Wafer processing method
Through the combination of the hot pressing device and the thermoplastic sheet, the gap problem during the wafer segmentation process is solved, the productivity and effective area of the device chip are improved, and the stability and production efficiency of the partition groove are ensured.
Patent Information
- Application Number
- CN202410466694.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-04-18
- Publication Date
- 2024-11-12
AI Technical Summary
During the wafer division process, a gap between the adhesive tape and the wafer is caused by the step difference between the circular concave and the annular convex, resulting in a crack or fragmentation when the division groove is formed, and the gap between the adhesive tape expands with time, which affects the influence of Productivity and effective area of device chips.
The wafer is processed by a hot pressing device, and the wafer is fixed with the annular frame through the holding table of the hot pressing device, and the thermoplastic sheet is used to contact the wafer without locally applying large stress, so that the sheet is gradually heat-pressed to the wafer. On the other hand, a dividing groove is formed and the annular convex portion is removed.
The gap between the wafer and the hot pressing plate is effectively reduced, the productivity and effective area of the device chip are improved, the gap of the adhesive tape is expanded, and the stability and production efficiency of the wafer are ensured.
Smart Images

Figure CN118943082A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for processing a wafer having one surface having an annular convex portion on the outer periphery and a circular concave portion formed in a region surrounded by the annular convex portion. Background Art
[0002] Device chips are mounted in electronic devices such as mobile phones and personal computers. Device chips are generally manufactured by grinding a wafer having a plurality of devices such as ICs (Integrated Circuits) formed on the front side from the back side to thin it, and dividing the wafer into individual devices.
[0003] The wafer thinned by grinding has a reduced rigidity and is easily broken. Therefore, a region corresponding to a device formation region where a plurality of devices are formed on the back side of the wafer is ground to form a circular concave portion, and the surrounding portion is left as an annular convex portion. The annular convex portion serves to reinforce the thinned circular concave portion during wafer transport, etc. (for example, refer to Patent Document 1).
[0004] On the other hand, the annular convex portion will hinder the division when the wafer is divided into individual chips, so it is necessary to remove the annular convex portion from the wafer in advance. When removing the annular convex portion, an adhesive tape is pasted on the entire area of the back side of the wafer including the circular concave portion and the annular convex portion, and the wafer is held on the holding table through the adhesive tape. The holding table has a convex shape corresponding to the circular concave portion of the wafer, and the circular concave portion is consistent with the convex shape. Then, an annular dividing groove is formed on the wafer held by the holding table, and the annular convex portion is removed (for example, refer to patent document 2).
[0005] Patent Document 1: Japanese Patent Application Publication No. 2007-173487
[0006] Patent Document 2: Japanese Patent Application Publication No. 2011-61137
[0007] Here, when the adhesive tape is attached to one surface (back surface) of the wafer, a gap is generated between the adhesive tape and the wafer at the outer periphery of the circular concave portion due to the step difference between the circular concave portion and the annular convex portion. Furthermore, the wafer is not supported by the adhesive tape in the region overlapping the gap, so when the region is processed to form the dividing grooves, chipping or cracking may occur to an unacceptable degree on the wafer.
[0008] Therefore, it is necessary to form a dividing groove in an area that does not overlap with the gap. However, it is impossible to form a device on the wafer at the position where the dividing groove is formed. Therefore, when the dividing groove is formed to avoid the large gap, the effective area of the wafer is reduced and the productivity of the device chip is reduced.
[0009] In addition, when the adhesive tape is attached to one surface (back side) of the wafer, the adhesive tape is first attached to the annular convex portion, and then the adhesive tape is stretched inside the annular convex portion and attached to the circular concave portion under a large stress. Therefore, there is a problem that the gap between the adhesive tape and the wafer expands from the outer periphery of the circular concave portion as time passes from the attachment of the adhesive tape to the wafer. Summary of the invention
[0010] The present invention has been made in view of the above-mentioned problems, and its object is to provide a wafer processing method that can provide a sheet replacing the adhesive tape on one surface (back surface) of a wafer having a circular recess without generating a large gap and can suppress the expansion of the gap over time.
[0011] According to one embodiment of the present invention, a method for processing a wafer is provided, wherein a thermal compression bonding device is used to process the wafer, wherein the wafer has a surface having an annular convex portion on the outer periphery and a circular concave portion formed in an area surrounded by the annular convex portion, the thermal compression bonding device having: an upper chamber having a first concave portion connected to a first decompression unit and having a first opening; a lower chamber having a second concave portion connected to a second decompression unit and having a second opening; and a holding table disposed in the second concave portion for holding the wafer, wherein the upper chamber and the lower chamber can be closed by aligning the first opening and the second opening, and wherein the method for processing the wafer has the following steps: a holding step, wherein the holding table of the thermal compression bonding device is used to hold the wafer with one surface facing upward from below; a sealing step A step of clamping the sheet of the frame unit on the inner side of the opening by using the first opening of the first recess and the second opening of the second recess to close the first recess and the second recess, wherein the frame unit comprises: an annular frame having the opening in the center capable of accommodating the wafer; and the sheet fixed to the outer periphery of the annular frame; a decompression step of decompressing the first recess by using the first decompression unit and decompressing the second recess by using the second decompression unit after the sealing step; a contact step of increasing the pressure of the first recess after the decompression step so that the sheet contacts the one surface of the wafer and contacts the annular convex portion and the circular concave portion; and a hot pressing step of heating the sheet after the contact step so that the sheet is hot pressed to the one surface of the wafer.
[0012] Preferably, the wafer processing method further comprises the following steps: a dividing groove forming step, in which a dividing groove for cutting off the annular protrusion is formed on the wafer after the thermal compression bonding step; and a removing step, in which the annular protrusion is removed from the wafer after the dividing groove forming step.
[0013] In a wafer processing method according to one embodiment of the present invention, a sheet is brought into contact with an annular protrusion and a circular concave portion of a wafer, and the sheet is heated and thermally pressed to the wafer. Even if the sheet is in contact with the annular protrusion of the wafer, it will not adhere to the annular protrusion. Therefore, during the period until the sheet is in contact with the circular concave portion, the sheet is pulled into the circular concave portion from the outside of the annular protrusion. In this case, the stress applied to the sheet is dispersed, and the sheet is brought into contact with the circular concave portion without locally applying a large stress. Then, the sheet is thermally pressed to the wafer.
[0014] Thus, the sheet can be fixed to the wafer in a state where the gap between the wafer and the sheet is extremely small, so compared with the case where the adhesive tape is fixed to the wafer, the device formation area can be greatly reduced without considering the gap. That is, the effective area of the wafer can be relatively large, and the productivity of the device chip can be improved. In addition, no large stress is applied to the sheet that is thermally pressed to the wafer, so the expansion of the gap between the sheet and the wafer over time is also extremely limited.
[0015] Therefore, according to one embodiment of the present invention, a wafer processing method is provided, which can arrange a sheet replacing the adhesive tape on one surface (back surface) of a wafer having a circular recess without generating a large gap and can suppress the expansion of the gap over time. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 (A) is a perspective view schematically showing the back side (one side) of the wafer. Figure 1 (B) is a perspective view schematically showing the front side of the wafer.
[0017] Figure 2 (A) is a cross-sectional view schematically showing a thermal compression bonding device, Figure 2 (B) is a cross-sectional view schematically showing the thermocompression bonding device in the holding step.
[0018] Figure 3 (A) is a cross-sectional view schematically showing a thermocompression bonding device in a sealing step, Figure 3 (B) is a cross-sectional view schematically showing the thermocompression bonding device in the decompression step.
[0019] Figure 4 is a cross-sectional view schematically showing a thermocompression bonding device in a contacting step.
[0020] Figure 5 (A) is a cross-sectional view schematically showing a state where the sheet contacts the annular convex portion of the wafer. Figure 5 (B) is a cross-sectional view schematically showing a state where the sheet contacts the circular recess of the wafer.
[0021] Figure 6(A) is a cross-sectional view schematically showing a state where the adhesive tape contacts the annular convex portion of the wafer. Figure 6 (B) is a cross-sectional view schematically showing a state where the protection sheet is in contact with the circular recessed portion of the wafer.
[0022] Figure 7 (A) is a cross-sectional view schematically showing a state where the sheet is integrated with the wafer and the annular frame, Figure 7 (B) is a cross-sectional view schematically showing a state where the annular protrusion is separated from the wafer in the removal step.
[0023] Figure 8 : is a cross-sectional view schematically showing the cutting device in the dividing groove forming step.
[0024] Fig. 9 It is a flowchart showing the flow of each step of the wafer processing method.
[0025] Description of symbols
[0026] 11: wafer; 11a: front side; 11b: back side; 13: annular convex portion; 15: circular concave portion; 17: step difference; 19: predetermined dividing line; 21: device; 23: peripheral remaining area; 25: device forming area; 27: sheet; 29a, 29b: dots; 31: gap; 33: adhesive tape; 35a, 35b: dots; 37: gap; 39: annular frame; 39a: opening; 41: frame unit; 2: thermal compression bonding device; 4: upper chamber; 6: lower chamber; 8: first concave portion; 10: second concave portion; 12: first opening; 14: second opening Mouth; 16, 18: internal space; 20: first decompression unit; 22: second decompression unit; 24, 26: exhaust part; 28: first solenoid valve; 30: second solenoid valve; 32: holding table; 34: holding surface; 36: heater; 38: cutting device; 40: chuck table; 42: frame; 44: porous component; 46: holding surface; 48: circular convex part; 50: annular support part; 52: suction source; 54: suction path; 56: gasket; 58: cutting unit; 60: spindle; 62: spindle housing; 64: cutting tool; 66: cutting blade. DETAILED DESCRIPTION
[0027] An embodiment according to one aspect of the present invention will be described with reference to the drawings. Figure 1 (A) is a perspective view schematically showing the back side (one side) of the wafer. Figure 1 (B) is a perspective view schematically showing the front side of the wafer. First, a wafer processed by the wafer processing method of the present embodiment will be described.
[0028] The wafer 11 is a disk-shaped single crystal substrate formed of a semiconductor material such as silicon (Si) or silicon carbide (SiC). However, the shape, structure, size, etc. of the wafer 11 are not limited. Figure 1 As shown in FIG. 1B , a plurality of planned dividing lines 19 are set in a grid pattern on the front surface 11 a of the wafer 11. In each region partitioned by the plurality of planned dividing lines 19, a device 21 such as an IC or LSI is formed.
[0029] In the front surface 11a of the wafer 11, the area surrounding the outer periphery of the area where the plurality of devices 21 are formed is referred to as the outer peripheral remaining area 23. In addition, in the front surface 11a of the wafer 11, the area surrounded by the outer peripheral remaining area 23 and where the plurality of devices 21 are formed is referred to as the device forming area 25.
[0030] When the wafer 11 having a plurality of devices 21 formed thereon is ground and thinned from the back side 11b and the wafer 11 is divided along the predetermined dividing line 19, a plurality of thin device chips each having the device 21 are obtained. The division of the wafer 11 is performed, for example, by a cutting device having an annular cutting blade. However, the rigidity of the wafer 11 after grinding and thinning is reduced and it is easy to break, and operations such as transportation are not easy.
[0031] Therefore, if Figure 1 As shown in (A), a region corresponding to the device forming region 25 where a plurality of devices 21 are formed in the back surface 11b of the wafer 11 is ground to form a circular concave portion 15, and the periphery of the circular concave portion 15 is left as an annular convex portion 13. The annular convex portion 13 serves to reinforce the thinned circular concave portion 15 during the conveyance of the wafer 11. Thus, the rigidity of the wafer 11 is maintained, and it is not easy to be warped or broken, and it is easy to handle.
[0032] However, when the wafer 11 having the annular protrusion 13 on the back surface 11b is to be directly divided along the planned dividing line 19 by a cutting device, the thick annular protrusion 13 cannot be cut by the dividing groove formed in the wafer 11 in the same manner as the thin circular concave portion 15. In other words, the annular protrusion 13 will hinder the division when the wafer 11 is divided into individual chips.
[0033] Therefore, the annular convex portion 13 needs to be removed from the wafer 11 before the wafer 11 is divided. In the wafer processing method of the present embodiment, a sheet is thermally pressed onto the entire area of one surface (back surface 11b) of the wafer 11 including the circular concave portion 15 and the annular convex portion 13. The wafer 11 is held by a holding table of the dividing device via the sheet.
[0034] Next, the sheet bonded to the wafer 11 by thermal compression will be described. Figure 32 includes a schematic cross-sectional view of the sheet 27. The sheet 27 has a diameter larger than the outer diameter of the wafer 11 and does not have a paste layer. In addition, the sheet 27 is a thermoplastic sheet. The outer periphery of the sheet 27 is arranged on a metal ring frame 39 (see Figure 7 (A) Figure 7 (B) and Figure 8 ) on. The sheet 27 is, for example, a flexible resin sheet such as a polyolefin sheet or a polyester sheet, but the material of the sheet 27 is not limited thereto.
[0035] Here, the polyolefin-based sheet is a sheet of a polymer synthesized using olefin as a monomer. The polyolefin-based sheet used for the sheet 27 is, for example, a polyethylene sheet, a polypropylene sheet, a polystyrene sheet, or the like, which is transparent or translucent to visible light.
[0036] The polyester sheet is a polymer sheet 27 synthesized from dicarboxylic acid (a compound having two carboxyl groups) and diol (a compound having two hydroxyl groups) as monomers. The polyester sheet used for the sheet 27 is, for example, a sheet 27 transparent or translucent to visible light, such as a polyethylene terephthalate sheet or a polyethylene naphthalate sheet.
[0037] The sheet 27 does not have a paste layer (adhesive layer) and does not have sufficient adhesiveness, so it cannot be attached to the wafer 11. The sheet 27 has thermoplasticity, and when heated to a temperature near the melting point while being bonded to the wafer 11 under a predetermined pressure, it can be partially melted and fixed to the wafer 11. That is, the sheet 27 can be thermally pressed to the wafer 11.
[0038] In addition, if Figure 7 (A) Figure 7 (B) and Figure 8 As shown, the outer periphery of the sheet 27 is pre-arranged on a metal ring frame 39. The ring frame 39 has an opening (through hole) 39a having a diameter larger than the diameter of the wafer 11. For example, the sheet 27 is pre-bonded to the ring frame 39 by thermocompression. Alternatively, the sheet 27 is pre-bonded to the ring frame 39 by an adhesive or the like.
[0039] When the wafer 11, the sheet 27, and the annular frame 39 are finally integrated, a frame unit 41 is formed (see Figure 7 (A) Figure 7 (B), etc.). When the frame unit 41 is formed, the wafer 11 can be handled by the sheet 27, so the wafer 11 can be easily handled. In addition, when the wafer 11 as a part of the frame unit 41 is divided, the formed individual device chips are continuously supported by the sheet 27, so the device chips can also be easily handled.
[0040] Next, the thermocompression bonding apparatus 2 for thermocompression bonding the sheet 27 to the wafer 11 in the wafer processing method of the present embodiment will be described. Figure 2 (A) to Figure 4 A cross-sectional view schematically showing the thermocompression bonding device 2 is included.
[0041] Figure 2 (A) is a cross-sectional view schematically showing an example of a thermocompression bonding device 2. The thermocompression bonding device 2 is, for example, a chamber-shaped unit having a space capable of accommodating a wafer 11 inside, and has a function of thermocompression bonding the sheet 27 to the back surface 11b of the wafer 11. The thermocompression bonding device 2 has a concave lower chamber 6 opened upward and a concave upper chamber 4 disposed above the lower chamber 6 and opened downward.
[0042] The upper chamber 4 of the thermocompression bonding device 2 has a first recessed portion 8 connected to the first decompression unit 20 and having a first opening 12. The lower chamber 6 has a second recessed portion 10 connected to the second decompression unit 22 and having a second opening 14. The first decompression unit 20 and the second decompression unit 22 are, for example, vacuum pumps such as rotary pumps. However, the first decompression unit 20 and the second decompression unit are not limited thereto.
[0043] The thermocompression bonding device 2 has a holding table 32 disposed in the second recess 10 to hold the wafer 11. The upper chamber 4 and the lower chamber 6 can be closed by aligning the first opening 12 of the upper chamber 4 and the second opening 14 of the lower chamber 6.
[0044] The thermocompression bonding device 2 is described in more detail. The first opening 12 of the upper chamber 4 and the second opening 14 of the lower chamber 6 have an inner diameter larger than the diameter of the wafer 11. In addition, the first recess 8 of the upper chamber 4 and the second recess 10 of the lower chamber 6 have an outer diameter smaller than the inner diameter of the annular frame 39 provided on the outer periphery of the sheet 27.
[0045] For example, the upper chamber 4 can be raised and lowered. The second opening 14 of the lower chamber 6 is of the same shape as the first opening 12 of the upper chamber 4, and when the upper chamber 4 is lowered toward the lower chamber 6 in a manner that the first opening 12 overlaps with the second opening 14, a space isolated from the outside can be formed inside the upper chamber 4 and the lower chamber 6.
[0046] A table-shaped holding table 32 for supporting the wafer 11 is provided in the lower chamber 6. The upper surface of the holding table 32 is a flat holding surface 34 for supporting and holding the wafer 11. The holding table 32 may also have a suction path (not shown) connected to the holding surface 34 and a suction source (not shown) connected to the suction path. In this case, when the suction force generated by the suction source is applied to the wafer 11 placed on the holding surface 34 of the holding table 32 through the suction path, the holding table 32 can be used to suck and hold the wafer 11.
[0047] The height of the holding table 32 is adjusted so that the back side 11b of the wafer 11 is substantially the same height as the second opening 14 of the lower chamber 6 when the wafer 11 is placed on the holding surface 34. Alternatively, the height of the holding table 32 is adjusted so that the second opening 14 of the lower chamber 6 is higher than the back side 11b of the wafer 11.
[0048] An exhaust section 24 is connected to the top or side wall of the upper chamber 4. The exhaust section 24 is an exhaust path connected to the first recess 8 of the upper chamber 4 at one end and connected to the first decompression unit 20 at the other end. A first electromagnetic valve 28 (e.g., an electromagnetic valve) for switching the connection state between the upper chamber 4 and the first decompression unit 20 is provided on the exhaust path of the exhaust section 24. That is, when the first electromagnetic valve 28 is actuated, the connection state between the upper chamber 4 and the first decompression unit 20 and the disconnection state in which they are disconnected from each other are switched.
[0049] An exhaust portion 26 is connected to the bottom wall or the side wall of the lower chamber 6. The exhaust portion 26 is an exhaust path connected to the second recess 10 of the lower chamber 6 at one end and connected to the second decompression unit 22 at the other end. A second electromagnetic valve 30 (e.g., an electromagnetic valve) for switching the connection state between the lower chamber 6 and the second decompression unit 22 is provided on the exhaust path of the exhaust portion 26. That is, when the second electromagnetic valve 30 is actuated, the connection state between the lower chamber 6 and the second decompression unit 22 and the disconnection state in which they are disconnected from each other are switched.
[0050] When the first solenoid valve 28 is operated to connect the first decompression unit 20 and the upper chamber 4, the internal space 16 of the upper chamber 4 can be decompressed. In addition, when the second solenoid valve 30 is operated to connect the second decompression unit 22 and the lower chamber 6, the internal space 18 of the lower chamber 6 can be decompressed.
[0051] The thermocompression bonding device 2 has a heating unit for heating the wafer 11 placed on the holding table 32 and the sheet 27 placed on the wafer 11. For example, a heater 36 that can function as a heating unit is provided inside the holding table 32. The heater 36 is, for example, an electric heating wire. When the heater 36 is operated, the wafer 11 is heated, and the sheet 27 is heated through the wafer 11.
[0052] However, the heating unit of the thermal compression bonding device 2 is not limited thereto. For example, a heating unit (not shown) that supplies hot air to the internal space 16 of the upper chamber 4 may be provided in the first recess 8 of the upper chamber 4. The heating unit includes, for example, a blower that generates air flow and a heater that can heat the air. The wafer 11 is placed on the holding table 32 and the sheet 27 is arranged on the wafer 11. When hot air is supplied to the sheet 27 from the heating unit, the sheet 27 can be heated.
[0053] Next, a description will be given of a wafer processing method of the present embodiment performed using the thermocompression bonding apparatus 2. The wafer processing method of the present embodiment is performed as a part of a device chip manufacturing method of dividing the wafer 11 into device chips, for example. Fig. 9 This is a flowchart showing the flow of each step of a wafer processing method (device chip manufacturing method). The wafer processing method of this embodiment is described below, and the following description is also a description of each step of the device chip manufacturing method.
[0054] In the wafer processing method of the present embodiment, first, the holding step S10 is performed in which the wafer 11 with one surface (the back surface 11 b ) facing upward is held from below by the holding stage 32 of the thermocompression bonding device 2 . Figure 2 (B) is a cross-sectional view schematically showing the thermocompression bonding device 2 and the wafer 11 in the holding step S10.
[0055] In the holding step S10, the front side 11a of the wafer 11 is oriented downward, and the wafer 11 is moved to the top of the holding table 32 so that the front side 11a of the wafer 11 faces the holding surface 34 of the holding table 32. Then, the wafer 11 is placed on the holding surface 34 of the holding table 32, and the suction source of the holding table 32 is operated to suck and hold the wafer 11 by the holding table 32. At this time, one surface (the back side 11b) of the wafer 27 to be thermally pressed is exposed upward.
[0056] Next, the sealing step S20 is performed in which the sheet 27 fixed to the annular frame 39 is sandwiched between the upper chamber 4 and the lower chamber 6 of the thermocompression bonding device 2 to seal the internal space 16 of the upper chamber 4 and the internal space 18 of the lower chamber 6 . Figure 3 (A) is a cross-sectional view schematically showing the thermocompression bonding device 2 in the sealing step S20.
[0057] In the sealing step S20, the frame unit 41 (see Figure 7 (A) etc.) is placed in the lower chamber 6, and the frame unit 41 has: a ring-shaped frame 39 having an opening 39a capable of accommodating the wafer 11 in the center (refer to Figure 7 and the sheet 27 fixed to the outer periphery of the annular frame 39. At this time, the second opening 14 of the lower chamber 6 is blocked by the sheet 27. In addition, the position of the annular frame 39 is adjusted so that the annular frame 39 does not overlap with the first opening 12 and the second opening 14.
[0058] Then, the upper chamber 4 is lowered, and the sheet 27 of the frame unit 41 is sandwiched by the first opening 12 of the first recess 8 and the second opening 14 of the second recess 10 on the inner side of the opening 39a of the annular frame 39, thereby closing the first recess 8 and the second recess 10. At this time, the internal space 16 of the upper chamber 4 is sealed by the sheet 27 and the first recess 8. In addition, the internal space 18 of the lower chamber 6 is sealed by the sheet 27 and the second recess 10.
[0059] In the wafer processing method of this embodiment, after the sealing step S20 , the following decompression step S30 is performed: the first decompression unit 20 decompresses the first recess 8 and the second decompression unit 22 decompresses the second recess 10 . Figure 3 (B) is a cross-sectional view schematically showing the thermocompression bonding device 2 in the decompression step S30.
[0060] In the decompression step S30, the first solenoid valve 28 is operated to connect the first decompression unit 20 and the upper chamber 4. Then, the internal space 16 of the first recessed portion 8 of the upper chamber 4 is exhausted through the exhaust portion 24 by the first decompression unit 20, and the internal space 16 is decompressed. In addition, in the decompression step S30, the second solenoid valve 30 is operated to connect the second decompression unit 22 and the lower chamber 6. Then, the internal space 18 of the second recessed portion 10 of the lower chamber 6 is exhausted through the exhaust portion 26 by the second decompression unit 22, and the internal space 18 is decompressed.
[0061] In the chip processing method of this embodiment, after the decompression step S30, the following contact step S40 is implemented: the pressure of the first recess 8 is increased to make the sheet 27 contact with one surface (the back side 11b) of the chip 11, thereby making the sheet 27 contact with the annular protrusion 13 and the circular recess 15. Figure 4 2 is a cross-sectional view schematically showing the thermocompression bonding device 2 in the contact step S40 .
[0062] In the contact step S40, first, the first decompression unit 20 is stopped from decompressing the upper chamber 4. That is, the first electromagnetic valve 28 is operated to release the connection between the first decompression unit 20 and the upper chamber 4. At this time, the second electromagnetic valve 30 is not operated, and the connection between the second decompression unit 22 and the lower chamber 6 is maintained.
[0063] In this case, the pressure of the internal space 16 of the upper chamber 4 gradually rises. Alternatively, the thermal compression bonding device 2 may connect the upper chamber 4 to the outside air via the exhaust portion 24 or the like. In this case, when the upper chamber 4 is connected to the outside air, air flows rapidly into the internal space 16, and the pressure of the internal space 16 of the upper chamber 4 rises rapidly.
[0064] When the pressure of the internal space 16 of the upper chamber 4 is higher than the pressure of the internal space 18 of the lower chamber 6, a downward force is applied to the sheet 27 separating the internal space 16 and the internal space 18. Then, the sheet 27 is pushed toward one surface (back surface 11b) of the wafer 11 and deformed in a manner conforming to the shape of the one surface (back surface 11b) of the wafer 11.
[0065] In the contact step S40, the sheet 27 is initially in contact with the annular convex portion 13 on one surface (the back surface 11b) of the wafer 11. Alternatively, at the start of the contact step S40, the sheet 27 is already in contact with the annular convex portion 13. At this time, unlike an adhesive tape having a paste layer and having adhesive force, the sheet 27 is not attached to the annular convex portion 13. The sheet 27 can slide freely relative to the annular convex portion 13.
[0066] As the contact step S40 progresses, the sheet 27 is deformed in such a manner as to sink into the circular recess 15 on the inner side of the annular convex portion 13 and the sheet 27 advances toward the circular recess 15, and finally the sheet 27 contacts the circular recess 15. When the sheet 27 contacts a major portion of one surface (the back surface 11b) of the wafer 11 including the annular convex portion 13 and the circular recess 15, the contact step S40 is completed.
[0067] When the contact step S40 is completed, a force of sufficient magnitude for fixing the sheet 27 to the wafer 11 is not applied between the sheet 27 and the wafer 11. Therefore, in order to fix the sheet 27 to the wafer 11, after the contact step S40, a thermocompression step S50 is performed to heat the sheet 27 and thermocompress the sheet 27 to one surface (the back surface 11b) of the wafer 11.
[0068] In the thermocompression bonding step S50, the heating means of the thermocompression bonding apparatus 2 is operated to heat the sheet 27. For example, when the thermocompression bonding apparatus 2 has a heater 36 as the heating means, the heater 36 is operated to heat the sheet 27 together with the wafer 11.
[0069] When the sheet 27 is heated to a temperature near the melting point while the sheet 27 is pressed toward the wafer 11 by the pressure difference between the internal space 16 of the first recess 8 and the internal space 18 of the second recess 10, the sheet 27 is thermocompressed to the wafer 11. After the sheet 27 is thermocompressed, the heating unit (heater 36) is stopped to stop the heating of the sheet 27.
[0070] In addition, when performing thermal compression bonding, it is preferred to heat the sheet 27 to a temperature below the melting point. This is because when the heating temperature exceeds the melting point, the sheet 27 may melt and the shape of the sheet may not be maintained. In addition, it is preferred to heat the sheet 27 to a temperature above the softening point. This is because when the heating temperature does not reach the softening point, thermal compression bonding cannot be properly performed. That is, it is preferred to heat the sheet 27 to a temperature above the softening point and below the melting point.
[0071] In addition, a part of the sheet 27 may not have a clear softening point. Therefore, when performing thermocompression bonding, it is preferable to heat the sheet 27 to a temperature that is 20° C. lower than the melting point and is equal to or lower than the melting point.
[0072] For example, when the polyolefin sheet used as the sheet 27 is a polyethylene sheet, the heating temperature is preferably 120° C. to 140° C. Also, when the polyolefin sheet is a polypropylene sheet, the heating temperature is preferably 160° C. to 180° C. Also, when the polyolefin sheet is a polystyrene sheet, the heating temperature is preferably 220° C. to 240° C.
[0073] For example, when the polyester sheet used as the sheet 27 is a polyethylene terephthalate sheet, the heating temperature is 250° C. to 270° C. Also, when the polyester sheet is a polyethylene naphthalate sheet, the heating temperature is 160° C. to 180° C. However, the heating temperature of the sheet 27 is not limited thereto.
[0074] The heating unit is stopped to stop the heating of the sheet 27, and the second electromagnetic valve 30 is operated to disconnect the second decompression unit 22 from the lower chamber 6, so that the pressure of the internal space 18 of the lower chamber 6 is restored to atmospheric pressure, and then the upper chamber 4 is raised. Figure 7 As shown in (A), a frame unit 41 in which the sheet 27, the wafer 11 and the annular frame 39 are integrated is obtained.
[0075] Conventionally, when an adhesive tape having adhesiveness is attached to a wafer 11 having an annular protrusion 13 and a circular recess 15 on one surface (back surface 11b), a relatively large gap is generated between the adhesive tape and one surface of the wafer 11. In contrast, when the sheet 27 is thermally pressed to the wafer 11 using the wafer processing method of the present embodiment, a relatively small gap is generated between the sheet 27 and one surface of the wafer 11. One of the effects achieved by the wafer processing method of the present embodiment will be described in detail.
[0076] Figure 5 (A) is a cross-sectional view schematically showing the state in which the sheet 27 is in contact with the annular protrusion 13 on one surface (back surface 11b) of the wafer 11 in the contact step S40. At this moment, the sheet 27 is not thermally pressed and fixed to the wafer 11. Here, the focus is on the points 29a and 29b of the sheet 27 that overlap with the step 17 connecting the annular protrusion 13 and the circular recess 15.
[0077] When the contact step S40 is performed, the sheet 27 is pushed toward the circular recess 15 and deformed. Figure 5(B) is a cross-sectional view schematically showing a state in which the sheet 27 contacts the circular recess 15 on one surface (back surface 11b) of the wafer 11 in the contact step S40. At this point, the sheet 27 is not thermocompressed and fixed to the wafer 11 either.
[0078] Here, before the sheet 27 contacts the circular recess 15, the sheet 27 is also pulled in from the outside of the annular protrusion 13 toward the circular recess 15. Figure 5 As shown in (B), the points 29a and 29b of the sheet 27 also move. That is, as the points of the sheet 27 move greatly, the sheet 27 contacts the circular recess 15. Therefore, the stress applied to the sheet 27 is dispersed, and a large stress is not locally applied to the sheet 27 near the circular recess 15.
[0079] Furthermore, the sheet 27 is pulled sufficiently toward the circular recess 15, so that the gap 31 between the sheet 27 and the wafer 11 becomes extremely small. In addition, since no large stress remains on the sheet 27 thermally pressed onto the wafer 11, the peeling of the sheet 27 from the wafer 11 over time is extremely limited.
[0080] For comparison, a case where the adhesive tape is attached to the wafer 11 by a conventional method different from the wafer handling method of the present embodiment is examined. Figure 6 (A) is a cross-sectional view schematically showing a state in which the adhesive tape 33 is in contact with the annular convex portion 13 on one surface (back surface 11b) of the wafer 11. When the adhesive tape 33 is in contact with the annular convex portion 13 of the wafer 11, the adhesive tape 33 is fixed to the annular convex portion 13. Here, attention is paid to points 35a and 35b in the adhesive tape 33 that overlap with the step 17 connecting the annular convex portion 13 and the circular concave portion 15.
[0081] The adhesive tape 33 is pressed toward the circular recessed portion 15 and deformed. Figure 6 (B) is a cross-sectional view schematically showing a state in which the adhesive tape 33 is in contact with the circular concave portion 15 on one surface (back surface 11b) of the wafer 11. At this moment, the adhesive tape 33 is adhered and fixed to the circular concave portion 15 of the wafer 11. Here, the adhesive tape 33 is fixed to the annular convex portion 13, so that the adhesive tape 33 is not pulled into the circular concave portion 15 from the outside of the annular convex portion 13 before the adhesive tape 33 and the circular concave portion 15 are in contact.
[0082] Therefore, if Figure 6As shown in (B), the points 35a and 35b of the adhesive tape 33 do not move. That is, the adhesive tape 33 is deformed only in the area inside the annular protrusion 13, so that the adhesive tape 33 is attached to the circular recess 15. In this process, the adhesive tape 33 is locally deformed to a large extent, so that a large stress is locally applied to the adhesive tape 33. When the adhesive tape 33 is fixed to the circular recess 15 in a state where a large stress is applied, the adhesive tape 33 is easily peeled off from the wafer 11 as time passes.
[0083] In addition, the adhesive tape 33 is not pulled toward the circular recess 15, so a large gap 37 is formed between the adhesive tape 33 and the wafer 11. As described later, when the annular protrusion 13 is cut from the wafer 11, a cutting tool is made to cut into the outer periphery of the circular recess 15, but the circular recess 15 is not sufficiently supported in the portion overlapping with the gap 37, so it is not suitable for processing with a cutting tool.
[0084] Therefore, when removing the annular protrusion 13, the cutting tool must be cut into the wafer 11 at a position substantially inside the outer periphery of the circular recess 15. In this case, the device 21 cannot be formed in the area where the cutting tool is cut (see Figure 1 (B)), so the effective area of the wafer 11 is reduced, the number of device chips manufactured from the wafer 11 is reduced, and thus the manufacturing efficiency of the device chips is reduced.
[0085] In contrast, according to the wafer processing method of the present embodiment, the gap 31 generated between the sheet 27 and the wafer 1 is relatively small. Therefore, the wafer 11 can be cut by a cutting tool at a position closer to the outer periphery of the circular recess 15, so that a relatively large effective area of the wafer 11 can be ensured. That is, the number of device chips that can be manufactured from the wafer 11 can be increased, and the manufacturing efficiency of the device chips is improved. In addition, the gap 31 is not likely to expand over time, so the shelf life of the frame unit 41 after the sheet 27 is thermally pressed onto the wafer 11 is good.
[0086] In the wafer processing method of the present embodiment, after the thermocompression bonding step S50 , a dividing groove forming step S60 is performed to form a dividing groove for cutting off the annular convex portion 13 on the wafer 11 . Figure 8 It is a cross-sectional view partially showing the cutting device 38 for performing the dividing groove forming step S60.
[0087] Here, the cutting device 38 will be described. The cutting device 38 includes a chuck table 40 that holds the wafer 11 (frame unit 41 ) and a cutting unit 58 that cuts the wafer 11 held by the chuck table 40 .
[0088] The chuck table 40 includes a porous member 44 having a planar upper surface that can enter the circular recess 15, and a frame 42 that accommodates the porous member 44 and exposes the porous member 44 upward. The frame 42 mainly includes a circular convex portion 48 that supports the circular recess 15 of the wafer 11, and an annular support portion 50 that is arranged on the outer periphery of the circular convex portion 48 and mainly supports the annular convex portion 13 of the wafer 11.
[0089] The circular convex portion 48 of the frame 42 has a housing recess for housing the porous member 44 on the upper surface. The planar shape of the upper surface of the circular convex portion 48 is a shape that can enter the circular concave portion 15 of the wafer 11, and is slightly smaller than the circular concave portion 15. The annular support portion 50 of the frame 42 has a width (the distance between the inner periphery and the outer periphery) greater than the width (the distance between the inner periphery and the outer periphery) of the annular convex portion 13 of the wafer 11. The height difference between the upper surface of the annular support portion 50 and the upper surface of the circular convex portion 48 is equivalent to the height difference between the circular concave portion 15 and the annular convex portion 13 of the wafer 11.
[0090] A suction passage 54 is formed inside the frame 42. One end of the suction passage 54 is connected to the porous member 44, and the other end is connected to a suction source 52 such as an ejector. Figure 8 In FIG. 5 , for the sake of convenience of explanation, the suction path 54 is represented by a line.
[0091] When the wafer 11 (frame unit 41) is placed on the chuck table 40 and the suction source 52 is operated, negative pressure is applied to the wafer 11 (particularly, the main part of the circular recess 15) through the suction path 54 and the porous member 44. That is, the wafer 11 is held by suction on the chuck table 40. In addition, the upper surface of the circular protrusion 48 of the frame body 42 serves as a holding surface 46 for holding the wafer 11 by suction.
[0092] A gasket 56 is disposed on the upper surface of the annular support portion 50. The gasket 56 is formed of an elastic member such as a resin layer, and its thickness varies in accordance with the deviation of the height difference between the circular concave portion 15 and the annular convex portion 13 of the wafer 11. The suction path 54 formed inside the frame 42 may also be branched, and the branch path of the suction path 54 is connected to the gasket 56. When the suction source 52 is operated, negative pressure also acts on the wafer 11 (particularly the annular convex portion 13) through the branch path of the suction path 54 and the gasket 56. In this case, the wafer 11 is more firmly sucked and held.
[0093] In addition, a rotational drive source (not shown) such as a motor is connected to the chuck table 40, and the rotational drive source rotates the chuck table 40 around a rotation axis that is substantially parallel to the holding surface 46. In addition, a plurality of clamps (not shown) may be provided around the chuck table 40 to hold and fix the annular frame 39 that supports the wafer 11 via the sheet 27.
[0094] A cutting unit 58 for cutting the wafer 11 is disposed above the chuck table 40. The cutting unit 58 includes a cylindrical spindle 60 disposed in a direction substantially parallel to the holding surface 46 of the chuck table 40. An annular cutting tool 64 for cutting the wafer 11 is mounted at the front end (one end) of the spindle 60.
[0095] The base end (the other end) of the spindle 60 is rotatably accommodated in the spindle housing 62. A rotational drive source (not shown) such as a motor is accommodated in the spindle housing 62, and the base end of the spindle 60 is connected to the rotational drive source (not shown). The cutting tool 64 is rotated by the power transmitted from the rotational drive source via the spindle 60.
[0096] As the cutting tool 64 mounted on the front end of the spindle 60, for example, a hub-type cutting tool (hub tool) is used. The hub tool is composed of an annular base made of metal or the like and an annular cutting blade 66 formed along the outer periphery of the base. In addition, the cutting blade 66 of the hub-type cutting tool is composed of an electroformed grinder, and the electroformed grinder has abrasive grains made of diamond or the like fixed by a bonding material such as a nickel plating layer.
[0097] However, a washer-type cutting tool (waster tool) can also be used as the cutting tool 64. The washer tool is composed of an annular cutting edge 66 in which abrasive grains are fixed by a bonding material composed of metal, ceramic, resin, etc. In either case, the cutting tool 64 can cut the wafer 11 using the annular cutting edge 66.
[0098] The cutting unit 58 is connected to a moving unit (not shown) to adjust the position of the cutting tool 64 cutting into the wafer 11. The cutting unit 58 is connected to a lifting unit (not shown) to change the height position of the lower end of the annular cutting blade 66.
[0099] When the wafer 11 is cut by the cutting device 38 to remove the annular convex portion 13, first, the frame unit 41 is placed on the chuck table 40. At this time, the position of the wafer 11 is adjusted so that one surface (back surface 11b) of the wafer 11 faces the holding surface 46 and the center of the holding surface 46 overlaps with the center of one surface of the wafer 11. Then, the suction source 52 is operated, and the wafer 11 is sucked and held by the chuck table 40 via the sheet 27.
[0100] The position of the wafer 11 where the dividing groove is to be formed is set to a circular area centered on the center of the circular recess 15. According to the wafer processing method of this embodiment, the gap 31 between the wafer 11 and the sheet 27 is sufficiently small, so the area where the dividing groove is to be formed can be set to a position relatively outside the circular recess 15. By moving the cutting unit 58, the cutting edge 66 of the cutting tool 64 is positioned above the area where the dividing groove is to be formed.
[0101] Next, the rotation drive source provided inside the spindle housing 62 is operated to start the rotation of the cutting tool 64, and the cutting unit 58 is lowered to make the cutting blade 66 cut into the wafer 11. Then, the cutting unit 58 is lowered until the lower end of the cutting blade 66 reaches the height position of the sheet 27, and the rotation of the chuck table 40 is started. Then, when the chuck table 40 rotates one or more times, a circular dividing groove is formed on the wafer 11, and the annular convex portion 13 is cut off from the wafer 11.
[0102] In addition, the dividing groove forming step S60 is not limited to this. For example, the height of the cutting unit 58 is adjusted in advance so that the height of the lower end of the cutting blade 66 is lower than the height of the upper surface of the sheet 27 outside the wafer 11, so that the cutting blade 66 cuts into the outer periphery of the wafer 11. That is, the cutting unit 58 and the chuck table 40 are moved in a direction parallel to the holding surface 46, so that the cutting blade 66 cuts into the area where the dividing groove is to be formed. In this state, when the chuck table 40 is rotated once, a circular dividing groove is formed on the wafer 11.
[0103] After the dividing groove forming step S60 , a removing step S70 is performed to remove the annular convex portion 13 cut from the wafer 11 from the sheet 27 . Figure 7 (B) includes a cross-sectional view schematically showing the annular protrusion 13 when it is removed from the sheet 27 in the removal step S70. After the annular protrusion 13 is cut off from the wafer 11, when the frame unit 41 is removed from the chuck table 40, a portion of the circular recess 15 of the wafer 11 and the annular protrusion 13 remain on the sheet 27.
[0104] In this state, the annular protrusion 13 is lifted and peeled off from the sheet 27. Thus, a frame unit 41 is obtained in which the wafer 11, the sheet 27 and the annular frame 39 are integrated and removed from the annular protrusion 13. Then, when the wafer 11, the sheet 27 and the annular frame 39 are integrated along the dividing line 19 (see Figure 1 When the wafer 11 is divided by (B), individual device chips having the device 21 can be obtained.
[0105] As described above, the wafer processing method of this embodiment can provide the sheet 27 replacing the adhesive tape 33 without generating a large gap 31 on one surface (back surface 11b) of the wafer 11 having the circular recess 15, and can suppress the expansion of the gap 31 over time.
[0106] In addition, in the above-mentioned embodiment, the case where the dividing groove is formed on the wafer 11 using the cutting device 38 equipped with the cutting tool 64 in the dividing groove forming step S60 is described, but one embodiment of the present invention is not limited to this. That is, in the dividing groove forming step S60, a laser processing device (not shown) that can irradiate a laser beam to the wafer 11 and perform laser processing on the wafer 11 may also be used.
[0107] For example, a laser beam containing a wavelength component absorbed by the wafer 11 is irradiated to a region in the wafer 11 where a dividing groove is to be formed, and the wafer 11 is ablated. Alternatively, a laser beam containing a wavelength component that transmits the wafer 11 is focused on a region in the wafer 11 where a dividing groove is to be formed, a modified layer along the region is formed on the wafer 11, and the wafer 11 is divided with the modified layer as a dividing starting point. In this case, according to the wafer processing method of one embodiment of the present invention, the dividing groove can also be formed at a position relatively close to the outer periphery of the circular recess 15 of the wafer 11.
[0108] Furthermore, the structures, methods, and the like according to the above-described embodiments and modifications may be implemented with appropriate changes without departing from the scope of the purpose of the present invention. The above-described embodiments and modifications may also be combined as appropriate.
Claims
1. A method for processing a wafer, wherein the wafer is processed by a thermal compression bonding device, wherein the wafer has a surface having an annular convex portion on the outer periphery and a circular concave portion formed in an area surrounded by the annular convex portion, the thermal compression bonding device comprising: an upper chamber having a first concave portion connected to a first decompression unit and having a first opening; a lower chamber having a second concave portion connected to a second decompression unit and having a second opening; and a holding table disposed in the second concave portion for holding the wafer, wherein the upper chamber and the lower chamber can be closed by aligning the first opening and the second opening, wherein: The wafer processing method has the following steps: A holding step, using the holding workbench of the thermal compression bonding device to hold the wafer with one surface facing upward from below; A sealing step of clamping a sheet of a frame unit at the inner side of the opening by using the first opening of the first recess and the second opening of the second recess to close the first recess and the second recess, wherein the frame unit comprises: an annular frame having the opening in the center capable of accommodating the wafer; and the sheet fixed to the outer periphery of the annular frame; a decompression step, after the sealing step, decompressing the first recess by using the first decompression unit, and decompressing the second recess by using the second decompression unit; a contacting step of increasing the pressure of the first recessed portion after the decompression step to bring the sheet into contact with the one surface of the wafer so that the sheet contacts the annular convex portion and the circular recessed portion; and A thermocompression bonding step is performed after the contacting step, wherein the sheet is heated and thermocompressed to bond the sheet to the one surface of the wafer.
2. The wafer processing method according to claim 1, characterized in that: The wafer processing method also has the following steps: a dividing groove forming step of forming a dividing groove for cutting off the annular convex portion on the wafer after the thermal compression bonding step; and A removing step of removing the annular protrusion from the sheet after the dividing groove forming step.