a permanent magnet having a Curie temperature exceeding 400°C can be obtained. It should be noted that the structure of the grain boundary can be observed using a scanning transmission electron microscope (STEM: Scanning Transmission Electron Microscope). The Curie temperature can be measured using a vibrating sample magnetometer (VSM: Vibrating Sample Magnetometer). In addition, the coercive force can be obtained based on the JH curve obtained using a DC magnetization characteristic analyzer.
[0059] [Device]
[0060] The present disclosure may also provide a device having the permanent magnet involved in the present embodiment. As specific examples of such devices, clocks, motors, various instruments, communication equipment, computer terminal equipment, speakers, video disks, sensors, etc. may be cited. In addition, since the permanent magnet of the present disclosure is not easy to deteriorate even in a high temperature environment, it can also be appropriately used in angle sensors, ignition coils, hybrid electric vehicles (HEV) and other drive motors used in automobile engine compartments.
[0061] [Method for manufacturing permanent magnet]
[0062] The method for producing a permanent magnet according to the present embodiment comprises: step (I) of preparing a molten metal having a composition represented by the chemical formula (1); step (II) of heating the molten metal to a temperature of 50 to 100 °C. 7 K / sec to rapidly cool the melt to form an alloy; in step (III), the alloy is crushed into powder; in step (IV), the powder is formed into a formed body; in step (V), the formed body is sintered in a temperature range of 950°C to 1250°C to form a sintered body; and in step (VI), the sintered body is aged in a temperature range of 700°C to 900°C and then rapidly cooled.
[0063] According to the manufacturing method of the present embodiment, the permanent magnet of the present embodiment can be appropriately manufactured. The permanent magnet powder has ThMn 12 The main phase of the nanostructured carbon foam is composed of microcrystals.
[0064] First, prepare a melt having a composition represented by the above chemical formula (1) (step (I)). The melt can be prepared by obtaining a commercially available product of an alloy having the desired composition, or by preparing the alloy by blending each element into the desired composition. It should be noted that when there is a possibility of evaporation of elements in subsequent steps, adjustments are made so that the composition of the permanent magnet after manufacture satisfies chemical formula (1). The prepared alloy is dissolved to form a melt. The dissolution method can be appropriately selected from arc dissolution, high-frequency dissolution, etc.
[0065] Next, 50 to 10 7 The melt is rapidly cooled at a cooling rate of 50 K / sec or higher (step (II)). By rapidly cooling the melt at a cooling rate of 50 K / sec or higher, an amorphous phase can be formed, and fine crystals are obtained by heat treatment, so a permanent magnet with high coercivity can be obtained.
[0066] The alloy after rapid cooling can also be further heat treated to make the structure uniform. The rapid cooling rate is preferably 10 3 ~10 6 K / sec. In addition, from the viewpoint of forming an amorphous phase by rapid cooling, the above alloy is preferably in the form of a thin sheet. From the viewpoint of easy rapid cooling, the thickness of the thin sheet is preferably 1 to 100 μm, more preferably 20 to 90 μm. It should be noted that since the above alloy contains boron, the viscosity becomes low, so when the melt is rapidly cooled using a melt spinning method or the like, a thin sheet of the above thickness is easily obtained.
[0067] The crystallite size of the crystal structure can be evaluated, for example, by X-ray diffraction spectrum using the θ-2θ method. Specifically, the characteristic X-rays of CuKα are incident on the permanent magnet in the range of θ = 20° to 90°, and the X-ray diffraction spectrum of the permanent magnet is measured. Then, the crystallite size is calculated based on the half-value width (FWHM) of multiple 1-12 phase X-ray spectra containing 211 faces, and the average value is used as the crystallite size. Figure 1 is the half-value width (FWHM) of the peak corresponding to the 211 face of the 1-12 phase (211) ) and crystallite size, Figure 1 It is shown that the larger the half value width is, the smaller the crystallite size is.
[0068] Next, the alloy is crushed (step (III)). As an example of a method for crushing an alloy, first, the alloy is coarsely crushed by a crusher such as a disc mill in an inert atmosphere. In the case of poor crushability, the alloy may be subjected to a hydrogen storage treatment in advance. The hydrogen storage treatment makes the alloy brittle and becomes easier to coarsely crush.
[0069] Then, the coarsely pulverized material is further finely pulverized. The fine pulverization can be dry pulverization or wet pulverization. As dry pulverization, for example, jet milling method and the like can be mentioned. In addition, as wet pulverization, wet ball milling method and the like can be mentioned. During the pulverization process, a lubricant can also be added to give lubricity to the powder. In addition, the mixture of the organic solvent and the fine powder after pulverization is dried in an inert gas. The average particle size of the powder after fine pulverization can shorten the sintering time of the sintering step described later. In addition, from the viewpoint of manufacturing a uniform permanent magnet, the average particle size is preferably 1 to 10 μm.
[0070] Next, the obtained powder is pressurized to form a molded body of the desired shape (step (IV)). In the present disclosure, from the viewpoint of improving the magnetic properties by aligning the crystal orientation of the powder, it is preferred to perform pressurization in a constant magnetic field. The relationship between the direction of the magnetic field and the direction of pressurization is not particularly limited and can be appropriately selected according to the shape of the product, etc. For example, in the case of manufacturing an annular magnet or a thin plate-shaped magnet, a parallel magnetic field pressurization in which a magnetic field is applied in a direction parallel to the pressurization direction can be used. On the other hand, from the viewpoint of excellent magnetic properties, it is preferred to use a right-angle magnetic field pressurization in which a magnetic field is applied at right angles to the pressurization direction.
[0071] The size of the magnetic field is not particularly limited. It can be, for example, a magnetic field of less than 15 kOe or a magnetic field of more than 15 kOe, depending on the purpose of the product. Among them, from the viewpoint of excellent magnetic properties, it is preferred to perform press molding in a magnetic field of more than 15 kOe. In addition, the pressure during press molding can be appropriately adjusted according to the size and shape of the product. As an example, the pressure can be set to 0.5 to 2.0 ton / cm 2 That is, in the method for manufacturing a permanent magnet according to the present embodiment, from the viewpoint of magnetic properties, it is particularly preferred to conduct the magnetization in a magnetic field of 15 kOe or more at a temperature perpendicular to the magnetic field and 0.5 to 2.0 ton / cm 2 The powder was pressed and compacted at the following pressure.
[0072] Next, the formed body is sintered to form a sintered body (process (V)). The sintering temperature is preferably 950-1250°C, and more preferably 950-1100°C. If the temperature is too low, the sintered body will not be densified, and the residual magnetic flux density (Br) will decrease. In addition, if the temperature is too high, the grains will coarsen, resulting in a decrease in coercive force. In addition, the 1-12 phases may decompose. In addition, the sintering time is preferably 20-240 minutes, and more preferably 60-120 minutes. It should be noted that from the viewpoint of suppressing oxidation, the sintering process is preferably carried out in a vacuum of less than 1000 Pa or in an inert gas atmosphere. From the viewpoint of increasing the density of the sintered body, it is preferably sintered in a vacuum of less than 1000 Pa, and preferably sintered in a vacuum of less than 100 Pa.
[0073] After step (V), the obtained sintered body is preferably subjected to continuous aging treatment. By the aging treatment, ThMn 12 Type crystal structure. The aging treatment temperature is preferably 700-900°C, more preferably 800-900°C. If the temperature is too low, the aging treatment is not performed, and the crystal structure is difficult to homogenize, resulting in reduced magnetic properties. In addition, if the temperature is too high, the grains are coarsened, resulting in reduced coercivity. In addition, the 1-12 phase may decompose. The heat treatment time can be set to, for example, 0.5 to 20 hours, and can be preferably set to 1 to 10 hours.
[0074] Then, the sintered body after the heat treatment is rapidly cooled (step (VI)). The homogenized crystal structure can be maintained by rapid cooling. The rapid cooling rate in step (VI) may be 60 to 250°C / min, preferably 100 to 250°C / min.
[0075] In this way, the permanent magnet according to the present embodiment can be manufactured. The permanent magnet powder has ThMn 12 The main phase of the nanostructured carbon foam is composed of microcrystals.
[0076] [Method for producing permanent magnet powder]
[0077] The method for producing permanent magnet powder according to the present embodiment comprises: step (I) of preparing a molten metal having a composition represented by the above chemical formula (1); step (II) of heating the molten metal to a temperature of 50 to 100 °C; 7 K / sec to rapidly cool the melt to form an alloy; in step (III), the alloy is crystallized within a temperature range of 700°C to 900°C; and in step (IV), the alloy is crushed into powder.
[0078] According to the manufacturing method of the present embodiment, the permanent magnet powder of the present embodiment can be appropriately manufactured. The permanent magnet powder has ThMn 12 The main phase of the nanostructured carbon foam is composed of microcrystals.
[0079] First, a melt having a composition represented by the above chemical formula (1) is prepared (step (I)). 7 K / sec to rapidly cool the melt (step (II)). These steps can be performed by the same methods as steps (I) and (II) of the above-mentioned method for producing a permanent magnet, and detailed descriptions thereof will be omitted to avoid duplication.
[0080] Then, the alloy is precipitated and crystallized in a temperature range of 700°C to 900°C (step (III)). In order to increase the coercive force of the permanent magnet, the heat treatment temperature is preferably a higher temperature, and it is particularly preferred to be carried out at 800°C to 900°C. If the temperature is too low, the main phase crystals will not precipitate. On the other hand, if the temperature is too high, the grains will coarsen, resulting in a decrease in coercive force. In addition, the 1-12 phase may decompose.
[0081] After step (III), the obtained alloy is pulverized into powder (step (IV)). This step can be performed by the same method as step (III) of the above-mentioned method for producing a permanent magnet, and the details are omitted.
[0082] In this way, the permanent magnet powder according to the present embodiment can be manufactured. The permanent magnet powder has ThMn 12 The main phase of the nanostructured carbon foam is composed of microcrystals.
[0083] [Example]
[0084] Hereinafter, the present disclosure will be specifically described with reference to Examples and Comparative Examples, but it should be noted that the present disclosure is not limited to these descriptions.
[0085] (Example 1)
[0086] The specified amounts of raw material elements are weighed separately to produce the composition of Example 1 shown in Table 1, and a master alloy is obtained by high-frequency dissolution. The master alloy is again subjected to high-frequency dissolution, and the liquid is quenched by melt spinning to obtain alloy flakes. The alloy flakes are coarsely crushed with a vibration mill and finely crushed with a wet ball mill to obtain a raw material powder. The raw material powder is formed into a pressurized powder by applying pressure in a magnetic field. The pressurized powder is sintered at 950°C and continuously subjected to aging treatment at 900°C. After the aging treatment, it is quenched to obtain the permanent magnet of the sintered body of Example 1.
[0087] (Examples 2 to 8)
[0088] Predetermined amounts of raw material elements were weighed to obtain the compositions of Examples 2 to 8 shown in Table 1, and alloy flakes were prepared in the same manner as in Example 1. The alloy flakes were heated at 900°C to precipitate crystals. Then, the alloy flakes were coarsely pulverized with a vibration mill to obtain magnet powder.
[0089] (Comparative Examples 1 to 3)
[0090] Magnet powders were obtained in the same manner as in Examples 2 to 8 except that predetermined amounts of raw material elements were weighed to give the compositions of Comparative Examples 1 to 3 shown in Table 1.
[0091] [evaluate]
[0092] The X-ray diffraction spectra of the permanent magnets of the above-mentioned embodiments and comparative examples were measured, and the half-value width (FWHM) of the peak corresponding to the 211 face of the crystal structure of the 1-12 phase was obtained based on the obtained X-ray diffraction spectra, and its crystallite size was calculated. In addition, the JH curve of each permanent magnet was measured using a DC magnetization characteristic analyzer to obtain the coercive force (Hcj). The results are shown in Table 1.
[0093] [Table 1]
[0094]
[0095] As shown in Table 1, the permanent magnets of Examples 1 to 8 satisfying the composition of the above chemical formula (1), i.e., having a Cu ratio (y) of 0.001 or more and containing 3.0 atomic % or more of B (boron), have a crystallite size of less than 45 nm and a high coercive force.
[0096] Figure 2 (a) to (d) show the X-ray diffraction spectra of Example 2 and Comparative Examples 1 to 3 after quenching (in the figure, As-Q: As-Quenched), heating at 700°C, 800°C, and 900°C, respectively. It should be noted that the heating time is as follows: Figure 2 The peaks corresponding to the 211 plane of the 1-12 phase are indicated by Symbols indicate that the 1-12 phase diffraction peak of Example 2 is broader than that of Comparative Examples 1 to 3. The content of B (boron) in Example 2 is higher than that of Comparative Examples 1 to 3, indicating that an amorphous phase is formed during rapid cooling and that the grains are refined by heat treatment.
[0097] Figure 3 The figure shows the correlation between the peak half width of the X-ray diffraction spectrum and the heat treatment temperature when the composition of B (boron) is changed in the sample of Example 2. Figure 3 As shown, it can be seen that when the B (boron) content increases, the half value width tends to become larger even if a high temperature heat treatment is performed, and crystal growth is suppressed.
[0098] Figure 4 (a) and (b) show the magnetization curves of the samples of Example 2 and Comparative Example 1 after rapid cooling (As-Q) and after heating at 700°C, 800°C, and 900°C for 60 minutes. Figure 4 As shown in (a), it can be seen that in Example 2, the coercive force is increased by heat treatment. Figure 4 As shown in (b), in Comparative Example 1, the increase in coercivity due to the heat treatment is small.
[0099] Figure 5: This is a diagram showing the correlation between the amount of B (boron) added and the crystal grain size. It shows the X-ray diffraction spectra of the permanent magnets when the concentration of B (boron) contained in the permanent magnets is set to 0.8 atomic%, 2.0 atomic%, 4.0 atomic%, 5.0 atomic%, 6.0 atomic%, and 8.0 atomic%. The permanent magnets with a B (boron) concentration of 0.8 atomic% and the permanent magnets with a B (boron) concentration of 5.0 atomic% correspond to Comparative Example 2 and Example 2, respectively. Figure 5 (a) is the X-ray diffraction spectrum of the permanent magnet after quenching (As-Q), Figure 5 (b) is the X-ray diffraction spectrum of the permanent magnet after heating at 900°C for 60 minutes. According to the obtained X-ray diffraction spectrum, it can be seen that as the amount of B (boron) added increases, the peak of the 1-12 phase becomes broader, and by adding B (boron), crystal growth is suppressed even if high-temperature heat treatment is performed.
[0100] Figure 6 is a scanning transmission electron microscope (STEM) image of a permanent magnet after heating at 900°C for 60 minutes. Figure 6 (a) shows a STEM image of the permanent magnet of Example 2, Figure 6 (b) shows a STEM image of Comparative Example 2. The region surrounded by a circular mark indicates a region where precipitates of the Ti—B phase (boride) were observed.
[0101] Figure 7 The magnetization curves of the permanent magnets of Example 2 and Comparative Example 2 after heating at 900° C. for 60 minutes are shown. It is known that the coercive force increases with the increase in the amount of B (boron) added. Furthermore, in the magnetization curve of the permanent magnet of Example 2, good rectangularity is obtained.
[0102] Based on the above STEM images and magnetization curves, the average Feret diameter of the Ti-B phase, the average Feret diameter of the 1-12 phase, and the coefficient of variation of the Feret diameter of the 1-12 phase were calculated. The results are shown in Table 2.
[0103] [Table 2]
[0104]
[0105] As shown in Table 2, the permanent magnet of Comparative Example 2 in which B (boron) is less than 3.0 atomic % shows that the average Feret's diameter of the boride as the precipitate and the average Feret's diameter of the 1-12 phase are large, and the coefficient of variation of the Feret's diameter of the 1-12 phase is large, that is, the deviation in the size of the Feret's diameter (crystal grain size) of the 1-12 phase is large.
[0106] According to the results shown in the examples, using Figure 8, the mechanism of grain refinement expected when the permanent magnet involved in the present disclosure contains precipitates of boride or carbide is explained. Figure 8 (a) is Example 2, i.e., the crystal growth model of a permanent magnet having an amorphous morphology after rapid cooling, Figure 8 (b) is a crystal growth model of Comparative Example 2, that is, a permanent magnet whose morphology after rapid cooling is crystalline.
[0107] When the morphology after rapid cooling is amorphous, fine 1-12 phase crystals and borides or carbides begin to precipitate by heat treatment. Since the boride or carbide inhibits the growth of 1-12 phase crystals, fine and uniform grains are formed after heat treatment.
[0108] On the other hand, when the form after rapid cooling is crystalline, crystals and precipitates of boride or carbide are generated at the moment after rapid cooling. In addition, since the amount of precipitates is small, crystal growth is not hindered, and the grains of 1-12 phases increase during heat treatment. Therefore, after heat treatment, grains with larger particle size and larger deviation of particle size are formed.
[0109] Thus, the permanent magnet of the present disclosure has a ThMn 12 The fine crystallites composed of the main phase of the type crystal structure can have a high coercive force.
Claims
1. A permanent magnet, wherein: Having a composition represented by the following chemical formula (1), Chemical formula (1): (R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c in, R represents at least one selected from rare earth elements, T represents at least one selected from the group consisting of Fe, Co and Ni, M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta and W, a, b and c represent atomic %, x, y and z represent the ratio of Zr, Cu and M, respectively, and the following conditions are satisfied: 5≤a≤10、 b = 100 - (a + c), 3≤c≤20、 0.01≤x≤0.5、 0.001≤y≤0.1、 0≤z≤0.1。 2. The permanent magnet according to claim 1, wherein The permanent magnet comprises a main phase having ThMn 12 Type crystal structure, In the X-ray diffraction spectrum, the half-value width in the X-ray diffraction peak corresponding to the 211 plane of the crystal structure is 0.20° or more.
3. The permanent magnet according to claim 2, wherein: The crystallite size of the crystal structure calculated based on the X-ray diffraction spectrum is less than 45 nm.
4. The permanent magnet according to any one of claims 1 to 3, wherein: The permanent magnet has precipitates of boride or carbide having an average Feret diameter of less than 20 nm.
5. The permanent magnet according to claim 4, wherein: In the presence of ThMn 12 In the main phase grains of the type crystal structure, the average Feret diameter is less than 100 nm and the coefficient of variation of the Feret diameter is less than 0.
4.
6. The permanent magnet according to any one of claims 1 to 3, wherein 50 atomic % or more of the R is Sm.
7. The permanent magnet according to any one of claims 1 to 3, wherein 50 atomic % or more of the T is Fe.
8. The permanent magnet according to any one of claims 1 to 3, wherein: The coercivity exceeds 3kOe.
9. The permanent magnet according to any one of claims 1 to 3, wherein: The Curie temperature exceeds 400°C.
10. A device, wherein: A permanent magnet according to any one of claims 1 to 3.
11. A method for manufacturing a permanent magnet, wherein: A melt having a composition represented by the following chemical formula (1) is prepared. Chemical formula (1): (R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c in, R represents at least one selected from rare earth elements, T represents at least one selected from the group consisting of Fe, Co and Ni, M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta and W, a, b and c represent atomic %, x, y and z represent the ratio of Zr, Cu and M, respectively, and the following conditions are satisfied: 5≤a≤10、 b = 100 - (a + c), 3≤c≤20、 0.01≤x≤0.5、 0.001≤y≤0.1、 0≤z≤0.1, 50~10 7 K / sec to quench the melt to form an alloy, The alloy is crushed into powder, The powder is shaped to form a shaped body, sintering the formed body at a temperature ranging from 950° C. to 1250° C. to obtain a sintered body, The sintered body is subjected to aging treatment at a temperature ranging from 700° C. to 900° C. and then rapidly cooled.
12. A method for producing permanent magnet powder, wherein: A melt having a composition represented by the following chemical formula (1) is prepared. Chemical formula (1): (R 1-x Zr x ) a (T 1-y-z Cu y M z ) b B c in, R represents at least one selected from rare earth elements, T represents at least one selected from the group consisting of Fe, Co and Ni, M represents at least one selected from the group consisting of C, N, Al, Si, P, Ti, V, Cr, Mn, Nb, Mo, Hf, Ta and W, a, b and c represent atomic %, x, y and z represent the ratios of Zr, Cu and M, respectively, and the following conditions are satisfied: 5≤a≤10、 b = 100 - (a + c), 3≤c≤20、 0.01≤x≤0.5、 0.001≤y≤0.1、 0≤z≤0.1, 50~10 7 K / sec to quench the melt to form an alloy, The alloy is crystallized at a temperature ranging from 700°C to 900°C, The alloy is pulverized into powder.