Manufacturing method of board-level fan-out type packaging structure

By adopting a symmetrical sandwich structure and the through-hole processing technology of the substrate itself in the plate-level fan-out packaging structure, the problem of warping and conductive through-hole processing after multi-layer wiring is solved, which improves processing efficiency and reduces costs.

CN118943078AActive Publication Date: 2024-11-12INST OF MICROELECTRONICS CHINESE ACAD OF SCI LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310532886.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12
Estimated Expiration
2043-05-11

AI Technical Summary

Technical Problem

The existing board-level fan-out packaging structure is prone to warping after multi-layer wiring, resulting in difficulty in processing, and the conductive via processing technology is complex and difficult.

Method used

The circuit is arranged on both sides of the substrate and interconnected. Through the combined structure of temporary bonding material layer and support plate, the landfill resin is laminated and pre-cured to form a symmetrical sandwich structure, reducing the modulus of the resin and avoiding warping. , and use the through-hole processing technology of the substrate itself to reduce the demand for copper column manufacturing.

Benefits of technology

It effectively reduces the warping and processing difficulty of the substrate, improves production efficiency, reduces costs, avoids structural cracking and layering problems, and simplifies the process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943078A_ABST
    Figure CN118943078A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a board-level fan-out type packaging structure. Comprising the steps of substrate windowing, first temporary bonding, first chip pasting, first pressing and resin filling, second temporary bonding, second chip pasting, second pressing and resin filling, first pre-curing, blind hole processing, circuit manufacturing, resin insulation layer processing, intermediate circuit manufacturing, de-bonding, third pressing and resin filling, curing and the like. The method includes the steps of substrate windowing, first temporary bonding, first chip pasting, first pressing and resin filling, second temporary bonding, second chip pasting, second pressing and resin filling, first pre-curing, blind hole processing, circuit manufacturing, resin insulation layer processing, intermediate circuit manufacturing, de-bonding, third pressing and resin filling, curing and the like. The processes from chip pasting, first resin layer and second resin layer forming to intermediate circuit manufacturing of the first substrate and the second substrate are completed under the supporting of the supporting plate, and the supporting effect of the supporting plate can prevent the substrates from being excessively warped and repeatedly bent in the machining process. The resin in the board-level fan-out type packaging structure is in a semi-curing state before curing, so that the processing process is completed in a low-warping state, warping and excessive bending of the substrate in the processing of the board-level fan-out type packaging structure are avoided, and the formed structure cracking and layering are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for manufacturing a board-level fan-out packaging structure. Background Art

[0002] In the prior art, during the manufacturing process of the board-level fan-out packaging structure, the chip is temporarily bonded on a large-format carrier board. After molding, the chip embedded in the molding resin and the plastic sealing board formed by molding are debonded, and then multi-layer wiring is performed on the surface of the plastic sealing board with the chip in front, and the layer units are cut to form a board-level fan-out packaging structure.

[0003] The board-level fan-out package forms POP (Package-on-Package) interconnection, which requires manufacturing conductive through holes that penetrate the plastic package board in the fan-out package structure, and manufacturing pads on the back of the plastic package board to form front and back interconnections based on the board-level fan-out package.

[0004] In addition, after wiring on the resin surface of the board-type fan-out package, the resin board with the chip embedded will warp significantly. The more wiring layers there are, the greater the warping. Usually, after more than three layers of wiring, wiring becomes difficult, making it difficult to process the circuit. In addition, the conductive through-hole processing of the resin board requires ultra-thick copper column electroplating, which makes the manufacturing process very difficult. Summary of the invention

[0005] The object of the present invention is to provide a method for manufacturing a board-level fan-out packaging structure to reduce substrate warping during processing, improve processing efficiency, and reduce manufacturing costs.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A method for manufacturing a board-level fan-out packaging structure, comprising:

[0008] Opening windows on substrates: opening cavities for accommodating chips on multiple substrates, with circuits arranged on both the front and back sides of the substrates and interconnected with each other;

[0009] A first temporary bonding is performed to bond the first surface of the first substrate having the accommodating cavity to the first bonding material layer, and a support plate is fixed to a side of the first bonding material layer facing away from the first substrate;

[0010] A first chip mounting method is to place the chip in the accommodation cavity of the first substrate;

[0011] A first pressing and filling resin, pressing and filling the resin on the second surface of the first substrate to form a first resin layer;

[0012] Second temporary bonding, disposing a second bonding material layer on a side of the support plate away from the first bonding material layer, and bonding the second bonding material layer to the first surface of the second substrate having the accommodating cavity;

[0013] A second chip mounting method is to place the chip in the receiving cavity of the second substrate;

[0014] A second pressing and filling resin, pressing and filling the resin on the second surface of the second substrate to form a second resin layer;

[0015] The first pre-curing cures the resin in the structure formed in the previous step to more than 50%;

[0016] Blind hole processing, opening blind holes on the upper and lower surfaces of the structure formed in the previous step;

[0017] Circuit fabrication, processing circuits on the upper and lower surfaces of the structure formed in the previous step;

[0018] Resin insulation layer processing, providing resin insulation layers on both the upper and lower surfaces of the structure formed in the previous step, and pre-curing to cure the resin insulation layer formed in this step to more than 50%;

[0019] To make an intermediate circuit, repeat the steps of blind hole processing, circuit production and resin insulation layer processing N times, N ≥ 0, to form an N-layer intermediate circuit, and no pre-curing is performed in the N-th resin insulation layer processing step, and pre-curing is performed after copper foil is pressed on the surface of the resin insulation layer formed in the N-th resin insulation layer processing step, so that the resin insulation layer in the formed structure is cured to more than 50%;

[0020] Laminating copper foil, laminating copper foil on the surface of the resin insulation layer of the Nth layer of the intermediate circuit from the inside to the outside of the structure formed in the previous step, and pre-curing to cure the resin insulation layer in the structure to more than 50%;

[0021] Debonding, debonding the first bonding material layer from the first surface of the first substrate, and debonding the second bonding material layer from the first surface of the second substrate;

[0022] Thirdly, the resin is pressed and embedded, the resin is pressed and embedded on the first surface of the first substrate and the copper foil is pressed on the surface of the formed resin layer to obtain a first temporary structure, and the resin is pressed and embedded on the first surface of the second substrate and the copper foil is pressed on the surface of the formed resin layer to obtain a second temporary structure;

[0023] The second pre-curing cures the resin in the first temporary structure and the second temporary structure to more than 50%;

[0024] Curing: the structure formed in the previous step is placed in a laminator, clamped by a mirror steel plate, under a preset vacuum degree and a preset pressure, so that the resin in the structure is cured to more than 90%;

[0025] Fabricating an outer layer circuit, performing blind hole processing and circuit fabrication steps on the cured structure to form an outer layer circuit;

[0026] Making a solder resist layer, making a solder resist layer on the surface of the outer layer circuit;

[0027] A coating is applied on the surface of the structure formed after the solder resist layer is made.

[0028] In one implementation, the first bonding material layer includes a foaming film, a support film and a pressure-sensitive adhesive film stacked in sequence, and the foaming film of the first bonding material layer is bonded to the first surface of the first substrate, and the pressure-sensitive adhesive film of the first bonding material layer is bonded to the support plate; and / or,

[0029] The second bonding material layer includes a foaming film, a supporting film and a pressure-sensitive adhesive film stacked in sequence, and the foaming film of the second bonding material layer is bonded to the first surface of the second substrate, and the pressure-sensitive adhesive film of the second bonding material layer is bonded to the side of the supporting plate facing away from the first bonding material layer.

[0030] In one implementation, the first pre-curing is specifically: curing the resin in the structure formed in this step to 50%-70%; or, the first pre-curing is specifically: placing the formed structure in a constant temperature environment of 130°C-155°C for 30min-60min to pre-cure the resin in the structure.

[0031] In one implementation, the pre-curing in the resin insulation layer processing step is specifically: curing the resin insulation layer in the structure to a degree of 50%-70%; or, the pre-curing in the resin insulation layer processing step is specifically: placing the formed structure in a constant temperature environment of 130°C-155°C for 30min-60min to pre-cure the resin in the structure.

[0032] In one implementation, the curing is specifically as follows: placing the formed structure in a laminator, clamping it between two mirror steel plates with a pressure of 0.1MPa-0.5MPa, in an environment of a constant temperature of 190°C-210°C and a vacuum degree of 1Pa-15Pa, and maintaining it for 50min-70min to cure the resin in the structure.

[0033] In one implementation, the raw materials used in the first pressing and filling resin step, the second pressing and filling resin step, the resin insulation layer processing step and the third pressing and filling resin step are all ABF resin sheets, and the ABF resin sheet includes an ABF main layer, an OPP film attached to the first side of the ABF main layer, and a PET film attached to the second side of the ABF main layer.

[0034] In one implementation, the first pressing and filling resin step is specifically: removing the OPP film of the ABF resin sheet, and pressing the first side of the ABF resin sheet onto the second surface of the first substrate to form a first resin layer, wherein the first resin layer retains a PET film on a side away from the first substrate;

[0035] The second resin embedding step is specifically to remove the OPP film of the ABF resin sheet and to laminate the first side of the ABF resin sheet onto the second surface of the second substrate to form a second resin layer, wherein the PET film is retained on the side of the second resin layer away from the second substrate.

[0036] In one implementation, the manufacturing of the outer layer circuit further includes the step of corroding the copper foil to remove the copper foil on the surface of the structure formed in the previous step.

[0037] In one implementation, after the debonding step, the method further includes: cleaning, cleaning the first surface of the first substrate and the first surface of the second substrate.

[0038] In one implementation, the curing temperature of the first pre-curing and the curing temperature of the pre-curing in the resin insulation layer processing step are lower than the debonding temperature of the first bonding material layer and the second bonding material layer.

[0039] In the present application, since the circuits are arranged on the front and back sides of the substrate itself and the circuits on the front and back sides of the substrate are interconnected, it has advantages for the subsequent board-level fan-out package to form POP (Package-on-Package) interconnection, avoiding the subsequent manufacturing step of the conductive through-hole, utilizing the through-hole processing and mature manufacturing process of the substrate itself, avoiding the use of high aspect ratio plate copper column manufacturing technology, and reducing the difficulty of processing. In addition, during the manufacturing process of the intermediate circuit, the two sides of the support plate are always symmetrically processed with the same wiring layer and insulation layer, so the entire sandwich temporary bonding structure has a symmetrical stress distribution, and is at an extremely low warping level in the multi-layer wiring processing, and will not cause the problem of being unable to be processed due to basic warping. And the first pre-curing is performed only after the first pressing and embedding resin and the second pressing and embedding resin are completed, and each time a layer of the intermediate circuit is processed and a resin insulation layer is set on the circuit surface, a pre-curing is performed, and it is not completely cured until all the resins are pressed and embedded and finally cured once, so that the resin in the structure is cured to more than 90%. The resin in the board-level fan-out packaging structure is in a semi-cured state before curing. At this time, the modulus of the resin material in the board-level fan-out packaging structure is low, and the substrate is in a low stress and low warpage state. In this way, the process of chip bonding, forming the first resin layer and the second resin layer, making the intermediate circuit to the third pressing and filling resin are all completed in a low warpage state, avoiding warping and excessive bending of the substrate during the processing of the board-level fan-out packaging structure, and thus avoiding cracking and delamination of the formed structure.

[0040] In addition, in the manufacturing method of the board-level fan-out packaging structure of the present application, a first bonding material layer and a first substrate are arranged on one side of the support plate, and a second bonding material layer and a second substrate are arranged on the other side of the support plate, that is, the processing structures on both sides of the support plate are arranged symmetrically, which fully utilizes the supporting function of the support plate, and simultaneously processes two board-level fan-out packaging structures, thereby improving manufacturing efficiency and reducing processing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0042] Figure 1 A schematic diagram of a process for manufacturing a board-level fan-out packaging structure provided by an embodiment of the present invention;

[0043] Figure 2 The structure of the first substrate formed after the substrate window opening step provided in the embodiment of the present invention;

[0044] Figure 3 A structure formed after the first temporary bonding step provided by an embodiment of the present invention;

[0045] Figure 4 The structure formed after the first chip mounting step provided in the embodiment of the present invention;

[0046] Figure 5 The structure formed after the first pressing and embedding resin step provided in the embodiment of the present invention;

[0047] Figure 6 A structure formed after the second temporary bonding step provided by an embodiment of the present invention;

[0048] Figure 7 The structure formed after the second chip mounting step provided in the embodiment of the present invention;

[0049] Figure 8 The structure formed after the second pressing and embedding resin step provided in the embodiment of the present invention;

[0050] Fig. 9 The structure formed after the blind hole processing step provided in the embodiment of the present invention;

[0051] Fig.10 The structure formed after the film stripping step provided in the embodiment of the present invention;

[0052] Fig.11 A structure formed after the circuit manufacturing steps provided in the embodiment of the present invention;

[0053] Fig.12 The structure formed after the step of manufacturing the intermediate circuit provided in the embodiment of the present invention;

[0054] Fig.13 A schematic diagram of a first substrate after a debonding step provided by an embodiment of the present invention;

[0055] Fig.14 A schematic diagram of a first temporary structure obtained after the third pressing and embedding resin step provided in an embodiment of the present invention;

[0056] Fig.15 A schematic diagram of a first temporary structure after a blind hole is processed according to an embodiment of the present invention;

[0057] Fig.16 A schematic diagram of the steps of manufacturing an outer layer circuit provided by an embodiment of the present invention;

[0058] Fig.17 A schematic diagram of the steps of making a solder resist layer provided in an embodiment of the present invention;

[0059] Fig.18 A schematic structural diagram of a first bonding material layer or a second bonding material layer provided in an embodiment of the present invention.

[0060] Reference numerals:

[0061] 1-first substrate, 1a-accommodating cavity, 1b-substrate circuit, 2-first bonding material layer, 3-support plate, 4-chip, 5-first resin layer, 6-second substrate, 7-second bonding material layer, 8-second resin layer, 9-blind hole, 10-inner circuit, 11-middle circuit, 12-third resin layer, 13-outer circuit, 14-solder resist layer;

[0062] a-foaming film, b-support film, c-pressure-sensitive adhesive film, d-PET film. DETAILED DESCRIPTION

[0063] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0064] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.

[0065] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.

[0066] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "front", "back", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.

[0067] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0068] See also Figure 1 , Figure 1 This is a flow chart of an embodiment provided by the present invention. The manufacturing method of the board-level fan-out packaging structure in this embodiment includes the steps of:

[0069] S1: Opening windows on substrates: opening cavities 1a for accommodating chips 4 on multiple substrates; circuits are arranged on both the front and back sides of the substrates and the circuits on the front and back sides are interconnected;

[0070] In step S1, the accommodating cavity 1a may be specifically provided on two substrates, namely the first substrate 1 and the second substrate 6. That is, the accommodating cavity 1a is provided on both the first substrate 1 and the second substrate 6, so as to facilitate the chip 4 to be arranged in the accommodating cavity in the subsequent steps.

[0071] In addition, in this step, Figure 2 The middle substrate has a substrate circuit 1b. Circuits are arranged on both the front and back sides of the substrate, and the circuits on the front side of the substrate are electrically connected to the circuits on the back side, so as to realize electrical connection between the multi-layer wiring on the front side and the multi-layer wiring on the back side after multiple wirings are performed on the front and back sides of the substrate. A window is opened in a substrate with interconnected front and back wirings. The substrate with interconnected front and back wirings adopts a conventional substrate manufacturing process, and multi-layer wirings are performed on the upper and lower surfaces of the substrate. The front and back wiring layers are interconnected through the through holes of the middle core board to form the interconnections of the front and back wiring layers. This double-sided wiring interconnection substrate can be a substrate with a core board or a coreless substrate without a core board.

[0072] Specifically, the two surfaces of the substrate along the thickness direction of the substrate are the first surface and the second surface respectively, or when the substrate is placed horizontally, that is, when the thickness direction of the substrate is along the vertical direction, the lower surface and the upper surface of the substrate are the first surface and the second surface respectively. Figure 2 shown.

[0073] The substrate can be a BT (Bismaleimide Triazine) resin substrate or a FR4 material substrate. BT resin material has a very high glass transition temperature, excellent dielectric properties, low thermal expansion coefficient, good mechanical characteristics and other properties, which are more suitable for the production of substrates. FR4 is a code for a flame retardant material grade, which means that the resin material must be able to extinguish itself after burning. Of course, the substrate can also be made of other materials, which are not limited here.

[0074] S2: first temporary bonding, bonding the first surface of the first substrate 1 with the accommodating cavity 1 a to the first bonding material layer 2, and a support plate 3 is fixed to a side of the first bonding material layer 2 facing away from the first substrate 1;

[0075] That is, the first bonding material layer 2 is bonded to the first surface of the first substrate 1 with the accommodating cavity 1a, and in this embodiment, the first surface of the first substrate 1 may be the lower surface of the first substrate 1. A support plate 3 is fixed to the side of the first bonding material layer 2 facing away from the first substrate 1.

[0076] like Fig.18 As shown, the first bonding material layer 2 may include a foaming film a, a supporting film b and a pressure-sensitive adhesive film c stacked in sequence, and the foaming film a of the first bonding material layer 2 is bonded to the first surface of the first substrate 1. When the foaming film a is at the debonding temperature, it only takes a few minutes for the foaming film a to be debonded and the supporting plate 3 to fall off by itself, completing the debonding, which is easy to operate and does not require special equipment assistance.

[0077] A support plate 3 is fixed to the side of the first bonding material layer 2 facing away from the first substrate 1, and the pressure-sensitive adhesive film c of the first bonding material layer 2 is bonded to the support plate 3, that is, the first bonding material layer 2 is located between the support plate 3 and the first substrate 1. The structure formed after the first temporary bonding step is as shown in FIG. Figure 3 As shown. In this embodiment, the first bonding material layer 2 can be 31950E temporary bonding adhesive produced by Nitto Company with 210°C heat foaming and debonding. Of course, other temporary bonding adhesives can also be selected according to actual conditions, which is not limited here. Of course, the first bonding material layer 2 can also be a single-layer film structure or other types of multi-layer film structures, which is not limited here.

[0078] It should be noted here that the first bonding material layer 2 can be first bonded to the support plate 3 and then bonded to the first substrate 1. In this way, the first bonding material layer 2 is first bonded to the support plate 3 for standby use. Of course, the first bonding material layer 2 can also be first bonded to the first substrate 1 and then bonded to the support plate 3, which is not limited here.

[0079] The support plate 3 may be a plate with high rigidity such as a double-sided copper-clad plate, a metal plate, a glass plate or a ceramic plate, or the material of the support plate 3 may be BT resin, and the support plate 3 may be a double-sided copper-clad plate made of BT resin. The thickness of the support plate 3 may be greater than or equal to 0.5 mm, specifically, the thickness of the support plate 3 may be 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, etc., so that the strength of the support plate 3 can be ensured, and the first substrate 1 and the second substrate 6 can be prevented from warping during processing.

[0080] S3: first attaching the chip 4, placing the chip 4 in the accommodating cavity 1a of the first substrate 1;

[0081] A chip 4 is arranged in the accommodating cavity 1a of the first substrate 1. In this step, the electrode side of the chip 4 can be oriented toward the side away from the first bonding material layer 2, that is, the electrode of the chip 4 is placed upward, and the electrode side of the chip 4 can also be placed downward. When the accommodating cavity 1a is a through hole, the chip 4 can be in contact with the first bonding material layer 2, and when the electrode side of the chip 4 is downward, its electrode is in contact with the first bonding material layer 2.

[0082] When the first bonding material layer 2 includes a foaming film a, a support film b and a pressure-sensitive adhesive film c stacked in sequence, the chip 4 can be in contact with the foaming film a of the first bonding material layer 2. Specifically, when the electrode side of the chip 4 is downward, its electrode is in contact with the foaming film a of the first bonding material layer 2. The structure formed after the chip 4 bonding step is as follows: Figure 4 shown.

[0083] Preferably, when the chip 4 is attached to the accommodating cavity 1a of the first substrate 1, the electrode side of the chip 4 can be oriented toward the side away from the first bonding material layer 2, that is, the electrode of the chip 4 faces upward, so that the foaming film a of the first bonding material layer 2 does not contact the chip 4 electrode, but contacts the back of the chip 4, which can prevent the chip 4 electrode surface from being contaminated, causing contamination to cause contaminants to be buried in the substrate and form serious reliability problems. Alternatively, the surface of the chip 4 has a protective film to prevent the chip 4 electrode surface from being contaminated. After the bonding is released, the protective film on the surface of the chip 4 can be removed. The protective film can be a copper foil or a film of other materials.

[0084] S4: first pressing and filling resin, pressing and filling resin on the second surface of the first substrate 1 to form a first resin layer 5;

[0085] That is, the embedding resin is pressed on the second surface of the first substrate 1, and the embedded resin forms the first resin layer 5. In this embodiment, the second surface of the first substrate 1 can be the upper surface of the first substrate 1. The embedding resin is pressed on the second surface of the first substrate 1, and specifically, a vacuum laminator can be used to press the resin on the second surface of the first substrate 1. During the process of pressing the embedding resin, the resin fills the gaps between the circuits on the surface of the first substrate 1 and the gaps around the chip 4. The structure formed after the first step of pressing and embedding the resin is as follows: Figure 5 shown.

[0086] The surface of the first resin layer 5 may be provided with a protective film, which may be removed before or after the blind hole 9 processing step. The protective film may prevent the first resin layer 5 from being contaminated.

[0087] In the first pressing and embedding resin step, an ABF (Ajinomoto Buildup Film) resin sheet may be selected. The ABF resin sheet includes an ABF layer, an OPP (O-phenylphenol) film attached to a first side of the ABF layer, and a PET (polyethylene glycol terephthalate) film attached to a second side of the ABF layer.

[0088] In the first lamination and resin embedding step, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is lamination-bonded to the second side of the first substrate 1 to form a first resin layer 5, and the side of the first resin layer 5 facing away from the first substrate 1 retains the PET film d. That is, in this step, the OPP film of the ABF resin sheet is torn off and the PET film d is retained. The ABF resin sheet is lamination-bonded to the second side of the first substrate 1 on one side of the OPP film removed.

[0089] Specifically, a vacuum laminator can be used for low-temperature vacuum lamination to press the ABF resin sheet with the OPP film removed onto the second surface of the first substrate 1. In this step, the ABF resin sheet is only laminated and leveled in the vacuum laminator. The vacuum laminator includes a vacuum laminating section and a leveling section. The vacuum laminating section is mainly used to press the ABF resin sheet onto the second surface of the first substrate 1. Since the surface of the inner layer circuit is uneven, the surface of the ABF resin sheet is still uneven after laminating by the vacuum laminating section. Then the leveling section levels the ABF resin sheet to make the surface of the ABF resin sheet flat.

[0090] The resin may be a GXT31 ABF resin sheet. Of course, the resin may also be a semi-cured PP (Prepreg) sheet or a copper-clad resin sheet RCC (Resin Coated Copper), the protective film of which is a copper foil layer, which is not limited here.

[0091] S5: second temporary bonding, disposing a second bonding material layer 7 on a side of the support plate 3 away from the first bonding material layer 2, and bonding the second bonding material layer 7 to a first surface of a second substrate 6 having an accommodating cavity 1a;

[0092] That is, the second bonding material layer 7 is bonded to the side of the support plate 3 facing away from the first bonding material layer 2 , and the second bonding material layer 7 is bonded to the first surface of the second substrate 6 . In this embodiment, the first surface of the second substrate 6 may be the upper surface of the second substrate 6 .

[0093] like Fig.18As shown, the second bonding material layer 7 may also include a foaming film a, a support film b and a pressure-sensitive adhesive film c stacked in sequence, and the foaming film a of the second bonding material layer 7 is bonded to the first surface of the second substrate 6. When the foaming film a is at the debonding temperature, it only takes a few minutes for the foaming film a to be debonded and the support plate 3 to fall off by itself. The debonding is easy to operate and does not require special equipment assistance.

[0094] The pressure-sensitive adhesive film c of the second bonding material layer 7 is bonded to the support plate 3, that is, the second bonding material layer 7 is located between the support plate 3 and the second substrate 6. The structure formed after the second temporary bonding step is as follows: Figure 6 As shown. In this embodiment, the second bonding material layer 7 can be 31950E temporary bonding adhesive produced by Nitto Company with a temperature of 200°C-210°C for thermal foaming and debonding. Of course, other temporary bonding adhesives can also be selected according to actual conditions, which is not limited here. Of course, the second bonding material layer 7 can also be a single-layer film structure or other types of multi-layer film structures, which is not limited here.

[0095] It should be noted here that the second bonding material layer 7 can be first bonded to the support plate 3 and then bonded to the second substrate 6. In this way, the second bonding material layer 7 can be bonded to the support plate 3 first for standby use. Of course, the second bonding material layer 7 can also be first bonded to the second substrate 6 and then bonded to the support plate 3, which is not limited here.

[0096] S6: attaching the second chip 4, placing the chip 4 in the accommodating cavity 1a of the second substrate 6;

[0097] The chip 4 is arranged in the accommodating cavity 1a of the second substrate 6. In this step, the electrode side of the chip 4 can be oriented toward the side away from the second bonding material layer 7, that is, the electrode of the chip 4 is placed downward, and the electrode side of the chip 4 can also be placed upward. When the accommodating cavity 1a is a through hole, the chip 4 can be in contact with the second bonding material layer 7, and when the electrode side of the chip 4 is upward, its electrode is in contact with the second bonding material layer 7.

[0098] When the second bonding material layer 7 includes a foaming film a, a supporting film b and a pressure-sensitive adhesive film c stacked in sequence, the chip 4 can be in contact with the foaming film a of the second bonding material layer 7, so that the chip 4 can be fixed in the accommodating cavity 1a by using the foaming film a. Specifically, when the electrode side of the chip 4 is facing upward, its electrode is in contact with the foaming film a of the second bonding material layer 7. The structure formed after the chip 4 is attached is as follows: Figure 7 shown.

[0099] Preferably, when the chip 4 is attached to the accommodating cavity 1a of the second substrate 6, the electrode side of the chip 4 can be oriented toward the side away from the second bonding material layer 7, that is, the electrode of the chip 4 faces downward, so that the foaming film a of the second bonding material layer 7 does not contact the chip 4 electrode, but contacts the back of the chip 4, which can prevent the chip 4 electrode surface from being contaminated, causing contamination to cause contaminants to be buried in the substrate to form serious reliability problems. It should be noted here that the chip 4 in the accommodating cavity 1a of the first substrate 1 and the chip 4 in the accommodating cavity 1a of the second substrate 6 can be arranged in opposite directions to be symmetrically arranged relative to the support plate 3. That is, the back of the chip 4 in the accommodating cavity 1a of the first substrate 1 contacts the first bonding material layer 2, and the back of the chip 4 in the accommodating cavity 1a of the second substrate 6 contacts the second bonding material layer 7. Alternatively, the surface of the chip 4 has a protective film to prevent the chip 4 electrode surface from being contaminated. After the bonding is released, the protective film on the surface of the chip 4 can be removed, and the protective film can be a film of copper foil or other materials.

[0100] S7: second pressing and filling resin, pressing and filling resin on the second surface of the second substrate 6 to form a second resin layer 8;

[0101] That is, the second surface of the second substrate 6 is pressed and filled with resin, and the filled resin forms a second resin layer 8. In this embodiment, the second surface of the second substrate 6 can be the lower surface of the second substrate 6. The second surface of the second substrate 6 is pressed and filled with resin, and specifically, a vacuum laminator can be used to press the resin on the second surface of the second substrate 6. During the pressing and filling resin process, the resin fills the gaps between the circuits on the surface of the second substrate 6 and the gaps around the chip 4. The structure formed after the second pressing and filling resin step is as follows: Figure 8 It is worth noting that no pre-curing is performed in the first pressing and embedding resin step and the second pressing and embedding resin step.

[0102] The surface of the second resin layer 8 may be provided with a protective film, which may be removed before or after the blind hole 9 processing step. The protective film may prevent the second resin layer 8 from being contaminated.

[0103] In the second pressing and embedding resin step, an ABF (Ajinomoto Buildup Film) resin sheet can also be selected. In the second pressing and embedding resin step, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is pressed on the second side of the second substrate 6 to form a second resin layer 8, and the side of the second resin layer 8 facing away from the second substrate 6 retains the PET film d. That is, in this step, the OPP film of the ABF resin sheet is torn off and the PET film d is retained. The ABF resin sheet removes one side of the OPP film and is pressed on the second side of the second substrate 6.

[0104] In this way, the PET film d can protect the ABF layer, and the PET film d can be torn off before or after processing the blind hole 9. The process of laminating the second resin layer 8 is also carried out in the vacuum laminator, which will not be described in detail here.

[0105] In this step, the resin can be specifically selected from the ABF resin sheet of model GXT31. Of course, the resin can also be a semi-cured PP sheet or a copper-clad resin sheet RCC, which is not limited here.

[0106] S8: first pre-curing, curing the resin in the structure formed in the previous step to more than 50%;

[0107] After the first resin layer 5 and the second resin layer 8 are pressed and buried, the first pre-curing is performed, that is, after the first resin layer 5 is pressed and buried, the pre-curing is not performed before the second resin layer 8 is pressed and buried.

[0108] Specifically, the resin in the structure formed in the previous step is cured to more than 50%, or in other words, the resin in the structure formed in the previous step is cured to a degree of curing of more than 50%, so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. The resin in the structure formed in this step can be cured to 50%, 60%, 70%, etc., but the first pre-curing can be low-temperature thermal curing, so that the first resin layer 5 and the second resin layer 8 are cured to a certain extent, but not completely cured. Before this step, no pre-curing treatment is performed.

[0109] S9: Processing blind holes 9, opening blind holes 9 on the upper and lower surfaces of the structure formed in the previous step;

[0110] That is, blind holes 9 are opened on the upper and lower surfaces of the structure formed in the previous step of the blind hole 9 processing step. In this embodiment, blind holes 9 are opened on the surfaces of the first resin layer 5 and the second resin layer 8, so that the circuits covered by the first resin layer 5 and the second resin layer 8 are electrically connected to other circuits through the blind holes 9. Specifically, the blind holes 9 can be opened by laser drilling. The structure formed after the blind hole 9 processing step is as follows: Fig. 9 shown.

[0111] S10: circuit fabrication, processing circuits on the upper and lower surfaces of the structure formed in the previous step;

[0112] Specifically, a circuit is processed on the surface of the structure formed by processing the blind hole 9 to form an inner layer circuit 10. In this embodiment, the circuit can be processed on the surface of the first resin layer 5 and the second resin layer 8, and the inner layer circuit 10 is electrically connected to the circuit covered by the first resin layer 5 and the second resin layer 8 through the blind hole 9. The structure formed after the circuit manufacturing step is as shown in FIG. Fig.11 shown.

[0113] S11: processing a resin insulation layer, providing a resin insulation layer on both the upper surface and the lower surface of the structure formed in the previous step, and performing pre-curing to cure the resin insulation layer formed in this step to more than 50%;

[0114] That is, the resin is pressed and buried on the upper and lower surfaces of the structure formed in the previous step to form a resin insulation layer on the upper and lower surfaces of the structure formed in the circuit making step. The resin fills the gaps between the circuits formed in the circuit making step. The resin insulation layer formed in this step covers the inner layer circuit 10 formed in the circuit making step and is partially in contact with the first resin layer 5 or the second resin layer 8. Pre-curing is performed to cure the resin insulation layer formed in this step to more than 50%, or in other words, the resin in the structure formed in this step is cured to a degree of curing of more than 50%, so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. The resin in the structure formed in this step can be cured to 50%, 60%, 70%, etc. This pre-curing is the second pre-curing, and the second pre-curing can be low-temperature thermal curing, so that the resin in the formed structure is cured to a certain extent, but not completely cured.

[0115] The resin insulation layer can also be made of an ABF resin sheet. In the processing of the resin insulation layer, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is pressed on the upper surface and the lower surface of the structure formed in the previous step, and pre-cured. A PET film d is retained on the side of the resin insulation layer away from the support plate 3 to protect the resin insulation layer from being contaminated.

[0116] In this step, the insulating layer resin can be specifically selected from the ABF resin sheet of model GXT31. Of course, the resin can also be a semi-cured PP sheet or a copper-clad resin sheet RCC, which is not limited here.

[0117] S12: manufacturing an intermediate circuit, repeating N times of blind hole 9 processing, circuit manufacturing and resin insulation layer processing steps, N ≥ 0, to form N layers of intermediate circuit 11, and no pre-curing is performed in the Nth resin insulation layer processing step, and pre-curing is performed after copper foil is pressed on the surface of the resin insulation layer formed in the Nth resin insulation layer processing step, so that the resin insulation layer in the formed structure is cured to more than 50%;

[0118] The steps of processing the blind hole 9, manufacturing the circuit and processing the resin insulation layer are repeated N times, N≥0. When N>0, N layers of intermediate circuits 11 can be processed in this step. When N=0, the outer layer circuit 13 is directly processed. That is, each time the steps of processing the blind hole 9, manufacturing the circuit and processing the resin insulation layer are repeated once, one layer of intermediate circuit 11 is processed. The method for manufacturing the board-level fan-out packaging structure provided in the application can process substrates of any number of layers, and is not limited to odd or even layers.

[0119] The key point in this embodiment is that, except for the Nth resin insulation layer processing step, each of the other resin insulation layer processing steps performs a pre-curing after the resin insulation layer is set on the circuit surface, and the curing is not complete. In addition, during the manufacturing process of the intermediate circuit, the two sides of the support plate are always symmetrically processed with completely identical wiring layers and insulation layers, so the entire sandwich temporary bonding structure has a symmetrical stress distribution, and is at an extremely low warpage level during multi-layer wiring processing, and will not cause the problem of being unable to be processed due to basic warpage.

[0120] Furthermore, after the copper foil is pressed on the surface of the resin insulation layer formed in the Nth resin insulation layer processing step, pre-curing is performed to cure the resin insulation layer in the formed structure to more than 50%.

[0121] Specifically, copper foil is laminated on the surface of the outermost resin insulating layer in the structure formed in the step of making the intermediate circuit. In this embodiment, copper foil can be laminated on the upper and lower surfaces of the structure formed in the step of making the intermediate circuit. It should be noted that if the surface of the outermost resin layer in the structure formed in the previous step has a PET film, the PET film is removed, and then the copper foil is laminated, and then pre-cured to cure the resin insulating layer in the structure to more than 50%. The structure formed after the copper foil lamination step is as follows: Fig.12 shown.

[0122] Alternatively, the resin insulation layer and the copper foil may be pressed together in the Nth resin insulation layer processing step, that is, when the last resin insulation layer is pressed, the last resin insulation layer and the copper foil are pressed together.

[0123] It should be noted that in the step of making the intermediate circuit S12, no pre-curing is performed after the resin insulation layer is pressed in the last resin insulation layer processing, or no pre-curing is performed in the Nth resin insulation layer processing, that is, the copper foil is directly pressed after the resin insulation layer is pressed, and then pre-curing is performed. In the step of making the intermediate circuit S12, except for the last resin insulation layer processing, pre-curing is performed after the resin insulation layer is pressed in the remaining N-1 resin insulation layer processing steps.

[0124] S13: debonding, debonding the first bonding material layer 2 from the first surface of the first substrate 1, and debonding the second bonding material layer 7 from the first surface of the second substrate 6;

[0125] The first bonding material layer 2 is separated from the first surface of the first substrate 1, and the first substrate 1 and the first bonding material layer 2 are debonded. Fig.13As shown. The second bonding material layer 7 is separated from the first surface of the second substrate 6. Specifically, the structure formed in the previous step can be heated to the debonding temperature of the first bonding material layer 2 and the second bonding material layer 7, and maintained for 1 min-3 min to achieve debonding. Therefore, the first bonding material layer 2 and the second bonding material layer 7 can be the same, so that the debonding temperatures of the first bonding material layer 2 and the second bonding material layer 7 are the same.

[0126] S14: thirdly press-filling the resin, press-filling the resin on the first surface of the first substrate 1 and press-filling the copper foil on the surface of the formed resin layer to obtain a first temporary structure, press-filling the resin on the first surface of the second substrate 6 and press-filling the copper foil on the surface of the formed resin layer to obtain a second temporary structure;

[0127] That is, the embedding resin is pressed on the first surface of the first substrate 1, and the third resin layer 12 of the first substrate 1 is formed. Specifically, the resin can be pressed on the first surface of the first substrate 1 using a vacuum laminator. During the process of pressing and embedding the resin, the resin fills the gaps between the circuits on the surface of the first substrate 1 and the gaps around the chip 4. After the embedding resin is pressed on the first surface of the first substrate 1, copper foil is pressed on the surface of the formed resin layer, that is, copper foil is pressed on the surface of the third resin layer 12. The structure formed after the embedding resin and copper foil are pressed on the first surface of the first substrate 1 is as shown in FIG. Fig.14 As shown, this structure is a first temporary structure.

[0128] The resin is pressed and embedded on the first surface of the second substrate 6 to form a resin insulation layer. Specifically, the resin can be pressed and embedded on the first surface of the second substrate 6 using a vacuum laminator. During the process of pressing and embedding the resin, the resin fills the gaps between the circuits on the surface of the second substrate 6 and the gaps around the chip 4. After the resin is pressed and embedded on the first surface of the second substrate 6, copper foil is pressed and embedded on the surface of the formed resin layer. The structure formed after the resin and copper foil are pressed and embedded on the first surface of the second substrate 6 is the second temporary structure.

[0129] An ABF resin sheet may also be used in the third resin lamination step. In the third resin lamination step, the OPP film of the ABF resin sheet is removed, and the first side of the ABF resin sheet is laminated to the first surface of the first substrate 1 or the first surface of the second substrate 6. In the first temporary structure, the PET film d is removed from the side of the resin insulation layer formed in the third resin lamination step facing away from the first substrate 1, and then the copper foil is laminated. In the second temporary structure, the PET film d is removed from the side of the resin insulation layer formed in the third resin lamination step facing away from the second substrate 6, and then the copper foil is laminated.

[0130] In this step, the resin can be ABF resin sheet with model GXT31. Of course, the resin can also be semi-cured PP sheet or copper-clad resin sheet RCC, which is not limited here. However, the resin material pressed on the first and second surfaces of the same substrate should be the same to prevent serious warping of the substrate.

[0131] S15: Second pre-curing, curing the resin in the first temporary structure and the second temporary structure to more than 50%;

[0132] Specifically, the first temporary structure and the second temporary structure are cured at a low temperature so that the resins in the first temporary structure and the second temporary structure are cured to more than 50%.

[0133] The second pre-curing may specifically include: curing the resin in the structure formed in this step to 50%-70%; specifically, the curing degree of the resin after the second pre-curing may be 50%, 60%, 70%, etc., so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. Preferably, the resin in the formed structure is cured to 70%.

[0134] Alternatively, the second pre-curing is specifically: placing the formed structure in a constant temperature environment of 130°C-155°C for 30min-60min to pre-cure the resin in the structure. Specifically, the formed structure can be placed in a constant temperature environment of 130°C, 135°C, 140°C or 150°C, and the holding time can be 25min, 30min or 35min. Preferably, the formed structure is placed in a constant temperature environment of 150°C for 30min-60min.

[0135] S16: The structure formed in the previous step is placed in a laminator, clamped by a mirror steel plate, under a preset vacuum degree and a preset pressure, so that the resin in the structure is cured to more than 90%;

[0136] High temperature curing can be used in this step. After this step is completed, the resin in the first temporary structure and the second temporary structure can be cured to more than 90%, that is, the degree of curing is more than 90%.

[0137] Specifically, the first temporary structure and the second temporary structure can be placed in a laminator, clamped by a mirror steel plate, in a constant temperature environment of 190°C-210°C to cure the resin in the structure to more than 90%. For example, the structure formed by circuit manufacturing can be placed in a constant temperature environment of 190°C, 195°C, 200°C, 205°C or 210°C to cure the resin in the structure to more than 90% or completely cured. Preferably, the structure formed by circuit manufacturing is placed in a constant temperature environment of 190°C-210°C, and at the same time, the environmental vacuum degree can be maintained at 1Pa-15Pa for 50min-70min. The preset vacuum degree is 1Pa-15Pa, and the preset pressure is 0.1MPa-0.5MPa. For example, the structure formed by circuit manufacturing is placed in a constant temperature environment of 200°C, while maintaining the environmental vacuum degree of 10Pa and the pressure of 0.5Mpa for 60min.

[0138] In this step, a laminator can be used, and two mirror steel plates can be used to clamp the first temporary structure or the second temporary structure respectively until this step is completed. It should be noted that in this application, all pre-curing and curing steps can be carried out in an oven.

[0139] S17: making an outer layer circuit, performing blind hole 9 processing and circuit making steps on the cured structure to form an outer layer circuit 13;

[0140] On the first temporary structure and the second temporary structure after solidification, blind holes 9 are processed and circuits are made to form an outer layer circuit 13. That is, blind holes 9 are opened again on the surface of the structure, and circuits are made to form an outer layer circuit 13. The outer layer circuit 13 is electrically connected to the internal circuit through the blind holes 9. After this step, the structure formed after the blind holes 9 are processed is as follows: Fig.15 As shown in the figure, after blind hole processing, the surface copper foil is removed by corrosion; the structure formed after circuit production is as follows Fig.16 shown.

[0141] S18: Making a solder resist layer, making a solder resist layer 14 on the surface of the outer layer circuit 13; the structure formed after the step of making the solder resist layer 14 is as follows Fig.17 shown.

[0142] S19: coating, coating the surface of the structure formed after the solder resist layer 14 is formed. The specific material of the coating can be NiPdAu (nickel palladium gold), NiAu (nickel gold), Sn (tin) or OSP (Organic Solderability Preservatives).

[0143] In the present application, since the circuits are arranged on the front and back sides of the substrate itself and the circuits on the front and back sides of the substrate are interconnected, it has advantages for the subsequent board-level fan-out package to form POP (Package-on-Package) interconnection, avoiding the subsequent manufacturing step of the conductive through-hole, utilizing the through-hole processing and mature manufacturing process of the substrate itself, avoiding the use of high aspect ratio plate copper column manufacturing technology, and reducing the difficulty of processing. In addition, during the manufacturing process of the intermediate circuit, the two sides of the support plate are always symmetrically processed with the same wiring layer and insulation layer, so the entire sandwich temporary bonding structure has a symmetrical stress distribution, and is at an extremely low warping level in the multi-layer wiring processing, and will not cause the problem of being unable to be processed due to basic warping. And the first pre-curing is performed only after the first pressing and embedding resin and the second pressing and embedding resin are completed, and each time a layer of the intermediate circuit 11 is processed and the resin insulation layer is set on the circuit surface, a pre-curing is performed, and it is not completely cured until all the resins are pressed and embedded and finally cured once, so that the resin in the structure is cured to more than 90%. The resin in the board-level fan-out packaging structure is in a semi-cured state before curing. At this time, the modulus of the resin material in the board-level fan-out packaging structure is low, and the substrate is in a low stress and low warping state. In this way, the process of attaching the chip 4, forming the first resin layer 5 and the second resin layer 8, and making the intermediate circuit 11 to the third pressing and filling resin are all completed in a low warping state, avoiding warping and excessive bending of the substrate during the processing of the board-level fan-out packaging structure, and thus avoiding cracking and delamination of the formed structure.

[0144] In addition, in the manufacturing method of the board-level fan-out packaging structure of the present application, a first bonding material layer 2 and a first substrate 1 are arranged on one side of the support plate 3, and a second bonding material layer 7 and a second substrate 6 are arranged on the other side of the support plate 3, that is, the processing structures on both sides of the support plate 3 are symmetrically arranged, and the supporting function of the support plate 3 is fully utilized. Two board-level fan-out packaging structures are processed at the same time, which improves the manufacturing efficiency and reduces the processing cost.

[0145] In a preferred embodiment, the first pre-curing is specifically: curing the resin in the structure formed in this step to 50%-70%; that is, the curing degree of the resin after the first pre-curing is 50%-70%, and the curing degree of the resin after the first pre-curing can be 50%, 60%, 70%, etc., so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. Preferably, the resin in the formed structure is cured to 70%.

[0146] Alternatively, the first pre-curing is specifically: placing the formed structure in a constant temperature environment of 130°C-155°C for 30min-60min to pre-cure the resin in the structure. Specifically, the formed structure can be placed in a constant temperature environment of 130°C, 135°C, 140°C or 150°C, and the holding time can be 25min, 30min or 35min. Preferably, the formed structure is placed in a constant temperature environment of 150°C for 30min-60min.

[0147] The pre-curing in the resin insulation layer processing step S11 is specifically: the resin in the structure formed in this step is cured to 50%-70%; that is, the curing degree of the resin after curing in step S11 is 50%-70%, and the curing degree of the resin insulation layer formed in this step can be 50%, 60%, 70%, 75%, etc., so as to harden the resin and improve the rigidity and mechanical impact resistance of the resin. Preferably, the resin in the formed structure is cured to 70%.

[0148] Alternatively, the pre-curing in the resin insulation layer processing step of step S11 is specifically: placing the formed structure in a constant temperature environment of 130°C-155°C for 30min-60min to pre-cure the resin in the structure. Specifically, the formed structure can be placed in a constant temperature environment of 130°C, 135°C, 140°C or 150°C, and the holding time can be 25min, 30min or 35min. Preferably, the formed structure is placed in a constant temperature environment of 150°C for 30min-60min.

[0149] Of course, specific parameters of the first pre-curing and the pre-curing in the resin insulation layer processing step S11 may also be adjusted according to actual conditions, and are not specifically limited here.

[0150] In another embodiment, when the raw materials used in the first pressing and embedding resin step and the second pressing and embedding resin step are both ABF resin sheets, step S17 before manufacturing the outer layer circuit also includes step S17': etching the copper foil to remove the copper foil on the surface of the structure formed in the previous step to facilitate subsequent circuit processing.

[0151] As an optional implementation, after step S13, step S13' of cleaning is further included: cleaning the first surface of the first substrate 1 and the first surface of the second substrate 6. In this way, resin residue can be prevented from remaining on the first surface of the first substrate 1 and the first surface of the second substrate 6. Specifically, a plasma cleaning machine can be used for cleaning, for example, in a degumming tank at 70°C-85°C for 2min-5min. Of course, other cleaning methods can also be used, such as ultrasonic alkaline solution cleaning, which is not limited here.

[0152] As an optional embodiment, the curing temperature of the first pre-curing and the curing temperature of the pre-curing in the resin insulation layer processing step are lower than the debonding temperature of the first bonding material layer 2 and the second bonding material layer 7. In this way, it can be ensured that when the first pre-curing and the pre-curing in the resin insulation layer processing step are performed, the first bonding material layer 2 is still bonded to the first substrate 1, and the second bonding material layer 7 is still bonded to the second substrate 6. Specifically, the curing temperature of the first pre-curing and the curing temperature of the pre-curing in the resin insulation layer processing step can be more than 10°C lower than the debonding temperature of the first bonding material layer 2 and the second bonding material layer 7. Preferably, the curing temperature of the first pre-curing and the curing temperature of the pre-curing in the resin insulation layer processing step can be 20°C lower than the debonding temperature of the first bonding material layer 2 and the second bonding material layer 7.

[0153] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.

[0154] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for manufacturing a board-level fan-out packaging structure, characterized in that: include: Opening windows on substrates: opening cavities for accommodating chips on multiple substrates, with circuits arranged on both the front and back sides of the substrates and interconnected with each other; A first temporary bonding is performed to bond the first surface of the first substrate having the accommodating cavity to the first bonding material layer, and a support plate is fixed to a side of the first bonding material layer facing away from the first substrate; A first chip mounting method is to place the chip in the accommodation cavity of the first substrate; A first pressing and filling resin, pressing and filling the resin on the second surface of the first substrate to form a first resin layer; Second temporary bonding, disposing a second bonding material layer on a side of the support plate away from the first bonding material layer, and bonding the second bonding material layer to the first surface of the second substrate having the accommodating cavity; A second chip mounting method is to place the chip in the receiving cavity of the second substrate; A second pressing and filling resin, pressing and filling the resin on the second surface of the second substrate to form a second resin layer; The first pre-curing cures the resin in the structure formed in the previous step to more than 50%; Blind hole processing, opening blind holes on the upper and lower surfaces of the structure formed in the previous step; Circuit fabrication, processing circuits on the upper and lower surfaces of the structure formed in the previous step; Resin insulation layer processing, providing resin insulation layers on both the upper and lower surfaces of the structure formed in the previous step, and pre-curing to cure the resin insulation layer formed in this step to more than 50%; To make an intermediate circuit, repeat the steps of blind hole processing, circuit production and resin insulation layer processing N times, N ≥ 0, to form an N-layer intermediate circuit, and no pre-curing is performed in the N-th resin insulation layer processing step, and pre-curing is performed after copper foil is pressed on the surface of the resin insulation layer formed in the N-th resin insulation layer processing step, so that the resin insulation layer in the formed structure is cured to more than 50%; Debonding, debonding the first bonding material layer from the first surface of the first substrate, and debonding the second bonding material layer from the first surface of the second substrate; Thirdly, the resin is pressed and embedded, the resin is pressed and embedded on the first surface of the first substrate and the copper foil is pressed on the surface of the formed resin layer to obtain a first temporary structure, and the resin is pressed and embedded on the first surface of the second substrate and the copper foil is pressed on the surface of the formed resin layer to obtain a second temporary structure; The second pre-curing cures the resin in the first temporary structure and the second temporary structure to more than 50%; Curing: the structure formed in the previous step is placed in a laminator, clamped by a mirror steel plate, under a preset vacuum degree and a preset pressure, so that the resin in the structure is cured to more than 90%; Fabricating an outer layer circuit, performing blind hole processing and circuit fabrication steps on the cured structure to form an outer layer circuit; Making a solder resist layer, and making a solder resist layer on the surface of the outer layer circuit; A coating is applied on the surface of the structure formed after the solder resist layer is made.

2. The method for manufacturing a board-level fan-out packaging structure according to claim 1, characterized in that: The first bonding material layer comprises a foaming film, a supporting film and a pressure-sensitive adhesive film which are stacked in sequence, and the foaming film of the first bonding material layer is bonded to the first surface of the first substrate, and the pressure-sensitive adhesive film of the first bonding material layer is bonded to the supporting plate; and / or, The second bonding material layer includes a foaming film, a supporting film and a pressure-sensitive adhesive film stacked in sequence, and the foaming film of the second bonding material layer is bonded to the first surface of the second substrate, and the pressure-sensitive adhesive film of the second bonding material layer is bonded to the side of the supporting plate facing away from the first bonding material layer.

3. The method for manufacturing a board-level fan-out packaging structure according to claim 1, characterized in that: The first pre-curing is specifically: curing the resin in the structure formed in this step to 50%-70%; or, the first pre-curing is specifically: placing the formed structure in a constant temperature environment of 130°C-155°C for 30min-60min to pre-cure the resin in the structure.

4. The method for manufacturing a board-level fan-out packaging structure according to claim 1, characterized in that: The pre-curing in the resin insulation layer processing step is specifically: curing the resin insulation layer in the structure to a degree of 50%-70%; or, the pre-curing in the resin insulation layer processing step is specifically: placing the formed structure in a constant temperature environment of 130°C-155°C for 30min-60min to pre-cure the resin in the structure.

5. The method for manufacturing a board-level fan-out packaging structure according to claim 1, characterized in that: The curing is specifically as follows: placing the formed structure in a laminator, clamping it between two mirror steel plates, the mirror steel plates having a pressure of 0.1MPa-0.5MPa, in an environment of a constant temperature of 190°C-210°C and a vacuum degree of 1Pa-15Pa, maintaining it for 50min-70min to cure the resin in the structure. The constant temperature of 190°C-210°C and the vacuum degree of 1Pa-15Pa are maintained for 50min-70min to solidify the resin in the structure.

6. The method for manufacturing a board-level fan-out packaging structure according to claim 1, characterized in that: The raw materials used in the first pressing and filling resin step, the second pressing and filling resin step, the resin insulation layer processing step and the third pressing and filling resin step are all ABF resin sheets, and the ABF resin sheet includes an ABF main layer, an OPP film attached to the first side of the ABF main layer, and a PET film attached to the second side of the ABF main layer.

7. The method for manufacturing a board-level fan-out packaging structure according to claim 6, characterized in that: The first pressing and filling resin step specifically comprises: removing the OPP film of the ABF resin sheet, and pressing the first side of the ABF resin sheet onto the second surface of the first substrate to form a first resin layer, wherein the first resin layer has a PET film retained on a side away from the first substrate; The second resin embedding step is specifically to remove the OPP film of the ABF resin sheet and to laminate the first side of the ABF resin sheet onto the second surface of the second substrate to form a second resin layer, wherein the PET film is retained on the side of the second resin layer away from the second substrate.

8. The method for manufacturing a board-level fan-out packaging structure according to claim 1, characterized in that: Before manufacturing the outer layer circuit, the method further comprises the step of: etching the copper foil to remove the copper foil on the surface of the structure formed in the previous step.

9. The method for manufacturing a board-level fan-out packaging structure according to any one of claims 1 to 8, characterized in that: After the debonding step, the method further includes: cleaning, cleaning the first surface of the first substrate and the first surface of the second substrate.

10. The method for manufacturing a board-level fan-out packaging structure according to any one of claims 1 to 8, characterized in that: The curing temperature of the first pre-curing and the curing temperature of the pre-curing in the resin insulating layer processing step are lower than the debonding temperatures of the first bonding material layer and the second bonding material layer.

Citation Information

Patent Citations

  • Method for manufacturing circuit board

    CN103874346A

  • Improved fanout panel level semiconductor chip package process

    CN104103527A

  • Laminated chip packaging structure and manufacturing method thereof

    CN111081564A

  • Chip packaging method and chip packaging structure based on fan-out packaging process

    CN111128760A

  • Fan-out plate level packaging method and fan-out plate level packaging structure