Lead frame and manufacturing method thereof

By using smooth surface copper material and silver plating layer in the lead frame of the resin-sealed semiconductor package, combined with an anodized film formed by the blackening treatment liquid, the adhesion problem of welding and sealing resin is solved, and efficient and low-cost Manufacturing process.

CN118943112AInactive Publication Date: 2024-11-12CHANG WAH TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311156482.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-02
Filing Date
2023-09-08
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The lead frames of conventional resin-sealed semiconductor packages have problems in welding and sealing resin adhesion, especially due to solvent leakage caused by capillary phenomenon and short circuit caused by solder expansion, and the roughening treatment increases manufacturing process and cost.

Method used

A lead frame is formed by a copper material formed of a smooth surface, a silver plating layer is formed around the connecting plating layer, and an anodized film with a surface area ratio of 1.7 to 2.3 is formed by a blackening liquid, thereby avoiding the formation of a coarse and gentle area. Directly using smooth surfaces reduces manufacturing steps and costs.

Benefits of technology

Excellent adhesion with the sealing resin in resin sealing is achieved, manufacturing process and cost are reduced, while wetting and expansion of solvent components and short-circuiting of solder are prevented.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943112A_ABST
    Figure CN118943112A_ABST
Patent Text Reader

Abstract

The invention provides a lead frame and a manufacturing method thereof. The invention provides a lead frame which is not provided with a coarsening mitigation region, is suitable for welding of a connected part for realizing connection and conduction of semiconductor elements and connection by using a chip mounting material, has excellent sealing performance with a sealing resin when a semiconductor package is manufactured by resin sealing, and can be manufactured with high efficiency and low cost. A lead frame (1) is formed using a plate-shaped copper material (10), at least one surface of which is a smooth surface. A predetermined connection plating layer (11) is provided at a portion of a plate-shaped copper material (10) that is formed by a smooth surface and that is connected to achieve connection and conduction of semiconductor elements, a portion (10a) at which the smooth surface of the copper material (10) is exposed in a ring shape is provided around the connection plating layer (11), and an anodic oxide film (13) of the copper material (10) is provided at another portion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a lead frame used for a semiconductor package sealed by resin and a method for manufacturing the lead frame. Background Art

[0002] Generally speaking, resin-sealed semiconductor packages use metal lead frames and sealing resins. Moreover, copper alloy materials are mainly used as the base material of the lead frame. Epoxy resin is mainly used as the sealing resin. This type of semiconductor package sometimes has problems with the adhesion between the surface of the lead frame and the sealing resin. In the case of wire bonding installation, there is a problem that the solvent of the chip mounting material, which is a semiconductor element bonding paste for connecting semiconductor elements, seeps out and damages the adhesion with the sealing resin. In the case of flip-chip installation, when solder is used for electrical connection, there is a problem of solder expansion and short circuit, and a problem of further deterioration of the adhesion with the sealing resin due to the expanded solder.

[0003] Therefore, it is known that in order to improve the adhesion with the sealing resin, a lead frame used in a resin-sealed semiconductor package is subjected to a roughening treatment, that is, an anodic oxide film is formed on the entire surface except for the parts required for connection and conduction of the semiconductor element.

[0004] For example, Patent Document 1 below discloses a technique in which a silver plating layer is formed at a portion to be electrically bonded, an anodic oxide film is formed on the entire surface of a lead frame base material on which the silver plating layer is not formed, and then the silver plating layer is peeled off.

[0005] However, when the surface of the lead frame is roughened, the solvent components contained in the chip mounting material used when fixing the semiconductor element to the lead frame mounting surface are likely to wet and spread on the roughened surface formed on the lead frame surface due to the capillary phenomenon. The wet and spread solvent components will reduce the close adhesion between the lead frame and the sealing resin. In addition, there is a concern that wire bonding may be hindered when wire bonding is performed.

[0006] However, Patent Document 2 discloses a lead frame in which a roughened surface is formed and a portion of the formed roughened surface is filled to form a roughened relief surface with high flatness, thereby having two types of roughened surfaces, namely, a roughened region and a roughened relief region with higher flatness than the roughened region. This suppresses the wetting and expansion of solvent components caused by capillary phenomena, suppresses the reduction in adhesion with the resin, and avoids wire bonding obstacles.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2021-019095

[0010] Patent Document 2: Japanese Patent Application Publication No. 2022-103594 Summary of the invention

[0011] Problems to be solved by the invention

[0012] Regarding the lead frame disclosed in Patent Document 2, in its manufacturing method, a lead frame shape is formed from a metal plate, a plating layer that can be lead-bonded is partially formed, and then the entire surface of the lead frame formed with the plating layer is roughened to form a roughened area, and then a mold is used to press a part of the roughened area to form a roughening relief area.

[0013] However, the technology disclosed in Patent Document 2 requires a pressing process using a mold to form a roughening mitigation region after forming a roughening region, which increases the number of manufacturing steps and reduces manufacturing efficiency. In addition, manufacturing equipment is required for the pressing process using a mold, which increases costs.

[0014] Furthermore, it is known that when solder is used for electrical connection, for example, the bonding strength is higher when directly soldering to a copper material than when soldering is performed via a connection plating layer formed by stacking a nickel plating layer, a palladium plating layer, and a gold plating layer in that order. Therefore, a lead frame is required in which both the connection plating layer and the copper material used for electrical connection are exposed at the location where solder bonding is performed and the other surfaces are provided with an anodized film.

[0015] The present invention is made in view of the above-mentioned existing problems, and its purpose is to provide a lead frame and a manufacturing method thereof, wherein the lead frame does not have a roughening relaxation area, is suitable for welding of connection parts for connecting and conducting semiconductor elements, and is suitable for connection using chip mounting materials. When resin sealing is performed to manufacture semiconductor packages, the lead frame has excellent adhesion with sealing resin, and can be manufactured efficiently and at a reduced cost.

[0016] Methods for solving problems

[0017] In order to achieve the above-mentioned purpose, the lead frame of the present invention is characterized in that it is a lead frame formed using a plate-like copper material whose surface on at least one side is composed of a smooth surface, and a predetermined connection plating layer is provided at a portion on one side of the plate-like copper material composed of a smooth surface for connection and conduction of a semiconductor element, and a portion around the connection plating layer is provided where the smooth surface of the copper material is exposed in a ring shape, and an anodized film of the copper material is provided at other portions.

[0018] Furthermore, in the lead frame of the present invention, it is preferred that the surface area ratio of the smooth surface of the copper material is 1.0 to 1.3, and the surface area ratio of the anodized film is 1.7 to 2.3.

[0019] In the lead frame of the present invention, the connection plating layer preferably includes a plating layer formed by laminating a nickel plating layer, a palladium plating layer, and a gold plating layer in this order on the plate-like copper material.

[0020] In addition, the manufacturing method of the lead frame of the present invention is characterized in that it includes the following steps: a step of preparing a plate-shaped copper material having at least one side thereof constituted by a smooth surface with a surface area ratio of 1.0 to 1.3; a step of forming a plating resist mask having an opening corresponding to a portion to be connected in order to connect and conduct a semiconductor element on one side of the plate-shaped copper material constituted by the smooth surface in the form of a lead frame; a step of forming a predetermined connection plating layer on the plate-shaped copper material exposed from the opening of the plating resist mask; a step of forming a silver plating layer covering the connection using a silver plating bath having a characteristic of penetrating to the interface between the plating resist mask and the connection plating layer and the interface between the plating resist mask and the surrounding of the connection plating layer. The invention relates to a process of forming a silver-plated layer of the plate-shaped copper material under the plating resist mask which connects the upper surface and side surfaces of the plating layer and covers the periphery of the connecting plating layer; a process of removing the plating resist mask; a process of forming the plate-shaped copper material formed with the silver-plated layer into the shape of the lead frame; a process of immersing the plate-shaped copper material formed into the shape of the lead frame in an alkaline solution to remove the oxide film on the surface; a process of immersing the plate-shaped copper material from which the oxide film has been removed as an anode in a blackening treatment solution to form an anodic oxide film with a surface area ratio of 1.7 to 2.3 on the portion of the plate-shaped copper material not covered by the silver-plated layer; and a process of peeling off the silver-plated layer to expose the smooth surface of the copper material in a ring shape around the connecting plating layer.

[0021] In the lead frame manufacturing method of the present invention, it is preferred to use 1.5 A / dm 2 The above-mentioned anodic oxide film is formed at the following low current density.

[0022] Furthermore, in the method for manufacturing a lead frame of the present invention, it is preferable that the silver plating bath is a high cyanide bath.

[0023] Furthermore, in the lead frame manufacturing method of the present invention, it is preferable that the connection plating layer is formed by laminating a nickel plating layer, a palladium plating layer, and a gold plating layer in this order on the plate-like copper material.

[0024] Effects of the Invention

[0025] According to the present invention, a lead frame and a method for manufacturing the lead frame can be obtained. The lead frame does not have a roughening relaxation area and is suitable for connection of semiconductor elements, conductive welding, and connection using chip mounting materials. When resin sealing is performed to manufacture a semiconductor package, the lead frame has excellent adhesion with the sealing resin and can be manufactured efficiently and at a reduced cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The present invention is an explanatory diagram schematically showing an example of a lead frame for flip chip mounting manufactured by a lead frame manufacturing method according to an embodiment of the present invention from one side, wherein (a) is a plan view and (b) is a partial enlarged view of (a).

[0027] Figure 2 The present invention is an explanatory diagram schematically showing an example of a lead frame for flip-chip mounting manufactured by a lead frame manufacturing method according to an embodiment of the present invention from the other side, wherein (a) is a plan view and (b) is a partial enlarged view of (a).

[0028] Figure 3 It is an explanatory diagram showing an example of a manufacturing process of a lead frame for flip chip mounting according to one embodiment of the present invention.

[0029] Figure 4 The present invention schematically illustrates a lead frame for wire bonding as another example of a lead frame manufactured by a lead frame manufacturing method according to an embodiment of the present invention, wherein (a) is a plan view viewed from one side, and (b) is a plan view viewed from the other side.

[0030] Explanation of symbols

[0031] 1: lead frame; 10: lead frame substrate (metal plate, plate-shaped copper material); 10a: portion where the smooth surface of the copper material is exposed in a ring shape; 11: plating layer for connection; 12: silver plating layer; 13: anodized film; 30: anti-etching mask for plating; 31: anti-etching mask for etching; R1, R2: anti-etching layer. DETAILED DESCRIPTION

[0032] Prior to the description of the embodiments, the process of deriving the present invention and the effects of the present invention will be described.

[0033] The technology disclosed in Patent Document 1 is a technology applied for by the applicant of the present application and derived by inventors and the like who are different from the inventors and the like of the present application.

[0034] In this technology, as a measure for manufacturing a lead frame in which a metal plate is exposed at a portion that needs to be connected in order to achieve connection and conduction of semiconductor elements, and an oxide film is formed on the entire surface except for the portion that needs to be connected, during repeated experiments, it was studied that even if the mask is immersed in a blackening treatment liquid that forms an anodized film, the mask will not peel off in the middle and the plating layer that can reduce the manufacturing cost is used, and thus it was concluded to use a silver plating layer.

[0035] Therefore, the inventors of the present application used the technology of patent document 1 and conducted the following research to obtain a lead frame that does not have a roughening relaxation area, is suitable for welding of connection parts for connecting and conducting semiconductor elements, and is suitable for connection using chip mounting materials, and has excellent adhesion with sealing resin when resin sealing is performed to manufacture semiconductor packages.

[0036] First, the inventors of the present application tried to use the technology of Patent Document 1, for example, forming a silver-plated layer of the same size on a connection-use plating layer formed by stacking a nickel-plated layer, a palladium-plated layer, and a gold-plated layer in that order at a location where connection is required, using the silver-plated layer as a mask to form an anodized film and then removing the silver-plated layer.

[0037] However, in such a method, for example, the anodized film becomes close to the periphery of the connection plating layer stacked on the portion to be connected, and the following problem cannot be eliminated: the solvent component contained in the chip mounting material used when fixing the semiconductor element to the lead frame mounting surface wets and spreads on the roughened surface formed on the lead frame surface due to capillary phenomenon, thereby reducing the adhesion with the sealing resin.

[0038] Moreover, when a silver-plated layer of the same size is formed on the connection plating layer stacked on the part that needs to be connected, copper ions are dissolved in the blackening treatment liquid used when forming the anodized film on the exposed surface of the subsequent metal plate (plate-shaped copper material), which easily causes the silver-plated layer and the side of the connection plating layer to discolor. Even if the silver-plated layer is removed, the lead frame will have discoloration on the peripheral edge of the connection plating layer, and the adaptability of the connection plating layer will be reduced, which will greatly damage the value of the product.

[0039] Therefore, the inventors of the present application have considered that it is necessary to provide a region corresponding to the roughening mitigation region described in Patent Document 2 between the connection plating layer and the anodized film.

[0040] However, when providing a roughening mitigation region as described in Patent Document 2, a process is required to press a portion of the roughening region using a mold, which increases the number of manufacturing steps and reduces manufacturing efficiency. In addition, manufacturing equipment is required for the pressing process using a mold, which increases costs.

[0041] Therefore, the inventors of the present application have studied a countermeasure for preventing the solvent components contained in the die attach material from spreading to the roughened surface of the anodic oxide film due to the capillary phenomenon without providing a roughening mitigation area. In addition, it is believed that by forming a silver plating layer over a large area around the entire circumference of the connection plating layer, and removing the silver plating layer after the anodic oxide film is formed, a smooth surface of the lead frame substrate can be provided between the connection plating layer and the anodic oxide film, and the solvent components contained in the die attach material used for connection to achieve connection and conduction of the semiconductor element can be prevented from spreading to the roughened surface of the anodic oxide film due to the capillary phenomenon.

[0042] Furthermore, in order to form a silver-plated layer over a large area around the entire connection plating layer while using the technology of Patent Document 1, the inventors of the present application considered separately forming a plating resist mask for forming the connection plating layer and a plating resist mask for forming the silver-plated layer to form a lead frame, and carried out the following first trial production.

[0043] (1st trial production)

[0044] A copper material (metal plate) having a surface area ratio of 1.3 or less for a lead frame and having both surfaces smooth and having a thickness of 0.2 mm was prepared.

[0045] A first plating resist mask having openings corresponding to the connection plating layer is formed on a plate-like copper material in the form of a lead frame, and nickel plating, palladium plating, and gold plating are plated in this order to form the connection plating layer.

[0046] The first plating resist mask is peeled off, and then a second plating resist mask with an opening of 20 μm wide is formed on one side around the formed connection plating layer, and a silver plating layer is formed on the plate-shaped copper material until the upper surface and side surfaces of the previously formed connection plating layer and a 20 μm area around the connection plating layer, and the second plating resist mask is peeled off.

[0047] Next, an etching resist mask having openings in a predetermined lead frame shape is formed on the plate-shaped copper material on which the silver plating layer is formed, and etching is performed to form the lead frame shape.

[0048] Next, the etching resist mask is removed, and the surface of the plate-shaped copper material formed into the shape of a lead frame is washed with an alkaline solution in order to promote the growth of the anodized film.

[0049] Next, a plate-shaped copper material formed into a lead frame shape is immersed in a blackening treatment solution as an anode to form an anodic oxide film having a surface area ratio of 1.7 to 2.3 on the surface of the plate-shaped copper material without a silver plating layer.

[0050] Then, the silver plating layer is peeled off to obtain a lead frame having a connection plating layer at a portion where connection is required, a portion where a smooth surface of the copper material is exposed in a ring shape around the connection plating layer, and an anodized film of the copper material at other portions.

[0051] It should be noted that in the formation of the anodic oxide film using the blackening treatment solution, if it is formed at a high current density, it becomes a short needle-shaped crystal with a surface area ratio of less than 1.5, but if it is formed at a low current density, it becomes an oxide film with a mixture of long needle-shaped crystals and short needle-shaped crystals, and the surface area ratio becomes 1.7 or more. 2 The anodic oxide film was formed at the following current density.

[0052] In the first trial production, it was confirmed that a lead frame can be obtained that can prevent the solvent component contained in the die attach material from spreading to the roughened surface on which the anodic oxide film is formed due to the capillary phenomenon without providing a roughening mitigation region.

[0053] However, it is necessary to separately form the first plating resist mask and the second plating resist mask. It was found that when the step of forming the second plating resist mask is added, the manufacturing cost increases, and it is difficult to apply to mass production.

[0054] Therefore, the inventors of the present application studied a measure for forming a silver plated layer in a large area around the entire periphery of the connecting plated layer without forming a plating resist mask twice.

[0055] In the course of research, the inventors of the present application and others focused on the fact that a conventional high-cyanide silver plating bath is prone to deteriorate the resist mask and is not suitable for partial plating. They believed that by utilizing the property that a high-cyanide silver plating bath is prone to deteriorate the resist mask during partial plating, it might be possible to allow the silver plating solution to penetrate into the interface between the plating resist mask and the connection plating layer and the interface between the plating resist mask and the plate-shaped copper material surrounding the connection plating layer.

[0056] Moreover, it is believed that if the silver plating solution penetrates between the side of the connecting plating layer and the side of the resist mask, and further penetrates under the resist mask, the copper material around the connecting plating layer can be covered by partial (local) silver plating, so that the copper ions dissolved in the blackening treatment solution during the formation of the anodized film can be prevented from contaminating the connecting plating layer and causing discoloration, and a lead frame can be obtained that can prevent the solvent components contained in the chip mounting material from expanding to the roughened surface of the anodized film due to the capillary phenomenon.

[0057] (Second trial production)

[0058] Therefore, as the second trial, the inventors of the present application prepared the same plate-shaped copper material as the first trial, formed the same first plating resist mask on the plate-shaped copper material, plated in the order of a nickel plating layer, a palladium plating layer, and a gold plating layer, and after forming the connection plating layer, the first resist mask was not peeled off, and a silver plating layer was formed using a high cyanide silver plating bath. After the silver plating layer was formed, a lead frame shape was formed in the same manner as the first trial, an anodized film was formed, and the silver plating layer was peeled off to obtain a lead frame.

[0059] The lead frame produced by the second trial production has a connection plating layer at the part to be connected, and the smooth surface of the copper material is exposed in a ring shape around the connection plating layer, and the other parts are formed with an anodic oxide film of the copper material. In addition, the peripheral part of the connection plating layer is not contaminated by copper ions, and no discoloration is observed.

[0060] As a result, the inventors of the present application have obtained the following conclusive evidence: if the resist mask used for forming the connecting plating layer is directly used and a high-cyanide silver plating bath is used to form a silver-plated layer, then a plating layer lower than the silver-plated layer can be formed using the same plating resist mask, and the silver-plated layer can be formed in a wider range than the connecting plating layer.

[0061] This is considered to be a phenomenon in which the silver plating solution penetrates into the interface between the plating resist mask and the connecting plated layer and the interface between the plating resist mask and the plate-shaped copper material around the connecting plated layer to form a silver plating layer.

[0062] In addition, in the second trial production, the silver plated layer was formed to have a thickness of 1 μm. The thickness of the resist mask was 25 μm.

[0063] Furthermore, the copper material exposed around the connection plating layer has a width of approximately 5 to 20 μm, and the smooth surface is exposed in a ring shape.

[0064] As a result of such repeated experiments, the inventors of the present application have been able to confirm that a lead frame can be obtained that does not have a roughening relief area and does not use a second plating resist mask, thereby preventing the discoloration of the connection plating layer set at the part to be connected due to copper ion contamination of the peripheral portion, and can prevent the solvent components contained in the chip mounting material used when connecting the semiconductor element from expanding to the roughened surface of the anodized film due to capillary phenomenon, thereby deriving the lead frame and its manufacturing method of the present invention.

[0065] The lead frame of the present invention is a lead frame formed using a plate-like copper material having at least one side thereof constituted by a smooth surface, and a portion on the side of the plate-like copper material constituted by a smooth surface where connection is performed in order to achieve connection and conduction of a semiconductor element is provided with a predetermined connection plating layer, and a portion around the connection plating layer where the smooth surface of the copper material is exposed in a ring shape, and an anodized film of the copper material is provided at other portions.

[0066] If, as in the lead frame of the present invention, the portion where the smooth surface of the copper material is exposed in a ring shape is provided around the prescribed connection plating layer provided at the portion for connection and conduction of the semiconductor element, and the other portions are provided with an anodic oxide film of the copper material, the solvent components contained in the chip attaching material used for connecting the connection plating layer and the semiconductor element can be prevented from entering the smooth surface between the connection plating layer and the anodic oxide film due to the capillary phenomenon of the anodic oxide film. Therefore, the adhesion with the sealing resin when performing resin sealing to manufacture the semiconductor package can be made excellent.

[0067] In addition, if, as in the lead frame of the present invention, a portion where the smooth surface of the copper material is exposed in a ring shape around a prescribed connection plating layer provided at a portion for connection and conduction of a semiconductor element is provided, the smooth surface of the plate-shaped copper material used for manufacturing the lead frame can be directly used, and there is no need for a pressing process using a mold to form a roughening relief area after forming a roughened surface as in Patent Document 2. Accordingly, the manufacturing process can be reduced, the manufacturing efficiency can be improved, and no manufacturing equipment is required, which can reduce costs.

[0068] Furthermore, in the lead frame of the present invention, it is preferred that the surface area ratio of the smooth surface of the copper material is 1.0 to 1.3, and the surface area ratio of the anodized film is 1.7 to 2.3.

[0069] According to this structure, the sealing resin has excellent adhesion and can prevent the solvent component contained in the die attach material used for connecting the semiconductor element from spreading to the anodized film.

[0070] In the lead frame of the present invention, it is preferable that the connection plating layer includes a plating layer formed by laminating a nickel plating layer, a palladium plating layer, and a gold plating layer in this order on the plate-like copper material.

[0071] According to this structure, it is possible to realize the lead frame of the present invention in which both the connection plating layer and the copper material for electrical connection are exposed at a portion where solder bonding is performed for connecting a semiconductor element, and the other surfaces are provided with an anodic oxide film.

[0072] In addition, the manufacturing method of the lead frame of the present invention includes the following steps: a step of preparing a plate-shaped copper material having at least one side thereof constituted by a smooth surface with a surface area ratio of 1.0 to 1.3; a step of forming a plating resist mask having an opening corresponding to a portion to be connected in order to connect and conduct a semiconductor element on one side of the plate-shaped copper material constituted by the smooth surface in the form of a lead frame; a step of forming a predetermined connection plating layer on the plate-shaped copper material exposed from the opening of the plating resist mask; a step of using a silver plating bath having a characteristic of penetrating to the interface between the plating resist mask and the connection plating layer and the interface between the plate-shaped copper material around the plating resist mask and the connection plating layer to form a silver plating layer covering the connection plating layer; The invention relates to a process for forming a silver-plated layer of the plate-shaped copper material under the plating resist mask which covers the upper surface and side surfaces of the coating and the surrounding of the connecting plating layer; a process for removing the plating resist mask; a process for forming the plate-shaped copper material with the silver-plated layer into the shape of the lead frame; a process for immersing the plate-shaped copper material formed into the shape of the lead frame in an alkaline solution to remove the oxide film on the surface; a process for immersing the plate-shaped copper material with the oxide film removed as an anode in a blackening treatment solution to form an anodic oxide film with a surface area ratio of 1.7 to 2.3 on the portion of the plate-shaped copper material not covered by the silver-plated layer; and a process for peeling off the silver-plated layer to expose the smooth surface of the copper material in a ring shape around the connecting plating layer.

[0073] If it is constituted in this way, there is no roughening relaxation area like the technology described in Patent Document 2, and the smooth surface of the copper material is exposed in a ring shape around the connection plating layer provided at the position where the connection is required to be connected and conduction is achieved for the semiconductor element, and the anodic oxide film of the copper material can be formed at other positions, and the discoloration caused by copper ion contamination of the peripheral portion of the connection plating layer can be prevented. Furthermore, in the manufacturing process, when forming the connection plating layer and the silver plating layer, it is not necessary to form a plating resist mask separately, and the same plating resist mask can be used for both.

[0074] Therefore, a lead frame suitable for welding at connection locations for connection and conduction of semiconductor elements and connection using chip mounting materials can be obtained, which has excellent adhesion with sealing resin when resin sealing is performed to manufacture semiconductor packages and can be manufactured efficiently and at a reduced cost.

[0075] In the lead frame manufacturing method of the present invention, it is preferred to use 1.5 A / dm 2 The above-mentioned anodic oxide film is formed at the following low current density.

[0076] If constructed in this way, an oxide film is formed in which long needle-shaped crystals and short needle-shaped crystals are mixed, and an anodized film having a surface area ratio of 1.7 or more is obtained. The anodized film does not peel off, and the adhesion with the sealing resin can be improved.

[0077] Furthermore, in the method for manufacturing a lead frame of the present invention, it is preferable that the silver plating bath is a high cyanide bath.

[0078] According to this structure, a silver plating bath having the property of penetrating into the interface between the plating resist mask and the connecting plating layer and the interface between the plating resist mask and the plate-shaped copper material around the connecting plating layer can be realized in the lead frame manufacturing method of the present invention.

[0079] Furthermore, in the lead frame manufacturing method of the present invention, it is preferable that the connection plating layer is formed by laminating a nickel plating layer, a palladium plating layer, and a gold plating layer in this order on the plate-like copper material.

[0080] According to this structure, it is possible to realize the method for manufacturing a lead frame of the present invention in which both the connection plating layer and the copper material are exposed at the portion where solder bonding is performed and the portion where the semiconductor element is mounted, and the other surfaces are provided with an anodic oxide film.

[0081] Therefore, according to the present invention, a lead frame and a method for manufacturing the lead frame can be obtained. The lead frame does not have a roughening relaxation area, is suitable for welding of connection parts for connecting and conducting semiconductor elements, and is suitable for connection using chip mounting materials. When resin sealing is performed to manufacture semiconductor packages, the lead frame has excellent adhesion with the sealing resin and can be manufactured efficiently and at a reduced cost.

[0082] Furthermore, it is preferable to perform soft etching before forming the connecting plating layer and to perform etching to a depth of less than 5 μm because this facilitates solder retention during solder reflow.

[0083] Hereinafter, embodiments of the present invention will be described with reference to the drawings.

[0084] The lead frame involved in this embodiment is a lead frame formed using a plate-shaped copper material having at least one side thereof formed of a smooth surface. A predetermined connection plating layer is provided at a portion of the plate-shaped copper material formed of a smooth surface for connection and conduction of a semiconductor element, and a portion where the smooth surface of the copper material is exposed in a ring shape is provided around the connection plating layer. In addition, an anodic oxide film of the copper material is provided at other portions.

[0085] It can be applied to lead frames having various shapes. The shape of the lead frame is not particularly limited. For convenience, Figure 1 , Figure 2 A lead frame of the shape shown is described as an example.

[0086] Figure 1 , Figure 2 In the lead frame 1 shown, a plate-shaped copper material 10 formed of copper or copper alloy as a strip metal material and having smooth surfaces on both sides is formed into a predetermined shape by etching and pressing, and a connection plating layer 11 formed by stacking a nickel plating layer, a palladium plating layer, and a gold plating layer in this order is formed at a portion on the upper surface side of the lead frame substrate electrically connected to a semiconductor element and a portion on the lower surface side connected to an external device. There is a portion 10a where the smooth surface of the copper material is exposed in a ring shape around the connection plating layer 11. In addition, an anodic oxide film 13 of the copper material is formed at other portions of the connection plating layer 11 and the portion 10a where the smooth surface of the copper material is exposed in a ring shape. The anodic oxide film 13 is formed of a single-layer film in which cuprous oxide (Cu2O), copper oxide (CuO), and copper hydroxide (Cu(OH)2) are mixed, and the single-layer film is composed of a film of copper oxide having a needle-shaped crystal structure with an average length of more than 200nm.

[0087] Next, about how Figure 1 , Figure 2 The lead frame manufacturing method of the present embodiment thus constructed uses Figure 3 In addition, Figure 3 In , for convenience, a local graph is used.

[0088] In the manufacturing method of this embodiment, first, a plate-shaped copper material 10 is prepared as a lead frame material (see FIG. 1 ) which is formed of copper or a copper alloy as a strip-shaped metal material and has both sides formed of smooth surfaces with a surface area ratio of 1.0 to 1.3. Figure 3 (a)).

[0089] Next, a resist layer R1 such as a dry film resist is formed on both surfaces of the plate-like copper material 10 (see Figure 3 (b)).

[0090] Next, the resist layers R1 on both sides are exposed and developed using a glass mask to form a plating resist mask 30 (see Figure 3 (c)) In the glass mask, the resist layer R1 on the upper surface side is depicted with a pattern corresponding to an opening portion corresponding to a portion electrically connected to an electrode of a semiconductor element in a flip-chip installation, and the resist layer R1 on the lower surface side is depicted with a pattern corresponding to an opening portion corresponding to a portion electrically connected to an external device.

[0091] Next, a connecting plating layer 11 (see FIG. 1 ) formed by stacking a nickel plating layer, a palladium plating layer, and a gold plating layer in this order is formed on the surface of the plate-shaped copper material 10 exposed from the opening of the plating resist mask 30 in the plate-shaped copper material 10. Figure 3 (d) Figure 3(d')).

[0092] Next, a silver plating bath (e.g., a high cyanide plating bath) having a property of penetrating to the interface between the plating resist mask 30 and the connecting plating layer 11 and the interface between the plating resist mask 30 and the plate-shaped copper material 10 around the connecting plating layer 11 is used to form a silver plating layer 12 of the plate-shaped copper material below the plating resist mask 30 that covers the upper surface and side surfaces of the connecting plating layer 11 and the surrounding of the connecting plating layer 11 (see Figure 3 (e) Figure 3 (e')).

[0093] Next, the plating resist mask 30 (see Figure 3 (f)).

[0094] Next, a resist layer R2 (see FIG. 1 ) such as a dry film resist is formed on both surfaces of the plate-shaped copper material 10 on which the connection plating layer 11 and the silver plating layer 12 are formed. Figure 3 (g)).

[0095] Next, the resist layer R2 on both sides is exposed and developed using a glass mask having a pattern of a predetermined lead frame shape, thereby forming an etching resist mask 31 (see FIG. Figure 3 (h)).

[0096] Next, etching is performed using an etching solution to form the plate-shaped copper material 10 partially provided with the silver-plated layer 12 into a predetermined lead frame shape (see FIG. Figure 3 (i)).

[0097] Next, the etching resist mask 31 (see Figure 3 (j)).

[0098] Thus, on the upper surface side of the plate-like copper material 10, a connection plating layer 11 is formed at a portion electrically connected to the electrode of the semiconductor element, and a silver-plated layer 12 is formed on the upper surface and side surfaces of the connection plating layer 11 and around the connection plating layer 11. On the lower surface side, a connection plating layer 11 is formed at a portion electrically connected to an external device, and a silver-plated layer 12 is formed on the upper surface and side surfaces of the connection plating layer 11 and around the connection plating layer 11, and the other portions have smooth surfaces exposed over the entire surface.

[0099] Next, a plate-shaped copper material (lead frame base material) 10 partially formed with a silver-plated layer 12 is immersed in a blackening treatment solution, and a metal plate is energized in the lead frame base material 10 as an anode, thereby forming an anodic oxide film 13 having a surface area ratio of 1.7 to 2.3 (see FIG. 1 ) on the entire surface of the lead frame base material 10 excluding the portion where the silver-plated layer 12 is formed covering the connection plating layer 11. Figure 3 (k) Figure 3 (k')).

[0100] Next, the silver plating layer 12 is peeled off, and the smooth surface of the copper material 10 is exposed in a ring shape around the connecting plating layer 11 (see Figure 3 (l) Figure 3 (l')).

[0101] Thus, we obtain Figure 1 , Figure 2 The lead frame shown has a connection plating layer 11 at a portion 10 for connection to achieve connection and conduction of semiconductor elements, and has a portion 10a where a smooth surface of copper material is exposed in a ring shape around the portion having the connection plating layer 11, and an anodized film 13 is formed on the entire surface.

[0102] In addition, in the lead frame of this embodiment, in addition to Figure 1 , Figure 2 In addition to the lead frame 1 for flip chip mounting shown, for example, Figure 4 As shown, the lead frame 1 for wire bonding connection can also be applied. Figure 4 In the lead frame 1 shown, a connection plating layer 11 formed by stacking a nickel plating layer, a palladium plating layer, and a gold plating layer in this order is formed at a portion connected to a semiconductor element via a chip mounting material through a pad portion located at the center of the upper surface side of the lead frame substrate, a portion electrically connected to an electrode of the semiconductor element by wire bonding as a lead portion located around the pad portion, and a portion connected to an external device on the lower surface side. Furthermore, around the connection plating layer 11 in the pad portion, there is a portion 10a where the smooth surface of the copper material is exposed in a ring shape. In addition, an anodized film 13 of copper material is formed on the connection plating layer 11 on the upper surface side of the pad portion, other portions of the portion 10a where the smooth surface of the copper material is exposed in a ring shape, and the entire back side of the pad portion. Other structures and Figure 1 , Figure 2 The lead frame 1 shown for flip-chip mounting is substantially the same.

[0103] According to the lead frame 1 of the present embodiment, since the connection-use plating layer 11 is provided at the portion for connection and conduction of the semiconductor element, and the portion 10a where the smooth surface of the copper material 10 is exposed in a ring shape is provided around the portion provided with the connection-use plating layer 11, and the other portions are provided with the anodized film 13 of the copper material 10, the smooth surface between the connection-use plating layer 11 and the anodized film 13 can improve the bonding strength of the solder used when electrically connecting to the connection-use plating layer 11, and prevent the solvent components contained in the chip attaching material used for mounting the semiconductor element from entering due to the capillary phenomenon of the anodized film 13. Therefore, the adhesion with the sealing resin when performing resin sealing to manufacture the semiconductor package can be made excellent.

[0104] In addition, according to the lead frame 1 of the present embodiment, since the smooth surface of the copper material 10 is exposed in a ring shape around the portion having the connection plating layer 11 provided at the portion for connection and conduction of the semiconductor element, the smooth surface of the plate-shaped copper material 10 used for manufacturing the lead frame can be directly used, and the pressing process of forming a roughening relief area using a mold after forming a roughened surface as in Patent Document 2 becomes unnecessary. Therefore, the manufacturing process can be reduced, the manufacturing efficiency can be improved, and the manufacturing equipment is not necessary, which can reduce the cost.

[0105] In addition, according to the lead frame 1 of the present embodiment, since the surface area ratio of the smooth surface of the copper material 10 is 1.0 to 1.3 and the surface area ratio of the anodized film 13 is 1.7 to 2.3, the sealing resin has excellent adhesion, and can improve the bonding strength of the solder used in the electrically connected parts, preventing the solvent components contained in the chip mounting material used for mounting the semiconductor element from spreading to the anodized film.

[0106] In addition, according to the lead frame 1 of the present embodiment, since the connection plating layer 11 is a plating layer formed by stacking a nickel plating layer, a palladium plating layer, and a gold plating layer in this order on the plate-shaped copper material 10, it is possible to realize a lead frame in which both the connection plating layer and the copper material are exposed at the location where solder bonding or bonding using a chip mounting material is performed, and the other surfaces have an anodized film.

[0107] In addition, according to the manufacturing method of the lead frame 1 of the present embodiment, since it is a structure including the following steps, it does not have a roughening relaxation area like the technology described in Patent Document 2, and can prevent the discoloration caused by the contamination of the peripheral portion of the connection plating layer provided at the portion to be connected by copper ions. The steps are: a step of preparing a plate-shaped copper material 10 having smooth surfaces with a surface area ratio of 1.0 to 1.3 on both sides; a step of forming a plating resist mask 30 with an opening corresponding to the portion of electrical connection on the smooth surface of the plate-shaped copper material 10 in the form of a lead frame; a step of forming a connection plating layer 11 on the plate-shaped copper material 10 exposed from the opening of the plating resist mask 30; a step of using a plate-shaped copper material having a surface area that penetrates to the interface between the plating resist mask 30 and the connection plating layer 11 and around the plating resist mask 30 and the connection plating layer 11 The present invention relates to a process for forming a silver-plated layer 12 of a plate-shaped copper material 10 under a plating resist mask 30 covering the upper surface and side surfaces of a connecting plating layer 11 and covering the periphery of the connecting plating layer 11 by using a high cyanide silver plating bath having the characteristics of the interface of the connecting plate 10; a process for removing the plating resist mask 30; a process for forming the plate-shaped copper material 10 with the silver-plated layer 12 formed thereon into a lead frame shape; a process for immersing the plate-shaped copper material 10 formed into a lead frame shape in an alkaline solution to remove the oxide film on the surface; a process for immersing the plate-shaped copper material 10 formed into a lead frame shape from which the oxide film has been removed as an anode in a blackening treatment solution to form an anodic oxide film 13 with a surface area ratio of 1.7 to 2.3 on a portion of the plate-shaped copper material 10 formed into a lead frame shape that is not covered by the silver-plated layer 12; a process for stripping the silver-plated layer 12 to expose the smooth surface of the copper material 10 in a ring shape around the connecting plating layer 11. Furthermore, in the manufacturing process, it is not necessary to form separate plating resist masks in forming the connection plating layer and forming the silver plating layer, and the same plating resist mask can be used for both.

[0108] Therefore, it is possible to obtain a lead frame which is suitable for soldering or connection with a die attach material, has excellent adhesion with a sealing resin when resin sealing is performed to manufacture a semiconductor package, and can be manufactured efficiently and at a reduced cost.

[0109] Furthermore, according to the method for manufacturing the lead frame 1 of the present embodiment, since the current is 1.5 A / dm 2 The following low current density forms a structure similar to the above-mentioned anodized film, thereby becoming an oxide film in which long needle-shaped crystals and short needle-shaped crystals are mixed together, and an anodized film with a surface area ratio of more than 1.7 can be obtained. The anodized film does not peel off and can improve the closeness with the sealing resin.

[0110] Furthermore, according to the method for manufacturing the lead frame 1 of the present embodiment, since a high cyanide bath is used as the silver plating bath, a silver plating bath having the property of penetrating to the interface between the plating resist mask 30 and the connecting plating layer 11 and the interface between the plating resist mask 30 and the plate-shaped copper material 10 around the connecting plating layer 11 can be realized.

[0111] In addition, according to the manufacturing method of the lead frame 1 of the present embodiment, since a connection plating layer 11 is formed by stacking a nickel plating layer, a palladium plating layer, and a gold plating layer in this order on a plate-shaped copper material 10, it is possible to realize a method for manufacturing a lead frame in which both the connection plating layer and the copper material for electrical connection are exposed at a location where semiconductor elements are connected or soldered, and the other surfaces have an anodized film.

[0112] Therefore, according to the present embodiment, a lead frame and a method for manufacturing the lead frame can be obtained which do not have a roughening relief area, are suitable for welding of connection portions for achieving connection and conduction of semiconductor elements, and for connection using chip mounting materials, have excellent adhesion to the sealing resin when resin sealing is performed to manufacture a semiconductor package, and can be manufactured efficiently and at a reduced cost.

[0113] Example 1

[0114] As the metal plate for the lead frame, a copper material with a thickness of 0.2 mm (Furukawa Electric Co., Ltd.: EFTEC64T) was prepared. The surface area ratio of the metal plate was 1.1. (Olympus short-wavelength laser microscope OLS-4100)

[0115] A dry film resist having a thickness of 25 μm was laminated on the surface of the prepared metal plate to form a resist layer.

[0116] Next, the resist layers on both sides are exposed and developed using a glass mask to form a plating resist mask in which approximately 100 mm thick of a portion corresponding to a portion electrically connected to an electrode of a semiconductor element is depicted on the resist layer on the upper surface side. The resist layer on the lower surface side has a pattern corresponding to the opening of the lower surface side, and a portion corresponding to the portion electrically connected to the external device is depicted. The pattern corresponding to the opening of .

[0117] Next, a nickel plating layer with a thickness of 1 μm is first formed on the metal plate exposed from the opening of the plating resist mask, a palladium plating layer with a thickness of about 0.03 μm is formed thereon, and finally a gold plating layer with a thickness of about 0.003 μm is formed, thereby forming a connection plating layer required for electrical connection.

[0118] Next, a silver plating layer of about 1 μm was formed by electroplating on the metal plate exposed from the opening of the plating resist mask using a high cyanide silver plating bath containing silver cyanide and potassium cyanide as main components, and the plating resist mask was removed.

[0119] Next, the same dry film resist is laminated on both surfaces of the metal plate having the silver-plated layer formed thereon to form a resist layer.

[0120] Next, the resist layers on both sides are exposed and developed using a glass mask on which a pattern of a predetermined lead frame shape is drawn, thereby forming an etching resist mask.

[0121] Next, the metal plate partially provided with the silver plating layer is formed into a predetermined lead frame shape by jet etching using a ferric chloride solution, and the etching resist mask is removed.

[0122] Next, the metal plate formed into a predetermined lead frame shape was immersed in a commercially available blackening treatment liquid as an alkaline solution at a concentration of 90 ml / l, a liquid temperature of room temperature, and a treatment time of 60 seconds.

[0123] Next, the same commercially available blackening treatment solution was used at a concentration of 90 ml / l, a liquid temperature of 70°C, a treatment time of 2.5 minutes, and a current density of 0.5 A / dm 2 Under the setting of , the metal plate is used as the anode and an anodic oxide film is formed on the entire surface by immersion treatment.

[0124] Next, the silver-plated layer contaminated by copper ions in the blackening treatment solution was stripped using a commercially available stripping solution.

[0125] The silver-plated layer is peeled off, and a nickel-plated layer, a palladium-plated layer and a gold-plated layer are stacked as connecting plating layers to obtain a lead frame in which the metal plate is exposed in an area of ​​approximately 5 to 20 μm around it and an anodized film is formed on the entire surface of the other metal plate formed into a specified lead frame shape.

[0126] The surface area ratio of the formed anodic oxide film was 1.7 to 2.3. In addition, it was confirmed that no discoloration due to contamination by copper ions in the blackening treatment liquid used for the treatment of forming the anodic oxide film was observed at the peripheral edge of the connecting plating layer, and the product was of good quality.

[0127] In addition, it is considered that the current density for forming the anodic oxide film used in Example 1 is 0.3 to 1.5 A / dm 2 The appropriate immersion time is 1 to 5 minutes.

[0128] Comparative Example 1

[0129] A lead frame of Comparative Example 1 was obtained by the same materials and manufacturing steps as those of Example 1, except that the plating bath used for forming the silver plating layer was changed to a low-cyanide silver plating bath.

[0130] It was confirmed that the lead frame of Comparative Example 1 was discolored due to contamination of the peripheral edge of the connecting plating layer by the blackening treatment liquid, and was not suitable as a product.

[0131] It is also found that the anodic oxide film is formed close to the connecting plating layer, and that no portion where the smooth surface of the metal plate is exposed is formed around the connecting plating layer, as in the lead frame of Example 1, which is not suitable for soldering or mounting of semiconductor elements.

[0132] Industrial Availability

[0133] The lead frame of the present invention is useful in the field of lead frames used in semiconductor manufacturing that need to be sealed with a sealing resin. In addition to lead frames that are composed of a plating layer at the connection site for connecting and conducting semiconductor elements, it is also useful for lead frames in which a metal plate such as a copper plate directly forms an electrical connection site.

Claims

1. A lead frame, characterized in that: The lead frame is formed using a plate-shaped copper material having at least one side thereof constituted by a smooth surface, and has a predetermined connection plating layer at a portion on one side of the plate-shaped copper material constituted by a smooth surface for connection and conduction of a semiconductor element, and has a portion around the connection plating layer where the smooth surface of the copper material is exposed in a ring shape, and has an anodic oxide film of the copper material at other portions.

2. The lead frame according to claim 1, characterized in that The surface area ratio of the smooth surface of the copper material is 1.0 to 1.3, and the surface area ratio of the anodized film is 1.7 to 2.

3.

3. The lead frame according to claim 1 or 2, characterized in that: The connection plating layer includes a plating layer formed by laminating a nickel plating layer, a palladium plating layer, and a gold plating layer in this order on the plate-shaped copper material.

4. A method for manufacturing a lead frame, characterized in that: The process includes the following steps: A step of preparing a plate-shaped copper material, wherein at least one side of the plate-shaped copper material is a smooth surface having a surface area ratio of 1.0 to 1.3; A step of forming a plating resist mask in the form of a lead frame on one side of the plate-like copper material consisting of a smooth surface, wherein the plating resist mask has openings at locations corresponding to locations to be connected in order to achieve connection and conduction of the semiconductor element; a step of forming a predetermined connection plating layer on the plate-shaped copper material exposed from the opening of the plating resist mask; A step of forming a silver-plated layer using a silver-plating bath, wherein the silver-plating bath has a property of penetrating to an interface between the plating resist mask and the connecting plating layer and an interface between the plating resist mask and the plate-shaped copper material around the connecting plating layer, wherein the silver-plated layer covers the upper surface and side surfaces of the connecting plating layer and covers the plate-shaped copper material below the plating resist mask around the connecting plating layer; A step of removing the plating resist mask; The step of forming the plate-shaped copper material having the silver-plated layer formed thereon into the shape of the lead frame; The step of immersing the plate-shaped copper material formed into the lead frame shape in an alkaline solution to remove an oxide film on the surface; The step of immersing the plate-shaped copper material from which the oxide film has been removed as an anode in a blackening treatment solution to form an anodic oxide film having a surface area ratio of 1.7 to 2.3 on a portion of the plate-shaped copper material not covered by the silver plating layer; as well as A step of peeling off the silver plating layer to expose the smooth surface of the copper material in a ring shape around the connection plating layer.

5. The method for manufacturing a lead frame according to claim 4, characterized in that: At 1.5A / dm 2 The anodic oxide film is formed at a low current density below.

6. The method for manufacturing a lead frame according to claim 4, characterized in that: The silver plating bath is a high cyanide bath.

7. The method for manufacturing a lead frame according to claim 4, characterized in that: The connection plating layer is formed by laminating a nickel plating layer, a palladium plating layer, and a gold plating layer in this order on the plate-shaped copper material.