Manufacturing method of embedded chip substrate and multilayer temporary bonding structure

Through the combination method of multi-layer temporary bonding structure and support plate, the problem of warping and cracking of the embedded substrate in the chip after landfilling the resin is solved, and the stability and reliability of the substrate are improved.

CN118943028APending Publication Date: 2024-11-12INST OF MICROELECTRONICS CHINESE ACAD OF SCI LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310533339.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing method of manufacturing embedded substrates in chips, the substrate is prone to warping and cracking after landfilling the resin, resulting in structural instability and affecting reliability.

Method used

Using a combination method of multi-layer temporary bonding structure and support plate, through multiple temporary bonding and debonding, the substrate is kept in a low warping state and the circuit processing is ensured that the resin completes all steps in the semi-cured state. , avoid excessive bending and cracking.

Benefits of technology

It effectively prevents warping and excessive bending of the substrate, improves the reliability and stability of the chip substrate, and avoids structural cracking and layering problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943028A_ABST
    Figure CN118943028A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of an embedded chip substrate and a multilayer temporary bonding structure, relates to the technical field of semiconductor packaging, and is used for solving the problems of warping and excessive bending of the substrate in the processing of the embedded chip substrate. The manufacturing method of the embedded chip substrate comprises the steps of substrate windowing, first temporary bonding, first chip pasting, first pressing and resin filling, second temporary bonding, second chip pasting, second pressing and resin filling, first pre-curing, blind hole processing, circuit manufacturing, insulating resin layer processing and the like. Through four times of temporary bonding and three times of de-bonding, a plurality of substrates are supported by the supporting plate in the steps of intermediate circuit, chip mounting, pre-curing and the like. Moreover, the manufacturing process of the intermediate circuits of the plurality of substrates is symmetrical processing, that is, the symmetrical intermediate circuits are manufactured on the substrates on the two sides of the supporting plate, so that the generated stresses are the same in magnitude and are mutually balanced, the substrates are always kept in a low-warping state in the processing process, and the substrates are prevented from being excessively bent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor packaging, and in particular to a method for manufacturing an embedded chip substrate and a multi-layer temporary bonding structure. Background Art

[0002] Embedding the chip in the substrate is an advanced packaging form. By embedding the bare chip in the substrate, the signal transmission distance between the chip and the packaging components on the substrate surface and between chips can be greatly reduced, the signal transmission loss can be reduced, and the signal transmission quality can be improved; at the same time, the package size can be reduced and the device usage space can be compressed.

[0003] At present, the main manufacturing method of embedded chip substrate is to dig a cavity in the core board of the printed circuit board, embed the bare chip, fill it with resin, and then perform multi-layer wiring on both sides of the core board to form a substrate.

[0004] In the existing chip embedded substrate manufacturing method, after one side of the substrate is filled with resin and then subjected to single-sided pressing, severe warping is prone to occur due to the asymmetry of the structure. During the insulation layer pressing and curing baking process on the other side of the substrate, the substrate is flattened again, so that the substrate forms repeated bends from warping to flattening. Due to the high modulus of the solidified embedded resin, excessive warping and flattening will cause the rigid resin to crack. The rigid embedded resin and chip interface have weak bonding strength, which will also cause interface cracking. Resin cracking and chip interface separation may cause the embedded substrate to fail, and even when the embedded substrate is in a humid environment, water vapor is enriched at the crack interface, leading to serious reliability problems such as burning of the embedded substrate. Therefore, how to reduce substrate warping during substrate processing and manufacturing is a technical problem in the processing and manufacturing of embedded substrates, and an important issue in improving the reliability of embedded substrates. Summary of the invention

[0005] The object of the present invention is to provide a method for manufacturing an embedded chip substrate and a multi-layer temporary bonding structure to avoid warping and excessive bending of the substrate during processing of the embedded chip substrate, thereby avoiding cracking and delamination of the formed structure.

[0006] A method for manufacturing an embedded chip substrate, comprising:

[0007] Opening windows on substrates, opening cavities for accommodating chips on multiple substrates;

[0008] A first temporary bonding is performed to bond the first surface of the first substrate having the accommodating cavity to the first bonding material layer, and a first supporting plate is fixed to a side of the first bonding material layer facing away from the first substrate;

[0009] A first chip mounting method is to place the chip in the accommodation cavity of the first substrate;

[0010] A first pressing and filling resin, pressing and filling the resin on the second surface of the first substrate to form a first resin layer;

[0011] Second temporary bonding, providing a second bonding material layer on a side of the first support plate away from the first bonding material layer, and bonding the second bonding material layer to the first surface of the second substrate having the accommodating cavity;

[0012] A second chip mounting method is to place the chip in the receiving cavity of the second substrate;

[0013] A second pressing and filling resin, pressing and filling the resin on the second surface of the second substrate to form a second resin layer;

[0014] The first pre-curing cures the resin in the formed structure to more than 50%;

[0015] Blind hole processing, opening blind holes on the upper and lower surfaces of the structure formed in the previous step;

[0016] Circuit fabrication, processing circuits on the upper and lower surfaces of the structure formed in the previous step;

[0017] Insulating resin layer processing, providing insulating resin layers on both the upper and lower surfaces of the structure formed in the previous step, and pre-curing to cure the insulating resin layer formed in this step to more than 50%;

[0018] First, an intermediate circuit is manufactured, and the steps of blind hole manufacturing, circuit manufacturing, and insulating resin layer manufacturing are repeated N times, where N≥0, to form a first temporary bonding structure;

[0019] Third temporary bonding, bonding a third bonding material layer on the side of the first temporary bonding structure having the first substrate, and a second supporting plate is provided on the side of the third bonding material layer facing away from the first temporary bonding structure; bonding a fourth bonding material layer on the side of the first temporary bonding structure having the second substrate, and a third supporting plate is provided on the side of the fourth bonding material layer facing away from the first temporary bonding structure;

[0020] A first debonding step is to debond the first surface of the first substrate from the first bonding material layer to obtain a second temporary bonding structure; and a first surface of the second substrate from the second bonding material layer to obtain a third temporary bonding structure;

[0021] Fourth temporary bonding: the first temporary bonding structure has a side of the first substrate bonded with a fifth bonding material layer, and the side of the third support plate of the third temporary bonding structure facing away from the fourth bonding material layer is bonded to the fifth bonding material layer; the first temporary bonding structure has a side of the second substrate bonded with a sixth bonding material layer, and the side of the second support plate of the second temporary bonding structure facing away from the third bonding material layer is bonded to the sixth bonding material layer, to obtain a fourth temporary bonding structure;

[0022] A second debonding step is to debond the first bonding material layer in the fourth temporary bonding structure from the first substrate, and to debond the second bonding material layer from the second substrate;

[0023] Second, the intermediate circuit is made. The upper surface and the lower surface of the structure formed in the previous step are both pressed and filled with resin to form a resin layer and pre-cured. The blind hole processing, circuit production and insulating resin layer processing are repeated M times, M≥0;

[0024] The third debonding is to debond the side of the fourth bonding material layer and the fifth bonding material layer away from the third support plate from the resin layer; and the side of the third bonding material layer and the sixth bonding material layer away from the second support plate from the resin layer;

[0025] Curing, curing the resin in the structure formed in the previous step to more than 90%;

[0026] Fabricating an outer layer circuit, performing blind hole processing and circuit fabrication steps on the cured structure to form an outer layer circuit;

[0027] Making a solder resist layer, making a solder resist layer on the surface of the outer layer circuit;

[0028] A coating is applied on the surface of the structure formed after the solder resist layer is made.

[0029] In one implementation, the first pre-curing is specifically: curing the resin in the structure formed in this step to 50%-70%; or, the first pre-curing is specifically: placing the formed structure in a constant temperature environment of 130°C-150°C for 20min-40min to pre-cure the resin in the structure.

[0030] In one implementation, the pre-curing in the insulating resin layer processing step is specifically: curing the insulating resin layer in the structure to a degree of 50%-70%; or, the pre-curing in the insulating resin layer processing step is specifically: placing the formed structure in a constant temperature environment of 130°C-150°C for 20min-40min to pre-cure the resin in the structure.

[0031] In one implementation, the curing is specifically: placing the formed structure in an environment with a constant temperature of 190° C.-210° C. and a vacuum degree of 8 Pa-15 Pa for 50 min-70 min to cure the resin in the structure.

[0032] In one implementation, the raw materials used in the first pressing and filling resin step, the second pressing and filling resin step, and the insulating resin layer processing step are all ABF resin sheets, and the ABF resin sheet includes an ABF main layer, an OPP film attached to the first side of the ABF main layer, and a PET film d attached to the second side of the ABF main layer.

[0033] In one implementation, the OPP film of the ABF resin sheet is removed in the first resin lamination and embedding step, the second resin lamination and embedding step, and the insulating resin layer processing step, and the PET film d of the ABF resin sheet is retained.

[0034] In one implementation, after the blind hole processing, the step of film removal is further included, in which the PET films d of the first resin layer and the second resin layer are removed.

[0035] A multi-layer temporary bonding structure, comprising a first support plate, a second support plate, a third support plate, a first bonding material layer, a second bonding material layer, a third bonding material layer, a fourth bonding material layer, a fifth bonding material layer, a sixth bonding material layer, a first semi-molded substrate, a second semi-molded substrate, a third semi-molded substrate and a fourth semi-molded substrate;

[0036] A first bonding material layer and a second bonding material layer are bonded to two sides of the first support plate respectively;

[0037] A third bonding material layer and a sixth bonding material layer are bonded to both sides of the second support plate, a side of the third bonding material layer facing away from the second support plate is bonded to a fourth semi-molded substrate, a side of the sixth bonding material layer facing away from the second support plate is bonded to one side of the third semi-molded substrate, and the other side of the third semi-molded substrate is bonded to a side of the second bonding material layer facing away from the first support plate;

[0038] A fourth bonding material layer and a fifth bonding material layer are bonded to both sides of the third support plate, respectively; a side of the fourth bonding material layer facing away from the second support plate is bonded to the first semi-molded substrate; a side of the fifth bonding material layer facing away from the third support plate is bonded to one side of the second semi-molded substrate; and the other side of the second semi-molded substrate is bonded to a side of the first bonding material layer facing away from the first support plate.

[0039] In one implementation, the structure of at least one of the first bonding material layer, the second bonding material layer, the third bonding material layer, the fourth bonding material layer, the fifth bonding material layer and the sixth bonding material layer includes a foaming film, a support film and a pressure-sensitive adhesive film stacked in sequence.

[0040] In one implementation, the debonding temperatures of the first bonding material layer and the second bonding material layer are at least 15° C. lower than the debonding temperatures of the third bonding material layer, the fourth bonding material layer, the fifth bonding material layer, and the sixth bonding material layer.

[0041] In the manufacturing method of the embedded chip substrate provided by the present application, a support plate is used to support the semi-formed substrate during the manufacturing process of all intermediate circuits. Specifically, through 4 temporary bonding and 3 debonding, multiple substrates are supported by the support plate in the steps of intermediate circuit processing, chip mounting and pre-curing, so that the substrates always maintain a low warpage state. In addition, the manufacturing process of the intermediate circuits of multiple substrates is symmetrical processing, that is, symmetrical intermediate circuits are manufactured on the substrates on both sides of the support plate, so that the stresses generated are the same and balanced, ensuring that the substrates always maintain a low warpage state during the processing process and preventing excessive bending of the substrates.

[0042] In addition, in the present application, each insulating resin layer is pre-cured after processing, and is not completely cured until all the resins are pressed and buried, and finally cured, so that the resin in the structure is cured to more than 90%. The resin in the embedded chip substrate is in a semi-cured state before curing. At this time, the modulus of the resin material in the embedded chip substrate is low, and the substrate is in a low stress and low warpage state. In this way, each step before curing is completed in a low warpage state, avoiding the warping and excessive bending of the substrate during the processing of the embedded chip substrate, thereby avoiding the cracking and delamination of the formed structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0044] Figure 1 A schematic diagram of a process for manufacturing a substrate with an embedded chip provided by an embodiment of the present invention;

[0045] Figure 2 The structure of the first substrate formed after the substrate window opening step provided in the embodiment of the present invention;

[0046] Figure 3 A structure formed after the first temporary bonding step provided by an embodiment of the present invention;

[0047] Figure 4The structure formed after the first chip mounting step provided in the embodiment of the present invention;

[0048] Figure 5 The structure formed after the first pressing and embedding resin step provided in the embodiment of the present invention;

[0049] Figure 6 A structure formed after the second temporary bonding step provided by an embodiment of the present invention;

[0050] Figure 7 The structure formed after the second chip mounting step provided in the embodiment of the present invention;

[0051] Figure 8 The structure formed after the second pressing and embedding resin step provided in the embodiment of the present invention;

[0052] Fig. 9 The structure formed after the blind hole processing step provided in the embodiment of the present invention;

[0053] Fig.10 The structure formed after the film stripping step provided in the embodiment of the present invention;

[0054] Fig.11 A structure formed after the circuit manufacturing steps provided in the embodiment of the present invention;

[0055] Fig.12 A first temporary bonding structure formed after the first step of making an intermediate circuit provided in an embodiment of the present invention;

[0056] Fig.13 A structure formed after the third temporary bonding step provided in an embodiment of the present invention;

[0057] Fig.14 A second temporary bonding structure formed after the first debonding step provided in an embodiment of the present invention;

[0058] Fig.15 A third temporary bonding structure formed after the first debonding step provided in an embodiment of the present invention;

[0059] Fig.16 A fourth temporary bonding structure formed after the fourth temporary bonding step provided in an embodiment of the present invention;

[0060] Fig.17 A schematic diagram of a first semi-molded substrate and a second semi-molded substrate obtained after the second debonding step provided in an embodiment of the present invention;

[0061] Fig.18 The structure formed after the second step of making the intermediate circuit provided in the embodiment of the present invention;

[0062] Fig.19A structure formed after the third debonding step provided in an embodiment of the present invention;

[0063] Fig. 20 The structure formed after the step of making the outer layer circuit provided in the embodiment of the present invention;

[0064] Fig.21 The structure formed after the step of making the solder resist layer provided in the embodiment of the present invention;

[0065] Fig. 22 A schematic structural diagram of a bonding material layer provided in an embodiment of the present invention.

[0066] Reference numerals:

[0067] 1-first substrate, 1a-accommodating cavity, 1b-substrate circuit, 2-first bonding material layer, 3-first supporting plate, 4-chip, 5-first resin layer, 6-second substrate, 7-second bonding material layer, 8-second resin layer, 9-blind hole, 10-intermediate circuit, 11-third bonding material layer, 12-second supporting plate, 13-fourth bonding material layer, 14-third supporting plate, 15-fifth bonding material layer, 16-sixth bonding material layer, 17-outer circuit, 18-solder resist layer;

[0068] A-first semi-molded substrate, B-second semi-molded substrate, C-third semi-molded substrate, D-fourth semi-molded substrate, a-foaming film, b-support film, c-pressure-sensitive adhesive film, d-PET film. DETAILED DESCRIPTION

[0069] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0070] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.

[0071] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.

[0072] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "front", "back", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.

[0073] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0074] See also Figure 1 , Figure 1 The flowchart of the embodiment provided by the present invention, the manufacturing method of the embedded chip 44 substrate in the embodiment comprises the steps of:

[0075] S1: Opening windows on substrates, opening accommodating cavities 1a for accommodating chips 4 on multiple substrates;

[0076] In step S1, the accommodating cavities 1a may be specifically opened on four substrates, including two first substrates 1 and two second substrates 6. That is, the accommodating cavities 1a are opened on four or more substrates, so as to place the chip 4 in the accommodating cavities in the subsequent steps.

[0077] In addition, in this step, the surface of the substrate may or may not have circuits. Figure 2 The middle substrate has a substrate circuit 1b. The specific substrate can be a resin substrate with no circuit on the surface or a double-sided copper-clad board with no circuit on the surface. Of course, copper circuits can also be set on the surface of the substrate. The accommodating cavity 1a opened on the substrate can be a through hole that runs through the thickness direction of the substrate. Specifically, the two sides of the substrate along the thickness direction of the substrate are the first surface and the second surface, respectively, or when the substrate is placed horizontally, that is, when the thickness direction of the substrate is along the vertical direction, the lower surface and the upper surface of the substrate are the first surface and the second surface, respectively. The structure formed after the window opening step of the first substrate 1 is as follows Figure 2 shown.

[0078] The substrate can be a BT (Bismaleimide Triazine) resin substrate or a FR4 material substrate. BT resin material has a very high glass transition temperature, excellent dielectric properties, low thermal expansion coefficient, good mechanical characteristics and other properties, which are more suitable for the production of substrates. FR4 is a code for a flame retardant material grade, which means that the resin material must be able to extinguish itself after burning. Of course, the substrate can also be made of other materials, which are not limited here.

[0079] S2: first temporary bonding, bonding the first surface of the first substrate 1 with the accommodating cavity 1 a to the first bonding material layer 2, and a first supporting plate 3 is fixed to a side of the first bonding material layer 2 facing away from the first substrate 1;

[0080] That is, the first bonding material layer 2 is bonded to the first surface of the first substrate 1 with the accommodating cavity 1a, and in this embodiment, the first surface of the first substrate 1 may be the lower surface of the first substrate 1. And a first supporting plate 3 is fixed to the side of the first bonding material layer 2 away from the first substrate 1.

[0081] like Fig. 20 As shown, the first bonding material layer 2 may include a foaming film a, a support film b and a pressure-sensitive adhesive film c stacked in sequence, and the foaming film a of the first bonding material layer 2 is bonded to the first surface of the first substrate 1. When the foaming film a is at the debonding temperature, it only takes a few minutes for the foaming film a to be debonded, and the first support plate 3 can fall off by itself, completing the debonding, which is easy to operate and does not require special equipment assistance.

[0082] A first support plate 3 is fixed to the side of the first bonding material layer 2 facing away from the first substrate 1, and the pressure-sensitive adhesive film c of the first bonding material layer 2 is bonded to the first support plate 3, that is, the first bonding material layer 2 is located between the first support plate 3 and the first substrate 1. The structure formed after the first temporary bonding step is as shown in FIG. Figure 3 As shown. In this embodiment, the first bonding material layer 2 can be a 3195N temporary bonding adhesive produced by Nitto Company with 170°C thermal foaming and debonding. Of course, other temporary bonding adhesives can also be selected according to actual conditions, which is not limited here. Of course, the first bonding material layer 2 can also be a single-layer film structure or other types of multi-layer film structures, which is not limited here.

[0083] It should be noted here that the first bonding material layer 2 can be first bonded to the first support plate 3 and then bonded to the first substrate 1. In this way, the first bonding material layer 2 is first bonded to the first support plate 3 for standby use. Of course, the first bonding material layer 2 can also be first bonded to the first substrate 1 and then bonded to the first support plate 3, which is not limited here.

[0084] S3: first attaching the chip 4, placing the chip 4 in the accommodating cavity 1a of the first substrate 1;

[0085] A chip 4 is placed in the receiving cavity 1a of the first substrate 1. In this step, the electrode side of the chip 4 can be oriented toward the side away from the first bonding material layer 2, that is, the electrode of the chip 4 is placed upward, or the electrode side of the chip 4 can be placed downward. When the receiving cavity 1a is a through hole, the chip 4 can be in contact with the first bonding material layer 2, and when the electrode side of the chip 4 is downward, its electrode is in contact with the first bonding material layer 2. The structure formed after the chip 4 attachment step is as follows: Figure 4 shown.

[0086] When the first bonding material layer 2 includes a foaming film a, a supporting film b and a pressure-sensitive adhesive film c stacked in sequence, the chip 4 can contact the foaming film a of the first bonding material layer 2. Specifically, when the electrode side of the chip 4 is facing downward, its electrode contacts the foaming film a of the first bonding material layer 2.

[0087] Preferably, when the chip 4 is attached to the accommodating cavity 1a of the first substrate 1, the electrode side of the chip 4 can be oriented toward the side away from the first bonding material layer 2, that is, the electrode of the chip 4 faces upward, so that the foaming film a of the first bonding material layer 2 does not contact the chip 4 electrode, but contacts the back of the chip 4, which can prevent the chip 4 electrode surface from being contaminated, causing contamination to cause contaminants to be buried in the substrate and form serious reliability problems. Alternatively, the surface of the chip 4 has a protective film to prevent the chip 4 electrode surface from being contaminated. After the bonding is released, the protective film on the surface of the chip 4 can be removed. The protective film can be a copper foil or a film of other materials.

[0088] S4: first pressing and filling resin, pressing and filling resin on the second surface of the first substrate 1 to form a first resin layer 5;

[0089] That is, the embedding resin is pressed on the second surface of the first substrate 1, and the embedded resin forms the first resin layer 5. In this embodiment, the second surface of the first substrate 1 can be the upper surface of the first substrate 1. The embedding resin is pressed on the second surface of the first substrate 1, and specifically, a vacuum laminator can be used to press the resin on the second surface of the first substrate 1. During the process of pressing the embedding resin, the resin fills the gaps between the circuits on the surface of the first substrate 1 and the gaps around the chip 4. The structure formed after the first step of pressing and embedding the resin is as follows: Figure 5 shown.

[0090] The surface of the first resin layer 5 may be provided with a protective film, which may be removed before or after the blind hole 9 processing step. The protective film may prevent the first resin layer 5 from being contaminated.

[0091] In the first pressing and embedding resin step, an ABF (Ajinomoto Buildup FIlm) resin sheet can be selected. The ABF resin sheet includes an ABF layer, an OPP (O-phenylphenol) film attached to a first side of the ABF layer, and a PET (polyethylene glycol terephthalate) film attached to a second side of the ABF layer.

[0092] In the first lamination and resin embedding step, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is lamination-bonded to the second side of the first substrate 1 to form a first resin layer 5, and the side of the first resin layer 5 facing away from the first substrate 1 retains the PET film d. That is, in this step, the OPP film of the ABF resin sheet is torn off and the PET film d is retained. The ABF resin sheet is lamination-bonded to the second side of the first substrate 1 on one side of the OPP film removed.

[0093] Specifically, a vacuum laminator can be used for low-temperature vacuum lamination to press the ABF resin sheet with the OPP film removed onto the second surface of the first substrate 1. In this step, the ABF resin sheet is only laminated and leveled in the vacuum laminator. The vacuum laminator includes a vacuum laminating section and a leveling section. The vacuum laminating section is mainly used to press the ABF resin sheet onto the second surface of the first substrate 1. Since the surface of the inner layer circuit is uneven, the surface of the ABF resin sheet is still uneven after laminating by the vacuum laminating section. Then the leveling section levels the ABF resin sheet to make the surface of the ABF resin sheet flat.

[0094] The resin may be a GXT31 ABF resin sheet. Of course, the resin may also be a semi-cured PP (Prepreg) sheet or a copper-clad resin sheet RCC (Resin Coated Copper), the protective film of which is a copper foil layer, which is not limited here.

[0095] S5: second temporary bonding, disposing a second bonding material layer 7 on a side of the first support plate 3 away from the first bonding material layer 2, and bonding the second bonding material layer 7 to a first surface of the second substrate 6 having the accommodating cavity 1a;

[0096] That is, the second bonding material layer 7 is bonded to the side of the first support plate 3 facing away from the first bonding material layer 2, and the side of the second bonding material layer 7 facing away from the first support plate 3 is bonded to the first surface of the second substrate 6, that is, the second bonding material layer 7 is located between the first support plate 3 and the second substrate 6. In this embodiment, the first surface of the second substrate 6 can be the upper surface of the second substrate 6.

[0097] like Fig.18As shown, the second bonding material layer 7 may also include a foaming film a, a support film b and a pressure-sensitive adhesive film c stacked in sequence, and the foaming film a of the second bonding material layer 7 is bonded to the first surface of the second substrate 6. When the foaming film a is at the debonding temperature, it only takes a few minutes for the foaming film a to be debonded and the first support plate 3 to fall off by itself. The debonding is easy to operate and does not require special equipment assistance.

[0098] The pressure-sensitive adhesive film c of the second bonding material layer 7 is bonded to the first support plate 3, that is, the second bonding material layer 7 is located between the first support plate 3 and the second substrate 6. The structure formed after the second temporary bonding step is as follows: Figure 6 As shown. In this embodiment, the second bonding material layer 7 can be a 3195N temporary bonding adhesive produced by Nitto Company with 170°C thermal foaming and debonding. Of course, other temporary bonding adhesives can also be selected according to actual conditions, which is not limited here. Of course, the second bonding material layer 7 can also be a single-layer film structure or other types of multi-layer film structures, which is not limited here.

[0099] It should be noted here that the second bonding material layer 7 can be first bonded to the first support plate 3 and then bonded to the second substrate 6. In this way, the second bonding material layer 7 can be first bonded to the first support plate 3 for standby use. Of course, the second bonding material layer 7 can also be first bonded to the second substrate 6 and then bonded to the first support plate 3, which is not limited here.

[0100] S6: attaching the second chip 4, placing the chip 4 in the accommodating cavity 1a of the second substrate 6;

[0101] The chip 4 is arranged in the accommodating cavity 1a of the second substrate 6. In this step, the electrode side of the chip 4 can be oriented toward the side away from the second bonding material layer 7, that is, the electrode of the chip 4 is placed downward, and the electrode side of the chip 4 can also be placed upward. When the accommodating cavity 1a is a through hole, the chip 4 can be in contact with the second bonding material layer 7, and when the electrode side of the chip 4 is upward, its electrode is in contact with the second bonding material layer 7.

[0102] When the second bonding material layer 7 includes a foaming film a, a supporting film b and a pressure-sensitive adhesive film c stacked in sequence, the chip 4 can be in contact with the foaming film a of the second bonding material layer 7, so that the chip 4 can be fixed in the accommodating cavity 1a by using the foaming film a. Specifically, when the electrode side of the chip 4 is facing upward, its electrode is in contact with the foaming film a of the second bonding material layer 7. The structure formed after the chip 4 is attached is as follows: Figure 7 shown.

[0103] Preferably, when the chip 4 is attached in the accommodating cavity 1a of the second substrate 6, the electrode side of the chip 4 can be oriented toward the side away from the second bonding material layer 7, that is, the electrode of the chip 4 faces downward, so that the foaming film a of the second bonding material layer 7 does not contact the chip 4 electrode, but contacts the back of the chip 4, which can prevent the chip 4 electrode surface from being contaminated, causing contamination to cause contaminants to be buried in the substrate to form serious reliability problems. It should be noted here that the chip 4 in the accommodating cavity 1a of the first substrate 1 and the chip 4 in the accommodating cavity 1a of the second substrate 6 can be arranged in opposite directions to be symmetrically arranged relative to the first support plate 3. That is, the back of the chip 4 in the accommodating cavity 1a of the first substrate 1 contacts the first bonding material layer 2, and the back of the chip 4 in the accommodating cavity 1a of the second substrate 6 contacts the second bonding material layer 7. Alternatively, the surface of the chip 4 has a protective film to prevent the chip 4 electrode surface from being contaminated. After the bonding is released, the protective film on the surface of the chip 4 can be removed, and the protective film can be a film of copper foil or other materials.

[0104] S7: second pressing and filling resin, pressing and filling resin on the second surface of the second substrate 6 to form a second resin layer 8;

[0105] That is, the second surface of the second substrate 6 is pressed and filled with resin, and the filled resin forms a second resin layer 8. In this embodiment, the second surface of the second substrate 6 can be the lower surface of the second substrate 6. The second surface of the second substrate 6 is pressed and filled with resin, and specifically, a vacuum laminator can be used to press the resin on the second surface of the second substrate 6. During the pressing and filling resin process, the resin fills the gaps between the surface circuits on the second surface of the second substrate 6 and the gaps around the chip 4. The structure formed after the second pressing and filling resin step is as follows: Figure 8 It is worth noting that no pre-curing is performed in the first pressing and embedding resin step and the second pressing and embedding resin step.

[0106] The surface of the second resin layer 8 may be provided with a protective film, which may be removed before or after the blind hole 9 processing step. The protective film may prevent the second resin layer 8 from being contaminated.

[0107] In the second pressing and embedding resin step, an ABF (Ajinomoto Buildup FIlm) resin sheet can also be selected. In the second pressing and embedding resin step, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is pressed on the second side of the second substrate 6 to form a second resin layer 8, and the side of the second resin layer 8 facing away from the second substrate 6 retains the PET film d. That is, in this step, the OPP film of the ABF resin sheet is torn off and the PET film d is retained. The ABF resin sheet removes one side of the OPP film and is pressed on the second side of the second substrate 6.

[0108] In this way, the PET film d can protect the ABF layer, and the PET film d can be torn off before or after processing the blind hole 9. The process of laminating the second resin layer 8 is also carried out in the vacuum laminator, which will not be described in detail here.

[0109] In this step, the resin can be specifically selected from the ABF resin sheet of model GXT31. Of course, the resin can also be a semi-cured PP sheet or a copper-clad resin sheet RCC, which is not limited here.

[0110] S8: first pre-curing, curing the resin in the formed structure to more than 50%;

[0111] After the first resin layer 5 and the second resin layer 8 are pressed and buried, the first pre-curing is performed, that is, after the first resin layer 5 is pressed and buried, the pre-curing is not performed before the second resin layer 8 is pressed and buried.

[0112] Specifically, the resin in the structure formed in the previous step is cured to more than 50%, or in other words, the resin in the structure formed in the previous step is cured to a degree of curing of more than 50%, so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. The resin in the structure formed in this step can be cured to 50%, 60%, 70%, etc., but the first pre-curing can be low-temperature thermal curing, so that the first resin layer 5 and the second resin layer 8 are cured to a certain extent, but not completely cured. Before this step, no pre-curing treatment is performed. The first pre-curing can be performed in an oven.

[0113] S9: Processing blind holes 9, opening blind holes 9 on the upper and lower surfaces of the structure formed in the previous step;

[0114] That is, blind holes 9 are opened on the upper and lower surfaces of the structure formed in the previous step of processing the blind holes 9. In this embodiment, blind holes 9 are opened on the surfaces of the first resin layer 5 and the second resin layer 8 so that the circuits covered by the first resin layer 5 and the second resin layer 8 are electrically connected to other circuits through the blind holes 9. Specifically, the blind holes 9 can be opened by laser drilling. The structure formed after the blind hole 9 processing step is as follows Fig. 9 shown.

[0115] S10: circuit fabrication, processing circuits on the upper and lower surfaces of the structure formed in the previous step;

[0116] Specifically, circuits are processed on both the upper and lower surfaces of the structure formed by processing the blind hole 9. In this embodiment, the circuits can be processed on the surfaces of the first resin layer 5 and the second resin layer 8, and the circuits processed on the surfaces of the first resin layer 5 and the second resin layer 8 are electrically connected to the substrate circuit 1b through the blind hole 9. The structure formed after the circuit manufacturing step is as shown in FIG. Fig.11 shown.

[0117] S11: Insulating resin layer processing, insulating resin layers are provided on both the upper surface and the lower surface of the structure formed in the previous step, and pre-curing is performed to cure the insulating resin layer formed in this step to more than 50%;

[0118] That is, the upper and lower surfaces of the structure formed in the previous step are pressed and filled with resin. In this embodiment, an insulating resin layer is formed on the upper and lower surfaces of the structure formed in the circuit making step. The resin fills the gaps between the circuits formed in the circuit making step. The insulating resin layer formed in this step covers the circuit formed in the circuit making step and is partially in contact with the first resin layer 5 or the second resin layer 8. And pre-curing is performed to cure the insulating resin layer formed in this step to more than 50%, or to cure the resin in the structure formed in this step to a degree of curing of more than 50%, so that the resin is hardened and the rigidity and mechanical impact resistance of the resin are improved. The resin in the structure formed in this step can be cured to 50%, 60%, 70%, etc. This pre-curing is the second pre-curing, and the second pre-curing can be low-temperature thermal curing, so that the resin in the formed structure is cured to a certain extent, but not completely cured. The pre-curing in the insulating resin layer processing step can also be carried out in an oven.

[0119] The insulating resin layer may also be an ABF resin sheet. In the processing of the insulating resin layer, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is pressed on the upper surface or the lower surface of the structure formed in the previous step, and pre-cured. A PET film d is retained on one side of the insulating resin layer to protect the insulating resin layer from contamination.

[0120] In this step, the insulating layer resin can be specifically selected from the ABF resin sheet of model GXT31. Of course, the resin can also be a semi-cured PP sheet or a copper-clad resin sheet RCC, which is not limited here.

[0121] S12: first manufacturing an intermediate circuit, repeating the steps of blind hole 9 manufacturing, circuit manufacturing and insulating resin layer manufacturing N times, N≥0, to form a first temporary bonding structure;

[0122] Among them, the steps of blind hole 9 processing, circuit manufacturing and insulating resin layer processing are repeated N times, N≥0. When N>0, N layers of intermediate circuits 10 can be processed in this step. When N=0, the outer layer circuit 17 is directly processed. That is, each time the steps of blind hole 9 processing, circuit manufacturing and insulating resin layer processing are repeated, one layer of intermediate circuit 10 is processed. It should be noted here that in the first step of manufacturing intermediate circuit 10, N layers of intermediate circuit 10 are processed on the second side of the first substrate 1 and the second side of the second substrate 6. The second side of the first substrate 1 is the side of the first substrate 1 with the second surface, and the second side of the second substrate 6 is the side of the second substrate 6 with the second surface. The intermediate circuit 10 of the embedded chip 4 substrate refers to each layer of circuit between the substrate and the outermost circuit 17. The method for manufacturing the embedded chip 4 substrate provided in this application can process substrates of any number of layers, and is not limited to odd or even layers.

[0123] The key point of this embodiment is that each time a layer of intermediate circuit 10 is processed and an insulating resin layer is provided on the circuit surface, a pre-curing is performed, and the curing is not complete. The structure formed after the first step of making the intermediate circuit 10 is a first temporary bonding structure, such as Fig.12 shown.

[0124] S13: third temporary bonding, bonding a third bonding material layer 11 to a side of the first temporary bonding structure having the first substrate 1, and a second supporting plate 12 is provided on a side of the third bonding material layer 11 facing away from the first temporary bonding structure; bonding a fourth bonding material layer 13 to a side of the first temporary bonding structure having the second substrate 6, and a third supporting plate 14 is provided on a side of the fourth bonding material layer 13 facing away from the first temporary bonding structure;

[0125] Specifically, the third bonding material layer 11 is bonded to the side of the first temporary bonding structure having the first substrate 1. In this embodiment, the third bonding material layer 11 is bonded to the upper surface of the first temporary bonding structure. In addition, a second support plate 12 is provided on the side of the third bonding material layer 11 away from the first temporary bonding structure, that is, the second support plate 12 is bonded to the side of the third bonding material layer 11 away from the first temporary bonding structure, and the third bonding material layer 11 is located between the second support plate 12 and the third bonding material layer 11.

[0126] When the third bonding material layer 11 includes a foaming film a, a supporting film b and a pressure-sensitive adhesive film c stacked in sequence, the foaming film a of the third bonding material layer 11 is bonded to the upper surface of the first temporary bonding structure, and the pressure-sensitive adhesive film c of the third bonding material layer 11 is bonded to the second supporting plate 12.

[0127] In this embodiment, the third bonding material layer 11 can be a 31950E temporary bonding adhesive produced by Nitto that is heat-foamed and debonded at 200°C-210°C. The fourth bonding material layer 13 can also be a 31950E temporary bonding adhesive produced by Nitto that is heat-foamed and debonded at 200°C-210°C. Of course, other temporary bonding adhesives can be selected according to actual conditions, which is not limited here. Of course, the third bonding material layer 11 and the fourth bonding material layer 13 can also be a single-layer film structure or other types of multi-layer film structures, which are not limited here.

[0128] In addition, a fourth bonding material layer 13 is bonded to the side of the first temporary bonding structure having the second substrate 6. In this embodiment, the fourth bonding material layer 13 is bonded to the lower surface of the first temporary bonding structure. In addition, a third support plate 14 is provided on the side of the fourth bonding material layer 13 away from the first temporary bonding structure, that is, the third support plate 14 is bonded to the side of the fourth bonding material layer 13 away from the first temporary bonding structure, and the fourth bonding material layer 13 is located between the third support plate 14 and the third bonding material layer 11.

[0129] When the fourth bonding material layer 13 includes a foaming film a, a supporting film b and a pressure-sensitive adhesive film c stacked in sequence, the foaming film a of the fourth bonding material layer 13 is bonded to the lower surface of the first temporary bonding structure, and the pressure-sensitive adhesive film c of the fourth bonding material layer 13 is bonded to the third supporting plate 14. The structure formed after the third temporary bonding step is as follows: Fig.13 shown.

[0130] Among them, the first support plate 3, the second support plate 12 and the third support plate 14 can be double-sided copper-clad plates, metal plates, glass plates or ceramic plates with high rigidity, or the material can be BT resin. The first support plate 3, the second support plate 12 and the third support plate 14 can be double-sided copper-clad plates made of BT resin. The thickness of the first support plate 3, the second support plate 12 and the third support plate 14 can be greater than or equal to 0.5mm. Specifically, the thickness of the first support plate 3, the second support plate 12 and the third support plate 14 can be 0.5mm, 0.6mm, 0.7mm, 0.8mm, etc., so that the strength of multiple support plates can be ensured to prevent the substrate from warping during processing.

[0131] S14: first debonding, debonding the first surface of the first substrate 1 from the first bonding material layer 2 to obtain a second temporary bonding structure; debonding the first surface of the second substrate 6 from the second bonding material layer 7 to obtain a third temporary bonding structure;

[0132] Specifically, after the first surface of the first substrate 1 is debonded from the first bonding material layer 2, the first substrate 1 and the intermediate circuit 10 processed on the second side thereof, the third bonding material layer 11 and the second support plate 12 together form a second temporary bonding structure. The structural schematic diagram of the second temporary bonding structure is as shown in FIG. Fig.14 After the first surface of the second substrate 6 and the second bonding material layer 7 are debonded, the second substrate 6 and the intermediate circuit 10 processed on the second side thereof, the fourth bonding material layer 13 and the third support plate 14 together form a third temporary bonding structure. The structural schematic diagram of the third temporary bonding structure is shown in FIG. Fig.15 shown.

[0133] The first debonding can be a low-temperature debonding, that is, in the S14 step, the first surface of the first substrate 1 is debonded from the first bonding material layer 2, and the first surface of the second substrate 6 is debonded from the second bonding material layer 7, and the two sides of the third bonding material layer 11 and the two sides of the fourth bonding material layer 13 are still kept bonded. Specifically, the third bonding material layer 11, the second support plate 12 and the first temporary bonding structure are not debonded in the S14 step and are still kept bonded, and the fourth bonding material layer 13, the third support plate 14 and the first temporary bonding structure are not debonded in the S14 step and are still kept bonded.

[0134] S15: fourth temporary bonding, the first temporary bonding structure has a side of the first substrate 1 bonded with a fifth bonding material layer 15, the side of the third support plate 14 of the third temporary bonding structure facing away from the fourth bonding material layer 13 is bonded to the fifth bonding material layer 15; the first temporary bonding structure has a side of the second substrate 6 bonded with a sixth bonding material layer 16, the side of the second support plate 12 of the second temporary bonding structure facing away from the third bonding material layer 11 is bonded to the sixth bonding material layer 16, to obtain a fourth temporary bonding structure;

[0135] Specifically, the resin layer on the surface of the first temporary bonding structure on one side of the first substrate 1 is bonded to the fifth bonding material layer 15. In this embodiment, the upper surface of the first temporary bonding structure is bonded to the fifth bonding material layer 15. The fifth bonding material layer 15 is bonded to the side facing away from the first temporary bonding structure and to the third support plate 14 of the third temporary bonding structure. In this embodiment, the fifth bonding material layer 15 is bonded to the side facing away from the first temporary bonding structure and to the lower surface of the third temporary bonding structure, and the fifth bonding material layer 15 is located between the first temporary bonding structure and the third temporary bonding structure.

[0136] When the fifth bonding material layer 15 includes a foaming film a, a support film b and a pressure-sensitive adhesive film c stacked in sequence, the foaming film a of the fifth bonding material layer 15 is bonded to the resin layer on the surface of the first temporary bonding structure, and the pressure-sensitive adhesive film c of the fifth bonding material layer 15 is bonded to the third support plate 14. The fifth bonding material layer 15 can also be a 31950E temporary bonding adhesive produced by Nitto Company with a temperature of 200°C-210°C for thermal foaming and debonding. Of course, other temporary bonding adhesives can also be selected according to actual conditions, which are not limited here.

[0137] In addition, the surface resin layer of the first temporary bonding structure on one side of the second substrate 6 is bonded to the sixth bonding material layer 16. In this embodiment, the lower surface of the first temporary bonding structure is bonded to the sixth bonding material layer 16. The sixth bonding material layer 16 is bonded to the side facing away from the first temporary bonding structure and to the second support plate 12 of the second temporary bonding structure. In this embodiment, the sixth bonding material layer 16 is bonded to the side facing away from the first temporary bonding structure and to the upper surface of the second temporary bonding structure, and the sixth bonding material layer 16 is located between the first temporary bonding structure and the second temporary bonding structure.

[0138] When the sixth bonding material layer 16 includes a foaming film a, a support film b and a pressure-sensitive adhesive film c stacked in sequence, the foaming film a of the sixth bonding material layer 16 is bonded to the resin layer on the surface of the first temporary bonding structure, and the pressure-sensitive adhesive film c of the sixth bonding material layer 16 is bonded to the second support plate 12. The sixth bonding material layer 16 can also be the 200℃-210℃ heat-foamed debonding 31950E temporary bonding adhesive produced by Nitto. Of course, other temporary bonding adhesives can also be selected according to actual conditions, which is not limited here. Of course, the fifth bonding material layer 15 and the sixth bonding material layer 16 can also be single-layer film structures or other types of multi-layer film structures, which are not limited here.

[0139] The structure formed after the fourth temporary bonding step is a fourth temporary bonding structure, such as Fig.16 As shown, it includes a third temporary bonding structure, a fifth bonding material layer 15, a first temporary bonding structure, a sixth bonding material layer 16 and a second temporary bonding structure bonded sequentially from top to bottom. It is worth noting that the fourth temporary bonding structure includes four semi-molded substrates, six bonding material layers and three support plates, wherein the semi-molded substrate is a substrate for embedded chips 4 generated during the processing and not yet fully processed, that is, a substrate that has not yet been fully formed. The four semi-molded substrates are the first semi-molded substrate A, the second semi-molded substrate B, the third semi-molded substrate C and the fourth semi-molded substrate D.

[0140] S16: second debonding, debonding the first bonding material layer 2 and the first substrate 1 in the fourth temporary bonding structure, and debonding the second bonding material layer 7 and the second substrate 6;

[0141] Specifically, the first surface of the first substrate 1 in the fourth temporary bonding structure is debonded from the first bonding material layer 2, and the first surface of the second substrate 6 is debonded from the second bonding material layer 7, but after the second debonding step, both sides of the third bonding material layer 11, both sides of the fourth bonding material layer 13, both sides of the fifth bonding material layer 15, and both sides of the sixth bonding material layer 16 are still bonded. Specifically, the third bonding material layer 11 is not debonded from the second support plate 12 and the resin layer of the semi-molded substrate in the S16 step and is still bonded, the fourth bonding material layer 13 is not debonded from the third support plate 14 and the resin layer of the semi-molded substrate in the S16 step and is still bonded, the fifth bonding material layer 15 is not debonded from the third support plate 14 and the resin layer of the semi-molded substrate in the S16 step and is still bonded, and the sixth bonding material layer 16 is not debonded from the second support plate 12 and the resin layer of the semi-molded substrate in the S16 step and is still bonded.

[0142] After the second debonding step, two temporary structures with the same structure are obtained, one of which is Fig.16 After the second debonding step, the two structures obtained are both semi-molded substrates with single-sided multi-layer wiring bonded on both sides of a support plate, and the semi-molded substrates with single-sided multi-layer wiring on both sides of the support plate are symmetrically arranged. Therefore, the stress distributions formed by the semi-molded substrates with single-sided multi-layer wiring on both sides of the support plate relative to the support plate are the same in magnitude and balanced with each other, which can effectively reduce the warping of the substrate during processing.

[0143] S17: secondly making the intermediate circuit, pressing and filling the resin on the upper and lower surfaces of the structure formed in the previous step to form a resin layer and pre-curing, repeating the steps of blind hole 9 processing, circuit production and insulating resin layer processing M times, M≥0;

[0144] That is, the upper and lower surfaces of the structure formed in the previous step are pressed and filled with resin. In this embodiment, after the second debonding step, the upper and lower surfaces of the two temporary structures with the same structure are pressed and filled with resin to form a resin layer. And pre-curing is carried out to cure the resin layer formed in this step to more than 50%, or in other words, the resin in the structure formed in this step is cured to a degree of curing of more than 50%, so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. The resin in the structure formed in this step can be cured to 50%, 60%, 70%, etc., and this pre-curing can be low-temperature thermal curing, so that the resin in the formed structure is cured to a certain extent, but not completely cured.

[0145] An ABF resin sheet may also be used in this step. In this step, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is pressed onto the upper surface or the lower surface of the structure formed in the previous step, and pre-cured. A PET film d is retained on one side of the resin layer to protect the resin layer from contamination.

[0146] In this step, the resin can be specifically selected from the ABF resin sheet of model GXT31. Of course, the resin can also be a semi-cured PP sheet or a copper-clad resin sheet RCC, which is not limited here.

[0147] Then, the blind hole 9 processing, circuit manufacturing and insulating resin layer processing steps are repeated M times, M≥0. When M>0, M layers of intermediate circuits 10 can be processed in this step. When M=0, the outer layer circuit 17 is directly processed. That is, each time the blind hole 9 processing, circuit manufacturing and insulating resin layer processing steps are repeated once, one layer of intermediate circuit 10 is processed. It should be noted here that in the first step of manufacturing the intermediate circuit 10, M layers of intermediate circuits 10 are processed on the first side of the first substrate 1 and the first side of the second substrate 6. The first side of the first substrate 1 is the side of the first substrate 1 having the first surface, and the first side of the second substrate 6 is the side of the second substrate 6 having the first surface. The intermediate circuit 10 of the embedded chip 4 substrate refers to each layer of circuits between the substrate and the outermost circuit 17.

[0148] The key point of this embodiment is that each time a layer of intermediate circuit 10 is processed and an insulating resin layer is provided on the circuit surface, a pre-curing is performed, and the curing is not complete. The structure formed after the second step of making the intermediate circuit 10 is as follows Fig.18 shown.

[0149] To ensure that the number of circuit layers on both sides of the first substrate 1 is the same as that on both sides of the second substrate 6, M = N. Of course, M can also be greater than or less than N, so that asymmetric first substrates 1 and second substrates 6 can be processed, which is not limited here.

[0150] S18: third debonding, debonding the side of the fourth bonding material layer 13 and the fifth bonding material layer 15 away from the third support plate 14 from the resin layer; debonding the side of the third bonding material layer 11 and the sixth bonding material layer 16 away from the second support plate 12 from the resin layer;

[0151] Specifically, the side of the fourth bonding material layer 13 facing away from the third support plate 14 is debonded from the resin layer of the semi-molded substrate, the side of the fifth bonding material layer 15 facing away from the third support plate 14 is debonded from the resin layer of the semi-molded substrate, the side of the third bonding material layer 11 facing away from the second support plate 12 is debonded from the resin layer of the semi-molded substrate, and the side of the sixth bonding material layer 16 facing away from the second support plate 12 is debonded from the resin layer of the semi-molded substrate. In this way, four semi-molded substrates are obtained, and a schematic diagram of one of the semi-molded substrates is shown as follows: Fig.19 shown.

[0152] S19: curing, curing the resin in the structure formed in the previous step to more than 90%;

[0153] High temperature curing can be used in this step. After this step is completed, the resin in the structure formed can be cured to more than 90%, that is, the degree of curing is more than 90%.

[0154] Specifically, the structure formed in the previous step can be placed in a constant temperature environment of 190°C-210°C to cure the resin in the structure to more than 90%. For example, the structure formed by circuit manufacturing can be placed in a constant temperature environment of 190°C, 195°C, 200°C, 205°C or 210°C to cure the resin in the structure to more than 90% or all of it. Preferably, the structure formed by circuit manufacturing is placed in a constant temperature environment of 190°C-210°C, and at the same time, the environmental vacuum degree can be maintained at 8Pa-15Pa for 50min-70min. For example, the structure formed by circuit manufacturing is placed in a constant temperature environment of 200°C, and at the same time, the environmental vacuum degree is maintained at 10Pa, and the pressure is maintained at 0.5Mpa for 60min.

[0155] In this step, a laminator can be used, using two mirror steel plates to clamp the structure formed in the previous step until this step is completed. It should be noted here that in this application, all pre-curing steps can be carried out in an oven, and only the curing step is carried out in a laminator. In addition, the first pre-curing and the pre-curing in the insulating resin layer processing step in this application are both low-temperature curing, and the curing temperature is below 180°C to prevent the pre-curing process from affecting the bonding of the bonding material layer.

[0156] S20: manufacturing the outer layer circuit 17, performing blind hole 9 processing and circuit manufacturing steps on the cured structure to form the outer layer circuit 17;

[0157] On the cured structure, blind holes 9 are processed and circuits are made to form an outer layer circuit 17. That is, blind holes 9 are opened again on the surface of the structure, and circuits are made to form an outer layer circuit 17. The outer layer circuit 17 is electrically connected to the internal circuit through the blind holes 9. After this step, the structure formed after the circuit is made is as follows: Fig. 20 shown.

[0158] S21: Making a solder resist layer, making a solder resist layer 18 on the surface of the outer layer circuit 17; the structure formed after the step of making the solder resist layer 18 is as follows Fig.21 shown.

[0159] S22: coating, coating the surface of the structure formed after the solder resist layer 18 is formed. The specific material of the coating may be NiPdAu (nickel palladium gold), NiAu (nickel gold), Sn (tin) or OSP (Organic Solderability Preservatives).

[0160] In the manufacturing method of the embedded chip substrate provided by the present application, a support plate is used to support the semi-formed substrate during the manufacturing process of all intermediate circuits 10. Specifically, through 4 temporary bonding and 3 debonding, multiple substrates are supported by the support plate during the intermediate circuit 10 processing, chip mounting 4 and pre-curing steps, so that the substrates always maintain a low warpage state. In addition, the manufacturing process of the intermediate circuits 10 of multiple substrates is symmetrical processing, that is, symmetrical intermediate circuits 10 are manufactured on the substrates on both sides of the support plate, so that the stresses generated are the same and balanced with each other, ensuring that the substrates always maintain a low warpage state during the processing process and preventing excessive bending of the substrates.

[0161] In addition, in the method for making an embedded chip substrate provided by the present application, each insulating resin layer is pre-cured after processing, and is not completely cured until all the resins are pressed and buried and finally cured, so that the resin in the structure is cured to more than 90%. The resin in the embedded chip substrate is in a semi-cured state before curing. At this time, the modulus of the resin material in the embedded chip substrate is low, and the substrate is in a low stress and low warping state. In this way, each step before curing is completed in a low warping state, avoiding warping and excessive bending of the substrate during the processing of the embedded chip substrate, thereby avoiding cracking and delamination of the formed structure. The method for making an embedded chip substrate of the present application is suitable for processing ultra-thin multilayer boards, coreless packaging (Coreless) substrates, etc.

[0162] In a preferred embodiment, the first pre-curing is specifically: curing the resin in the structure formed in this step to 50%-70%; that is, the curing degree of the resin after the first pre-curing is 50%-70%, and the curing degree of the resin after the first pre-curing can be 50%, 60%, 70%, 75%, etc., so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. Preferably, the resin in the formed structure is cured to 70%.

[0163] Alternatively, the first pre-curing is specifically: placing the formed structure in a constant temperature environment of 130° C.-150° C. for 20 min-40 min to pre-cure the resin in the structure. Specifically, the formed structure can be placed in a constant temperature environment of 130° C., 135° C., 140° C. or 150° C., and the holding time can be 25 min, 30 min or 35 min. Preferably, the formed structure is placed in a constant temperature environment of 140° C. for 30 min.

[0164] The pre-curing in the insulating resin layer processing step S11 is specifically: the resin in the structure formed in this step is cured to 50%-70%; that is, the curing degree of the resin after curing in step S11 is 50%-70%, and the curing degree of the insulating resin layer formed in this step can be 50%, 60%, 70%, etc., so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. Preferably, the resin in the formed structure is cured to 70%.

[0165] Alternatively, the pre-curing in the insulating resin layer processing step of step S11 is specifically: placing the formed structure in a constant temperature environment of 130°C-150°C for 20min-40min to pre-curing the resin in the structure. Specifically, the formed structure can be placed in a constant temperature environment of 130°C, 135°C, 140°C or 150°C, and the holding time can be 25min, 30min or 35min. Preferably, the formed structure is placed in a constant temperature environment of 140°C for 30min.

[0166] Of course, specific parameters of the first pre-curing and the pre-curing in the insulating resin layer processing step S11 may be adjusted according to actual conditions, and are not specifically limited here.

[0167] In another embodiment, when the raw materials used in the first pressing and embedding resin step and the second pressing and embedding resin step are both ABF resin sheets, step S9 includes step S9' after processing the blind hole 9: film removal, removing the PET film d of the first resin layer 5 and the second resin layer 8, so as to facilitate the subsequent circuit processing. In addition, when the raw materials used in the first pressing and embedding resin step and the second pressing and embedding resin step are both copper-clad resin sheets RCC, the copper foil layer of the copper-clad resin sheets RCC is removed in this step.

[0168] As an optional implementation, after step S14, step S14' of cleaning is also included: cleaning the first surface of the first substrate 1 and the first surface of the second substrate 6. In this way, resin residue can be prevented from remaining on the first surface of the first substrate 1 and the first surface of the second substrate 6. Specifically, a plasma cleaning machine can be used for cleaning, for example, in a degumming tank at 70°C-85°C for 2min-5min. Then bake at 100°C-130°C for 30 minutes to remove moisture. Of course, other cleaning methods can also be used, such as ultrasonic alkaline solution cleaning, which is not limited here.

[0169] In addition, the debonding temperature of the first debonding and the debonding temperature of the second debonding are both lower than the debonding temperature of the third debonding. In other words, the debonding temperatures of the first bonding material layer 2 and the second bonding material layer 7 are lower than the debonding temperatures of the third bonding material layer 11, the fourth bonding material layer 13, the fifth bonding material layer 15 and the sixth bonding material layer 16. Specifically, the debonding temperatures of the first bonding material layer 2 and the second bonding material layer 7 are lower than the debonding temperatures of the third bonding material layer 11, the fourth bonding material layer 13, the fifth bonding material layer 15 and the sixth bonding material layer 16 by more than 15°C, for example, 15°C, 20°C, 25°C, etc. Preferably, the debonding temperatures of the first bonding material layer 2 and the second bonding material layer 7 are lower than the debonding temperatures of the third bonding material layer 11, the fourth bonding material layer 13, the fifth bonding material layer 15 and the sixth bonding material layer 16 by 30°C. The debonding temperatures of the third bonding material layer 11 , the fourth bonding material layer 13 , the fifth bonding material layer 15 and the sixth bonding material layer 16 may be the same, and the debonding temperatures of the first bonding material layer 2 and the second bonding material layer 7 may be the same.

[0170] Moreover, the temperature of the first pre-curing and the pre-curing temperature in the insulating resin layer processing step should be lower than the debonding temperature of the first debonding, the debonding temperature of the second debonding and the debonding temperature of the third debonding. In other words, the temperature of the first pre-curing and the pre-curing temperature in the insulating resin layer processing step are lower than the debonding temperatures of the first bonding material layer 2, the second bonding material layer 7, the third bonding material layer 11, the fourth bonding material layer 13, the fifth bonding material layer 15 and the sixth bonding material layer 16. Preferably, the temperature of the first pre-curing and the pre-curing temperature in the insulating resin layer processing step are lower than the debonding temperature of the first debonding by more than 30°C, for example, the temperature of the first pre-curing and the pre-curing temperature in the insulating resin layer processing step are 20°C, 25°C or 30°C lower than the debonding temperature of the first debonding.

[0171] The embodiment of the present invention also provides a multi-layer temporary bonding structure, such as Fig.16As shown, the multi-layer temporary bonding structure is the fourth temporary bonding structure formed in the fourth temporary bonding of step S15. The multi-layer temporary bonding structure includes a first support plate 3, a second support plate 12, a third support plate 14, a first bonding material layer 2, a second bonding material layer 7, a third bonding material layer 11, a fourth bonding material layer 13, a fifth bonding material layer 15, a sixth bonding material layer 16, a first semi-molded substrate A, a second semi-molded substrate B, a third semi-molded substrate C and a fourth semi-molded substrate D.

[0172] The first bonding material layer 2 and the second bonding material layer 7 are bonded to both sides of the first support plate 3 , that is, one side of the first support plate 3 is bonded to the first bonding material layer 2 , and the other side of the second support plate 12 is bonded to the second bonding material layer 7 .

[0173] The third bonding material layer 11 and the sixth bonding material layer 16 are bonded to both sides of the second support plate 12, that is, one side of the second support plate 12 is bonded to the third bonding material layer 11, and the other side of the second support plate 12 is bonded to the sixth bonding material layer 16. One side of the third semi-molded substrate C is bonded to the side of the sixth bonding material layer 16 away from the second support plate 12, and the other side of the third semi-molded substrate C is bonded to the side of the second bonding material layer 7 away from the first support plate 3. That is, the third semi-molded substrate C is located between the second bonding material layer 7 and the sixth bonding material layer 16. One side of the fourth semi-molded substrate D is bonded to the side of the third bonding material layer 11 away from the second support plate 12.

[0174] The fourth bonding material layer 13 and the fifth bonding material layer 15 are bonded to both sides of the third support plate 14, that is, one side of the third support plate 14 is bonded to the fourth bonding material layer 13, and the other side of the third support plate 14 is bonded to the fifth bonding material layer 15. One side of the second semi-molded substrate B is bonded to the side of the fifth bonding material layer 15 away from the third support plate 14, and the other side of the second semi-molded substrate B is bonded to the side of the first bonding material layer 2 away from the first support plate 3. That is, the second semi-molded substrate B is located between the fifth bonding material layer 15 and the first bonding material layer 2. One side of the first semi-molded substrate A is bonded to the side of the fourth bonding material layer 13 away from the third support plate 14.

[0175] In the above-mentioned multi-layer temporary bonding structure, a symmetrical intermediate circuit 10 is manufactured on the substrates on both sides of each support plate, so that the stresses generated are of the same magnitude and balanced with each other, ensuring that the substrate always maintains a low warping state during the processing process, preventing excessive bending of the substrate, and avoiding the formation of cracks in the insulating resin and cracks in the interface between the chip 4 and the resin.

[0176] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.

[0177] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for manufacturing an embedded chip substrate, characterized in that: include: Opening windows on substrates, opening cavities for accommodating chips on multiple substrates; A first temporary bonding is performed to bond the first surface of the first substrate having the accommodating cavity to the first bonding material layer, and a first supporting plate is fixed to a side of the first bonding material layer facing away from the first substrate; A first chip mounting method is to place the chip in the accommodation cavity of the first substrate; A first pressing and filling resin, pressing and filling the resin on the second surface of the first substrate to form a first resin layer; Second temporary bonding, providing a second bonding material layer on a side of the first support plate away from the first bonding material layer, and bonding the second bonding material layer to the first surface of the second substrate having the accommodating cavity; A second chip mounting method is to place the chip in the receiving cavity of the second substrate; A second pressing and filling resin, pressing and filling the resin on the second surface of the second substrate to form a second resin layer; The first pre-curing cures the resin in the formed structure to more than 50%; Blind hole processing, opening blind holes on the upper and lower surfaces of the structure formed in the previous step; Circuit fabrication, processing circuits on the upper and lower surfaces of the structure formed in the previous step; Insulating resin layer processing, providing insulating resin layers on both the upper and lower surfaces of the structure formed in the previous step, and pre-curing to cure the insulating resin layer formed in this step to more than 50%; First, an intermediate circuit is manufactured, and the steps of blind hole manufacturing, circuit manufacturing, and insulating resin layer manufacturing are repeated N times, where N≥0, to form a first temporary bonding structure; Third temporary bonding, bonding a third bonding material layer on the side of the first temporary bonding structure having the first substrate, and a second supporting plate is provided on the side of the third bonding material layer facing away from the first temporary bonding structure; bonding a fourth bonding material layer on the side of the first temporary bonding structure having the second substrate, and a third supporting plate is provided on the side of the fourth bonding material layer facing away from the first temporary bonding structure; A first debonding step is to debond the first surface of the first substrate from the first bonding material layer to obtain a second temporary bonding structure; and a first surface of the second substrate from the second bonding material layer to obtain a third temporary bonding structure; Fourth temporary bonding, the first temporary bonding structure has a side of the first substrate bonded with a fifth bonding material layer, and the side of the third support plate of the third temporary bonding structure facing away from the fourth bonding material layer is bonded to the fifth bonding material layer; The first temporary bonding structure has a side of the second substrate bonded with a sixth bonding material layer, and the side of the second support plate of the second temporary bonding structure facing away from the third bonding material layer is bonded to the sixth bonding material layer to obtain a fourth temporary bonding structure; A second debonding step is to debond the first bonding material layer in the fourth temporary bonding structure from the first substrate, and to debond the second bonding material layer from the second substrate; Second, the intermediate circuit is made. The upper surface and the lower surface of the structure formed in the previous step are both pressed and filled with resin to form a resin layer and pre-cured. The blind hole processing, circuit production and insulating resin layer processing are repeated M times, M≥0; The third debonding is to debond the side of the fourth bonding material layer and the fifth bonding material layer away from the third support plate from the resin layer; and the side of the third bonding material layer and the sixth bonding material layer away from the second support plate from the resin layer; Curing, curing the resin in the structure formed in the previous step to more than 90%; Fabricating an outer layer circuit, performing blind hole processing and circuit fabrication steps on the cured structure to form an outer layer circuit; Making a solder resist layer, making a solder resist layer on the surface of the outer layer circuit; A coating is applied on the surface of the structure formed after the solder resist layer is made.

2. The method for manufacturing an embedded chip substrate according to claim 1, characterized in that: The first pre-curing is specifically: curing the resin in the structure formed in this step to 50%-70%; or, the first pre-curing is specifically: placing the formed structure in a constant temperature environment of 130°C-150°C for 20min-40min to pre-cure the resin in the structure.

3. The method for manufacturing an embedded chip substrate according to claim 1, characterized in that: The pre-curing in the insulating resin layer processing step is specifically: curing the insulating resin layer in the structure to a degree of 50%-70%; or, the pre-curing in the insulating resin layer processing step is specifically: placing the formed structure in a constant temperature environment of 130°C-150°C for 20min-40min to pre-cure the resin in the structure.

4. The method for manufacturing an embedded chip substrate according to claim 1, characterized in that: The curing is specifically as follows: placing the formed structure in an environment with a constant temperature of 190° C.-210° C. and a vacuum degree of 8 Pa-15 Pa for 50 min-70 min to cure the resin in the structure.

5. The method for manufacturing an embedded chip substrate according to claim 1, characterized in that: The raw materials used in the first pressing and filling resin step, the second pressing and filling resin step and the insulating resin layer processing step are all ABF resin sheets, and the ABF resin sheet includes an ABF main layer, an OPP film attached to the first side of the ABF main layer, and a PET film d attached to the second side of the ABF main layer.

6. The method for manufacturing an embedded chip substrate according to claim 5, characterized in that: In the first resin-filling pressing step, the second resin-filling pressing step, and the insulating resin layer processing step, the OPP film of the ABF resin sheet is removed, and the PET film d of the ABF resin sheet is retained.

7. The method for manufacturing an embedded chip substrate according to claim 5, characterized in that: The blind hole processing also includes the step of film removal, in which the PET films d of the first resin layer and the second resin layer are removed.

8. A multi-layer temporary bonding structure, characterized in that: It includes a first support plate, a second support plate, a third support plate, a first bonding material layer, a second bonding material layer, a third bonding material layer, a fourth bonding material layer, a fifth bonding material layer, a sixth bonding material layer, a first semi-molded substrate, a second semi-molded substrate, a third semi-molded substrate and a fourth semi-molded substrate; A first bonding material layer and a second bonding material layer are bonded to two sides of the first support plate respectively; A third bonding material layer and a sixth bonding material layer are bonded to both sides of the second support plate, a side of the third bonding material layer facing away from the second support plate is bonded to a fourth semi-molded substrate, a side of the sixth bonding material layer facing away from the second support plate is bonded to one side of the third semi-molded substrate, and the other side of the third semi-molded substrate is bonded to a side of the second bonding material layer facing away from the first support plate; A fourth bonding material layer and a fifth bonding material layer are bonded to both sides of the third support plate, respectively; a side of the fourth bonding material layer facing away from the second support plate is bonded to the first semi-molded substrate; a side of the fifth bonding material layer facing away from the third support plate is bonded to one side of the second semi-molded substrate; and the other side of the second semi-molded substrate is bonded to a side of the first bonding material layer facing away from the first support plate.

9. The method for manufacturing an embedded chip substrate according to any one of claims 1 to 7 or the multi-layer temporary bonding structure according to claim 8, characterized in that: At least one of the first bonding material layer, the second bonding material layer, the third bonding material layer, the fourth bonding material layer, the fifth bonding material layer and the sixth bonding material layer has a structure comprising a foaming film, a support film and a pressure-sensitive adhesive film stacked in sequence.

10. The method for manufacturing an embedded chip substrate according to any one of claims 1 to 7 or the multi-layer temporary bonding structure according to claim 8, characterized in that: The debonding temperatures of the first bonding material layer and the second bonding material layer are lower than the debonding temperatures of the third bonding material layer, the fourth bonding material layer, the fifth bonding material layer and the sixth bonding material layer by more than 15°C.

Citation Information

Cited By

  • Packaging control method and system of semiconductor device

    CN120854281A

  • A method and system for controlling the packaging of a semiconductor device

    CN120854281B