Solar cell and preparation method thereof

By forming a metal silicon compound alloy layer in a solar cell and forming ohmic contact with the electrode, the problem of insufficient contact effect between the back electrode and the polysilicon layer is solved, the filling factor and battery efficiency are improved, and the overall performance is improved.

CN118943244AActive Publication Date: 2024-11-12TRINA SOLAR CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411024573.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The existing TOPcon solar cells have insufficient ohmic contact effect between the back electrode and the polysilicon layer, resulting in low filling factor, which limits the improvement of battery efficiency.

Method used

In the preparation method of solar cells, an electron transport layer is formed and annealed, so that it reacts with the polysilicon layer to form a metal silicon compound alloy layer, the electrode and the alloy layer form ohmic contact, and the metal silicide alloy layer is used to reduce the polysilicon layer and the electrode. and the contact resistance between the two contact resistance and nitrogen impurities improve passivation performance and open circuit voltage.

Benefits of technology

The filling factor and efficiency of solar cells are improved, the passivation effect of the polysilicon layer is enhanced, and the overall performance of the battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943244A_ABST
    Figure CN118943244A_ABST
Patent Text Reader

Abstract

The invention relates to a solar cell, and particularly provides a solar cell and a preparation method thereof, so as to improve the ohmic contact effect of a back electrode and a polycrystalline silicon layer. The preparation method of the solar cell provided by the invention comprises the following steps: providing a cell substrate, wherein the cell substrate comprises a substrate, and a first passivation layer and a polycrystalline silicon layer which are sequentially formed on the first surface of the substrate; forming an electron transport layer on one side, far away from the substrate, of the polycrystalline silicon layer; annealing the electron transport layer to enable the electron transport layer to react with the polycrystalline silicon layer to form a metal silicon compound alloy layer; forming a second passivation layer on one side, far away from the substrate, of the electron transport layer; and forming an electrode which extends from the surface of the second passivation layer to a position between the electron transport layer and the first passivation layer, so that the electrode and the metal silicon compound alloy layer form ohmic contact. The contact resistance between the polycrystalline silicon layer and the electrode can be reduced by using the metal silicide alloy layer, so that the filling factor of the battery is improved, and the efficiency of the battery is finally improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and specifically provides a solar cell and a preparation method thereof. Background Art

[0002] At present, with the continuous consumption of traditional energy, energy issues have become an important issue of global concern, and promoting the development of renewable energy has become the focus. Among them, solar energy has significant advantages such as cleanliness, safety, and abundant resources. It has gradually emerged and become the focus of research and development. After decades of development, photovoltaic power generation technology has also made remarkable progress.

[0003] Among them, TOPcon battery is a kind of solar cell. The efficiency of the battery has exceeded 26%, and it has not yet reached the limit. The efficiency of TOPcon battery (for example, in terms of improving the open circuit voltage and fill factor of the battery) still has huge room for improvement. Among them, the fill factor is the ratio of the product of the current and voltage when the battery has maximum output power to the product of the short-circuit current and open circuit voltage. The physical meaning of the fill factor is the uniformity of the electric field strength in the solar cell, which can also be understood as the magnitude of the resistance to the movement of electrons in the solar cell. The higher the fill factor, the smoother the flow of electrons in the battery, and the more solar energy can be fully converted into electrical energy; conversely, the lower the fill factor, the more resistance there is to the flow of electrons inside the solar cell, and it is impossible to fully utilize solar energy to convert into electrical energy. Therefore, the fill factor can provide the actual performance of the output current and voltage of the solar cell, as well as the conversion efficiency of the solar cell.

[0004] In the TOPcon battery structure, the ohmic contact effect between the back electrode and the polysilicon layer is an important factor affecting the fill factor. The better the ohmic contact effect between the back electrode and the polysilicon layer, the higher the fill factor and the higher the battery efficiency.

[0005] Currently, the polysilicon layer is often heavily doped to enhance the ohmic contact effect between the back electrode and the polysilicon layer. However, the heavily doped polysilicon layer absorbs more sunlight and has more obvious parasitic absorption, which is not conducive to improving battery efficiency.

[0006] Therefore, there is an urgent need for a solar cell and a preparation method thereof to improve the ohmic contact effect between the back electrode and the polysilicon layer. Summary of the invention

[0007] The invention solves the problems existing in the prior art and provides a solar cell and a preparation method thereof.

[0008] In a first aspect, the present invention provides a method for preparing a solar cell, comprising: providing a cell substrate, the cell substrate comprising a substrate and a first passivation layer and a polysilicon layer sequentially formed on a first surface of the substrate; forming an electron transport layer on a side of the polysilicon layer away from the substrate; annealing the electron transport layer so that the electron transport layer reacts with the polysilicon layer to form a metal silicon compound alloy layer; forming a second passivation layer on a side of the electron transport layer away from the substrate; and forming an electrode, the electrode extending from a surface of the second passivation layer to between the electron transport layer and the first passivation layer, so that the electrode forms an ohmic contact with the metal silicon compound alloy layer.

[0009] In a specific embodiment of the method for preparing the solar cell, the material of the electron transport layer is a metal compound, and the metal is at least one of molybdenum, nickel and titanium.

[0010] In a specific embodiment of the method for preparing the solar cell, the material of the electron transport layer is metal nitride.

[0011] In a specific embodiment of the method for preparing the solar cell, the material of the electron transport layer is titanium nitride, the metal silicon compound alloy layer is a titanium silicon alloy layer, and the annealing temperature is 350°C to 950°C.

[0012] In a specific embodiment of the method for preparing the solar cell, the thickness of the electron transport layer is greater than 1 nm.

[0013] In a specific implementation of the method for preparing the solar cell, the orthographic projection of the electrode on the substrate is located within the orthographic projection of the electron transport layer on the substrate.

[0014] In a specific embodiment of the method for preparing the solar cell, the method further comprises: doping the second surface of the substrate to form a doping layer, and sequentially forming a third passivation layer and a fourth passivation layer on the doping layer.

[0015] In a specific embodiment of the above-mentioned method for preparing a solar cell, the polysilicon layer includes a first polysilicon layer of a first doping type and a second polysilicon layer of a second doping type, and the first polysilicon layer and the second polysilicon layer are insulated from each other; the electron transport layer is formed on the first polysilicon layer and the second polysilicon layer.

[0016] In a second aspect, the present disclosure provides a solar cell, comprising: a substrate; a first passivation layer, a polycrystalline silicon layer, a metal silicon compound alloy layer, an electron transport layer, and a second passivation layer arranged in sequence on a first surface of the substrate, the metal silicon compound alloy layer being located within the polycrystalline silicon layer; an electrode, the electrode extending from a surface of the second passivation layer to between the electron transport layer and the first passivation layer, and an ohmic contact being formed between the electrode and the metal silicide.

[0017] In a specific embodiment of the above-mentioned solar cell, the polycrystalline silicon layer and the substrate are of a first doping type, the second surface of the substrate has a doping layer of a second doping type, and a third passivation layer and a fourth passivation layer are sequentially arranged on the side of the doping layer away from the substrate; or, the polycrystalline silicon layer includes a first polycrystalline silicon layer and a second polycrystalline silicon layer insulated from each other, the doping types of the first polycrystalline silicon layer and the second polycrystalline silicon layer are opposite, and the metal silicon compound alloy layer is arranged in the first polycrystalline silicon layer and the second polycrystalline silicon layer.

[0018] In a specific embodiment of the solar cell, the orthographic projection of the electrode on the substrate is located within the orthographic projection of the electron transport layer on the substrate; or, the thickness of the electron transport layer is greater than 1 nm.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The preparation method of the solar cell provided by the present disclosure includes: providing a battery substrate, the battery substrate includes a substrate and a first passivation layer and a polysilicon layer sequentially formed on the first surface of the substrate; forming an electron transport layer on the side of the polysilicon layer away from the substrate; annealing the electron transport layer so that the electron transport layer reacts with the polysilicon layer to form a metal silicon compound alloy layer; forming a second passivation layer on the side of the electron transport layer away from the substrate; forming an electrode, the electrode extends from the surface of the second passivation layer to between the electron transport layer and the first passivation layer, so that the electrode forms an ohmic contact with the metal silicon compound alloy layer. The use of the metal silicide alloy layer can reduce the contact resistance between the polysilicon layer and the electrode, thereby improving the fill factor of the battery and ultimately improving the efficiency of the battery.

[0021] Furthermore, the material of the electron transport layer is metal nitride. During the process of annealing to form metal silicon compounds, the nitrogen atoms in the metal nitride can form nitrogen impurities. The nitrogen atoms in the nitrogen impurities combine with hydrogen atoms to form nitrogen-hydrogen bonds, thereby capturing more hydrogen elements, thereby improving the passivation performance of the battery, and then improving the open circuit voltage of the battery, and ultimately improving the efficiency of the battery; in addition, the nitrogen impurities can also inhibit the diffusion of phosphorus elements in the polysilicon layer, thereby improving the passivation effect of the polysilicon layer, thereby improving the efficiency of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings, in which:

[0023] Figure 1 is a flow chart of a method for preparing a solar cell provided by the present disclosure;

[0024] FIG. 2A to FIG. 2E is a cross-sectional view of the first solar cell disclosed in the present invention during the preparation process;

[0025] Figure 2F is a cross-sectional view of the first solar cell provided by the present disclosure;

[0026] FIG. 3A to FIG. 3E is a cross-sectional view of the second solar cell disclosed in the present invention during the preparation process;

[0027] Figure 3F is a cross-sectional view of a second solar cell provided by the present disclosure;

[0028] Figure 3G is a cross-sectional view of a third solar cell provided by the present disclosure.

[0029] Description of reference numerals:

[0030] 1. substrate; 11. doping layer; 2. first passivation layer; 3. polysilicon layer; 31. first polysilicon layer; 32. second polysilicon layer; 33. isolation region; 34. isolation trench; 4. third passivation layer; 5. fourth passivation layer; 6. second passivation layer; 7. electron transport layer; 8. metal silicon compound alloy layer; 91. first electrode; 92. second electrode. DETAILED DESCRIPTION

[0031] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0032] It should be noted that in the description of the present invention, the terms "upper", "lower", "left", "right", "inner", "outer" and the like indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings, which are only for the convenience of description, and do not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0033] Figure 1 The present invention provides a flow chart of a method for preparing a solar cell.

[0034] like Figure 1As shown, the present disclosure provides a method for preparing a solar cell, comprising: providing a cell substrate, the cell substrate comprising a substrate and a first passivation layer and a polysilicon layer sequentially formed on a first surface of the substrate; forming an electron transport layer on a side of the polysilicon layer away from the substrate; annealing the electron transport layer so that the electron transport layer reacts with the polysilicon layer to form a metal silicon compound alloy layer; forming a second passivation layer on a side of the electron transport layer away from the substrate; forming an electrode, the electrode extending from the surface of the second passivation layer to between the electron transport layer and the first passivation layer, so that the electrode forms an ohmic contact with the metal silicon compound alloy layer.

[0035] Next, the method for preparing the solar cell provided by the embodiment of the present disclosure is introduced.

[0036] Embodiment 1

[0037] FIG. 2A to FIG. 2E is a cross-sectional view of the first solar cell disclosed in the present invention during the preparation process; Figure 2F 1 is a cross-sectional view of the first solar cell provided by the present disclosure. In this embodiment, the solar cell is specifically a TOPcon cell.

[0038] S1, such as Figure 2A As shown, a substrate 1 is provided, wherein the substrate 1 has a first surface and a second surface opposite to the first surface, wherein the first surface is a backlight surface, and the second surface is a frontlight surface.

[0039] The substrate 1 is a semiconductor substrate 1 such as silicon or germanium that is doped. For example, the substrate 1 is an N-type doped silicon substrate, and the corresponding dopant may include any one or more of phosphorus (P), arsenic (As), bismuth (Bi), and antimony (Sb) in the V group. For another example, the substrate 1 is a P-type doped silicon substrate, and the corresponding dopant may include any one or more of boron (B), aluminum (Al), gallium (Ga), and indium (In) in the III group.

[0040] For example, the first surface and the second surface of the substrate 1 are textured; or, the first surface and the second surface of the substrate 1 are textured, and then at least part of the first surface is polished, so that the first surface has a planar structure or a part of it has a planar structure and the other part has a velvet structure. After the second surface is textured, the surface area and surface complexity of the second surface can be increased, thereby reducing the reflection of the incident light, thereby improving the short circuit current interruption of the battery, and then improving the photoelectric conversion efficiency of the battery. After the second surface of the substrate 1 is textured, the film layers formed on the second surface have the same velvet structure as the second surface.

[0041] For example, the substrate 1 is an N-type substrate 1, and the substrate 1 is immersed in a KOH or NaOH solution with a temperature of 60° C. to 80° C. and a mass fraction of 1% to 3% for texturing, and the texturing time is controlled to be 15 minutes to 25 minutes.

[0042] S2. Doping is performed on the second surface of the substrate 1 to form a doping layer 11 of a second doping type on the second surface.

[0043] For example, when the substrate 1 is N-type doped, the doping type of the doping layer 11 is P-type doping, thereby forming a PN junction. As a specific example, the N-type single crystal silicon substrate 1 is placed in a boron diffusion furnace tube for a boron diffusion process, and the process temperature of the boron diffusion is 900° C. to 1100° C. Boron sources such as trimethyl borate, boron tribromide, and boron trichloride can be used for boron diffusion. In the process of forming the boron doping layer 11 (i.e., the doping layer 11) on the second surface, a BSG (borosilicate glass) layer will naturally form under the action of oxygen.

[0044] For example, the doping layer 11 has a thickness of 0.01 μm to 0.02 μm and a sheet resistance of 100 ohm / sq to 180 ohm / sq.

[0045] It should be noted that the present disclosure does not impose specific restrictions on the boron source, process temperature, diffusion depth, etc. of the boron diffusion or phosphorus diffusion process. Personnel in this field can design according to actual needs, and the above limitations are only some specific examples.

[0046] S3. Remove the boron diffusion layer that has expanded on the first surface, while retaining the BSG layer on the second surface.

[0047] S4, forming a first passivation layer 2 and a doped polysilicon layer 3 on the first surface of the substrate 1 in sequence, forming a Figure 2A The structure shown. The first passivation layer 2 can saturate the dangling bonds on the surface of the substrate 1, reduce the interface defect state density on the first surface of the substrate 1, thereby reducing the recombination center on the first surface of the substrate 1, thereby reducing the recombination rate of carriers, and ultimately increasing the open circuit voltage of the solar cell, and improving the photoelectric conversion efficiency of the solar cell. The material of the first passivation layer 2 is a dielectric material, specifically, it can be at least one of silicon oxide, amorphous silicon, polycrystalline silicon, silicon carbide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide. Among them, the first passivation layer 2 can contain doping elements of the same type as the doping elements of the substrate 1.

[0048] The doping type of the polysilicon layer 3 is the same as the doping type of the substrate 1. For example, when the substrate 1 is N-type doped, the doping type of the polysilicon layer 3 is also N-type, and the doping element is phosphorus. In addition, one or more of the three elements of oxygen, carbon and nitrogen can also be doped into the polysilicon layer 3. For example, the thickness of the polysilicon layer 3 is 3nm to 150nm.

[0049] In some examples, the semiconductor structure manufactured by steps S1 to S4 can be used as a battery substrate for performing step S5 and subsequent steps.

[0050] S5. An electron transport layer 7 is formed on the side of the polysilicon layer 3 away from the substrate 1. The material of the electron transport layer 7 is a metal compound (such as a metal oxide or a metal nitride), wherein the metal is at least one of molybdenum, nickel, and titanium. For example, the material of the electron transport layer 7 is any one or more of titanium nitride, titanium oxide, molybdenum nitride, molybdenum oxide, nickel nitride, and nickel oxide.

[0051] In some examples, the electron transport layer 7 is formed on the entire surface of the polysilicon layer 3. In other examples, the electron transport layer 7 is formed only in a partial area on the polysilicon layer 3 after being shielded by a mask, and the area where the electron transport layer 7 is formed corresponds to the back electrode of the battery, such as Figure 2B For example, the electron transport layer 7 is formed by magnetron sputtering.

[0052] S6, such as Figure 2C As shown, the electron transport layer 7 is annealed to react with the polysilicon layer 3 to form a metal silicon compound alloy layer 8. The thickness of the electron transport layer 7 is greater than 1 nm to ensure that the electron transport layer 7 can react with the polysilicon layer 3 to form a metal silicon compound alloy layer 8 of sufficient thickness.

[0053] For example, when the materials of the electron transport layer 7 are metal compounds of molybdenum, nickel, and titanium, respectively, the metal silicon compound alloy layer 8 is a molybdenum silicon alloy layer, a nickel silicon alloy layer, and a titanium silicon alloy layer, respectively.

[0054] In addition, when the electron transport layer 7 is a metal nitride, during the process of annealing to form a metal silicon compound, the nitrogen atoms in the metal nitride can form nitrogen impurities. The nitrogen atoms in the nitrogen impurities combine with hydrogen atoms to form nitrogen-hydrogen bonds, thereby capturing more hydrogen elements, thereby improving the passivation performance of the battery, and then improving the open circuit voltage of the battery, and ultimately improving the efficiency of the battery. In addition, the nitrogen impurities can also inhibit the diffusion of phosphorus elements in the polysilicon layer 3, thereby improving the passivation effect of the polysilicon layer 3, thereby improving the efficiency of the battery.

[0055] As a specific example, the material of the electron transport layer 7 is titanium nitride, and the annealing temperature is 350° C. to 950° C., preferably 400° C. to 900° C., to ensure that the electron transport layer 7 and the polysilicon layer 3 can fully react to form a titanium silicon alloy layer.

[0056] S7, such as Figure 2D As shown, a third passivation layer 4 is formed on a side of the doping layer 11 away from the substrate 1 .

[0057] As a specific example, the material of the third passivation layer 4 is aluminum oxide, which is formed by plasma enhanced chemical vapor deposition. For example, a mixed gas of trimethylaluminum and oxygen or nitrogen oxide (i.e., a mixed gas of trimethylaluminum and oxygen, or a mixed gas of trimethylaluminum and nitrogen oxide) is introduced, and the reaction temperature is between 200° C. and 350° C., thereby forming the third passivation layer 4 of aluminum oxide.

[0058] S8, forming a second passivation layer 6 on the side of the electron transport layer 7 away from the substrate 1, and forming a fourth passivation layer 5 on the side of the third passivation layer 4 away from the substrate 1. Wherein, after the electron transport layer 7 is shielded by a mask, it is only formed in a partial area on the polysilicon layer 3, and the area where the electron transport layer 7 is formed corresponds to the back electrode of the battery, the second passivation layer 6 is specifically located on the electron transport layer 7 and the exposed polysilicon layer 3, such as Figure 2D The second passivation layer 6 and the fourth passivation layer 5 are also called anti-reflection layers, which mainly play the role of reducing the reflection of incident light, thereby improving, and also play a certain passivation effect to improve the open circuit voltage of the battery.

[0059] As a specific example, the material of the second passivation layer 6 and the fourth passivation layer 5 is silicon nitride, and is formed by plasma enhanced chemical vapor deposition. For example, a mixed gas of SiH4 and NH3 is introduced, and the reaction temperature is between 300° C. and 550° C., thereby forming the second passivation layer 6 and the fourth passivation layer 5 of silicon nitride.

[0060] S9, forming a first electrode 91 and a second electrode 92. The first electrode 91 extends from the surface of the fourth passivation layer 5 to the doping layer 11, and the second electrode 92 extends from the surface of the second passivation layer 6 to between the electron transport layer 7 and the first passivation layer 2 (i.e., extending into the metal silicon compound alloy layer 8 or the polysilicon layer 3), so that the second electrode 92 forms an ohmic contact with the metal silicon compound alloy layer 8. The use of the metal silicide alloy layer can reduce the contact resistance between the polysilicon layer 3 and the second electrode 92, thereby improving the fill factor of the battery and ultimately improving the efficiency of the battery.

[0061] The specific process of forming the first electrode 91 and the second electrode 92 includes:

[0062] like Figure 2EAs shown, metal paste is printed on the second passivation layer 6 and the fourth passivation layer 5; the metal paste is sintered, and the metal paste on the second passivation layer 6 corrodes the second passivation layer 6 and the first passivation layer 2 to form an ohmic contact with the doping layer 11, and the metal paste on the fourth passivation layer 5 corrodes the fourth passivation layer 5 and the electron transport layer 7 to form an ohmic contact with the metal silicon compound alloy layer 8. Figure 2F As shown, the metal paste on the second passivation layer 6 forms a first electrode 91 after cooling, and the metal paste on the fourth passivation layer 5 forms a second electrode 92 after cooling.

[0063] In some possible examples, during the sintering process, the metal slurry located on the fourth passivation layer 5 may also corrode part of the metal silicon compound alloy layer 8 and the polysilicon layer 3, and then extend the metal slurry into the polysilicon layer 3, so that the second electrode 92 formed by cooling the metal slurry can form ohmic contact with the metal silicon compound alloy layer 8 and the polysilicon layer 3 at the same time.

[0064] For example, the orthographic projection of the second electrode 92 on the substrate 1 is located within the orthographic projection of the electron transport layer 7 on the substrate 1. When printing the metal paste for forming the second electrode 92, the metal paste is more easily aligned with the electron transport layer 7. In a specific embodiment, the gate line width of the mask used when forming the electron transport layer 7 is greater than the gate line width of the mask used when printing the metal paste for forming the second electrode 92.

[0065] In summary, the solar cell provided by the present disclosure has at least the following advantages:

[0066] (1) An electron transport layer 7 is formed on the polysilicon layer 3, and then the electron transport layer 7 is annealed so that the electron transport layer 7 reacts with the polysilicon layer 3 to form a metal silicon compound alloy layer 8, and then an electrode is formed so that the electrode and the metal silicon compound alloy layer 8 form an ohmic contact; the metal silicide alloy layer can reduce the contact resistance between the polysilicon layer 3 and the second electrode 92, thereby improving the fill factor of the battery and ultimately improving the efficiency of the battery.

[0067] (2) The material of the electron transport layer 7 is metal nitride. During the process of annealing to form a metal silicon compound, the nitrogen atoms in the metal nitride can form nitrogen impurities. The nitrogen atoms in the nitrogen impurities combine with hydrogen atoms to form nitrogen-hydrogen bonds, thereby capturing more hydrogen elements, thereby improving the passivation performance of the battery, and then improving the open circuit voltage of the battery, and ultimately improving the efficiency of the battery; in addition, the nitrogen impurities can also inhibit the diffusion of phosphorus elements in the polycrystalline silicon layer 3, thereby improving the passivation effect of the polycrystalline silicon layer 3, thereby improving the efficiency of the battery.

[0068] like Figure 2FAs shown, the embodiment of the present disclosure further provides a solar cell, including a substrate 1. The substrate 1 has a first surface and a second surface, the first surface is a backlight surface, and the second surface is a light-facing surface.

[0069] The second surface of the substrate 1 has a doping layer 11, and the doping type of the doping layer 11 is opposite to the doping type of the substrate 1. For example, the doping type of the substrate 1 is N-type doping, and the doping type of the doping layer 11 is P-type doping, thereby forming a PN junction.

[0070] The third passivation layer 4 and the fourth passivation layer 5 are sequentially arranged on the side of the doped layer 11 away from the substrate 1. The third passivation layer 4 is mainly used to passivate the doped layer 11. The fourth passivation layer 5 can, on the one hand, enhance the passivation effect of the light-facing side of the battery, and on the other hand, reduce the reflection of incident light, so that more sunlight is absorbed by the solar cell, thereby increasing the short-circuit current of the battery, and also has a certain passivation effect to increase the open-circuit voltage of the battery.

[0071] The first surface of the substrate 1 is provided with a first passivation layer 2 and a polysilicon layer 3 in sequence in a direction away from the substrate 1. The first passivation layer 2 can reduce the recombination rate of carriers, thereby increasing the open circuit voltage of the solar cell and ultimately improving the photoelectric conversion efficiency of the solar cell.

[0072] A metal silicon compound alloy layer 8 and an electron transport layer 7 are provided on the polysilicon layer 3. The material of the electron transport layer 7 is a metal compound (such as a metal oxide or a metal nitride), wherein the metal is at least one of molybdenum, nickel, and titanium. The metal silicon compound alloy layer 8 is formed by the reaction of the metal atoms in the electron transport layer 7 with the polysilicon after annealing.

[0073] A second passivation layer 6 is disposed on the exposed polysilicon layer 3 and the electron transport layer 7 , and the second passivation layer 6 is used to passivate the backlight surface of the battery.

[0074] The solar cell also includes a first electrode 91 and a second electrode 92 insulated from each other. The first electrode 91 extends from the surface of the fourth passivation layer 5 to the doping layer 11, so that an ohmic contact is formed between the first electrode 91 and the doping layer 11. The second electrode 92 extends from the surface of the second passivation layer 6 to between the electron transport layer 7 and the first passivation layer 2 (i.e., extends to the metal silicon compound alloy layer 8 or the polysilicon layer 3), so that the second electrode 92 forms an ohmic contact with the metal silicon compound alloy layer 8. The use of the metal silicide alloy layer can reduce the contact resistance between the polysilicon layer 3 and the second electrode 92, thereby improving the fill factor of the battery and ultimately improving the efficiency of the battery.

[0075] Embodiment 2

[0076] FIG. 3A to FIG. 3E It is a cross-sectional view of the second solar cell disclosed in the present invention during the preparation process. Figure 3Fis a cross-sectional view of a second solar cell provided by the present disclosure. Figure 3G 1 is a cross-sectional view of the third solar cell provided by the present disclosure. The solar cell in this embodiment is specifically a TBC (TOPCon back contact) cell.

[0077] The method for preparing a solar cell provided by the embodiment of the present disclosure is specifically as follows:

[0078] S1, such as Figure 3A As shown, a substrate 1 is provided. The substrate 1 has a first surface and a second surface opposite to the first surface. The first surface of the substrate 1 is a backlight surface, and the second surface of the substrate 1 is a light-facing surface. The doping type of the substrate 1 can be P-type doping or N-type doping.

[0079] S2. Texturing the second surface of the substrate 1 to reduce the reflection of incident light, thereby improving the short circuit current interruption of the battery, and further improving the photoelectric conversion efficiency of the battery. After the second surface of the substrate 1 is texturized, the film layers formed on the second surface all have the same velvet structure as the second surface.

[0080] The first surface of the substrate 1 is also textured or polished.

[0081] S3, sequentially forming a third passivation layer 4 and a fourth passivation layer 5 on the second surface of the substrate 1. For example, the method of forming the third passivation layer 4 and the fourth passivation layer 5 is the same as that of the first embodiment.

[0082] S4, forming a first passivation layer 2 and an intrinsic polysilicon layer 3 on the first surface of the substrate 1 in sequence, forming a Figure 3A The material of the first passivation layer 2 is a dielectric material, specifically at least one of silicon oxide, amorphous silicon, polycrystalline silicon, silicon carbide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide.

[0083] For example, the first passivation layer 2 and the intrinsic polysilicon layer 3 are formed by LPCVD (Low Pressure Chemical Vapor Deposition).

[0084] S5, such as Figure 3B As shown, doping is performed on the intrinsic polysilicon layer 3 to form a first polysilicon layer 31 of a first doping type and a second polysilicon layer 32 of a second doping type. An isolation region 33 is provided between the first polysilicon layer 31 and the second polysilicon layer 32 to ensure electrical insulation between the first polysilicon layer 31 and the second polysilicon layer 32.

[0085] S6, such as Figure 3CAs shown, an electron transport layer 7 is formed on the side of the polysilicon layer 3 away from the substrate 1, wherein the electron transport layer 7 is provided on both the first polysilicon layer 31 and the second polysilicon layer 32. As an example, the electron transport layer 7 is formed only in a partial area on the first polysilicon layer 31 and the second polysilicon layer 32 after being shielded by a mask, and the area where the electron transport layer 7 is formed corresponds to the back electrode of the battery.

[0086] The material of the electron transport layer 7 is a metal compound (such as a metal oxide or a metal nitride), wherein the metal is at least one of molybdenum, nickel, and titanium. For example, the material of the electron transport layer 7 is any one or more of titanium nitride, titanium oxide, molybdenum nitride, molybdenum oxide, nickel nitride, and nickel oxide.

[0087] S7, such as Figure 3D As shown, the electron transport layer 7 is annealed to react with the polysilicon layer 3 to form a metal silicon compound alloy layer 8. The thickness of the electron transport layer 7 is greater than 1 nm to ensure that the electron transport layer 7 can react with the polysilicon layer 3 to form a metal silicon compound alloy layer 8 of sufficient thickness.

[0088] For example, when the materials of the electron transport layer 7 are metal compounds of molybdenum, nickel, and titanium, respectively, the metal silicon compound alloy layer 8 is a molybdenum silicon alloy layer, a nickel silicon alloy layer, and a titanium silicon alloy layer, respectively.

[0089] In addition, when the electron transport layer 7 is a metal nitride, during the process of annealing to form a metal silicon compound, the nitrogen atoms in the metal nitride can form nitrogen impurities. The nitrogen atoms in the nitrogen impurities combine with hydrogen atoms to form nitrogen-hydrogen bonds, thereby capturing more hydrogen elements, thereby improving the passivation performance of the battery, and then improving the open circuit voltage of the battery, and ultimately improving the efficiency of the battery. In addition, the nitrogen impurities can also inhibit the diffusion of phosphorus elements in the polysilicon layer 3, thereby improving the passivation effect of the polysilicon layer 3, thereby improving the efficiency of the battery.

[0090] As a specific example, the material of the electron transport layer 7 is titanium nitride, and the annealing temperature is 350° C. to 950° C., preferably 400° C. to 900° C., to ensure that the electron transport layer 7 and the polysilicon layer 3 can fully react to form a titanium silicon alloy layer.

[0091] S8, such as Figure 3E As shown, a second passivation layer 6 is formed on a side of the electron transport layer 7 away from the substrate 1 . The second passivation layer 6 is specifically located on the electron transport layer 7 and the exposed polysilicon layer 3 .

[0092] S9 . Form the first electrode 91 and the second electrode 92 .

[0093] Among them, Figure 3FAs shown, the first electrode 91 extends from the surface of the second passivation layer 6 to between the electron transport layer 7 and the first passivation layer 2, and the first electrode 91 forms an ohmic contact with the metal silicon compound alloy layer 8 located in the first polysilicon layer 31; the second electrode 92 extends from the surface of the second passivation layer 6 to between the electron transport layer 7 and the first passivation layer 2, and the second electrode 92 forms an ohmic contact with the metal silicon compound alloy layer 8 located in the second polysilicon layer 32. The use of the metal silicide alloy layer can reduce the contact resistance between the first polysilicon layer 31 and the first electrode 91 and the contact resistance between the second polysilicon layer 32 and the second electrode 92, thereby improving the fill factor of the battery and ultimately improving the efficiency of the battery.

[0094] The materials of the first electrode 91 and the second electrode 92 include, but are not limited to, one or more of aluminum, titanium, nickel, cobalt, silver, copper, and tin. The first electrode 91 and the second electrode 92 may be formed by screen printing, laser transfer, and electroplating. In the embodiment of the present application, the first electrode 91 and the second electrode 92 may be understood as metal grid lines, and the width and thickness of the metal grid lines are not limited.

[0095] like Figure 3F As shown, some embodiments of the present disclosure further provide a solar cell, including a substrate 1. The substrate 1 has a first surface and a second surface, the first surface is a backlight surface, and the second surface is a light-facing surface.

[0096] The second surface of the substrate 1 is sequentially provided with a third passivation layer 4 and a fourth passivation layer 5. Sunlight is incident on the substrate 1 from the fourth passivation layer 5 and the third passivation layer 4, and the sunlight reflected by the substrate 1 is reflected by the fourth passivation layer 5 and the third passivation layer 4 and then incident on the substrate 1 again, thereby improving the light absorption efficiency of the solar cell.

[0097] A first passivation layer 2 and a polysilicon layer 3 are sequentially disposed on the first surface of the substrate 1 .

[0098] The first passivation layer 2 can reduce the recombination rate of carriers, thereby increasing the open circuit voltage of the solar cell and ultimately improving the photoelectric conversion efficiency of the solar cell.

[0099] The polysilicon layer 3 includes a first polysilicon layer 31 and a second polysilicon layer 32 insulated from each other. The first polysilicon layer 31 and the second polysilicon layer 32 have opposite doping types, for example, the first polysilicon layer 31 is P-type doped and the second polysilicon layer 32 is N-type doped.

[0100] In some examples, such as Figure 3F As shown, an isolation region 33 is formed between the first polysilicon layer 31 and the second polysilicon layer 32 . The isolation region 33 contains undoped intrinsic polysilicon. The first polysilicon layer 31 and the second polysilicon layer 32 are isolated by the intrinsic polysilicon layer 3 in the isolation region 33 .

[0101] In other examples, such as Figure 3G As shown, an isolation trench 34 is formed between the first polysilicon layer 31 and the second polysilicon layer 32 , and the isolation trench 34 is used to isolate the first polysilicon layer 31 from the second polysilicon layer 32 .

[0102] A metal silicon compound alloy layer 8 and an electron transport layer 7 are disposed on the first polysilicon layer 31 and the second polysilicon layer 32. The material of the electron transport layer 7 is a metal compound (such as a metal oxide or a metal nitride), wherein the metal is at least one of molybdenum, nickel, and titanium. The metal silicon compound alloy layer 8 is generated by the reaction of metal atoms in the electron transport layer 7 with polysilicon after annealing.

[0103] A second passivation layer 6 is disposed on the exposed first polysilicon layer 31 , the exposed second polysilicon layer 32 and the electron transport layer 7 , and the second passivation layer 6 is used to passivate the backlight surface of the battery.

[0104] The solar cell also includes a first electrode 91 and a second electrode 92 insulated from each other. The first electrode 91 extends from the surface of the second passivation layer 6 to between the electron transport layer 7 and the first passivation layer 2, and the first electrode 91 forms an ohmic contact with the metal silicon compound alloy layer 8 located in the first polysilicon layer 31. The second electrode 92 extends from the surface of the second passivation layer 6 to between the electron transport layer 7 and the first passivation layer 2, and the second electrode 92 forms an ohmic contact with the metal silicon compound alloy layer 8 located in the second polysilicon layer 32. The use of the metal silicide alloy layer can reduce the contact resistance between the first polysilicon layer 31 and the first electrode 91 and the contact resistance between the second polysilicon layer 32 and the second electrode 92, thereby improving the fill factor of the battery and ultimately improving the efficiency of the battery.

[0105] There are a few points to note:

[0106] (1) The drawings of the embodiments of the present disclosure only relate to the structures related to the embodiments of the present disclosure, and other structures may refer to the general design.

[0107] (2) For the sake of clarity, in the drawings used to describe the embodiments of the present disclosure, the thickness of layers or regions is enlarged or reduced, that is, these drawings are not drawn according to the actual scale.

[0108] (3) In the absence of conflict, the embodiments of the present disclosure and the features therein may be combined with each other to obtain new embodiments.

[0109] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. A method for preparing a solar cell, characterized in that: include: Providing a battery substrate, the battery substrate comprising a substrate, and a first passivation layer and a polysilicon layer sequentially formed on a first surface of the substrate; forming an electron transport layer on a side of the polysilicon layer away from the substrate; Annealing the electron transport layer to allow the electron transport layer to react with the polysilicon layer to form a metal silicon compound alloy layer; forming a second passivation layer on a side of the electron transport layer away from the substrate; An electrode is formed, wherein the electrode extends from a surface of the second passivation layer to between the electron transport layer and the first passivation layer, so that the electrode forms an ohmic contact with the metal silicon compound alloy layer.

2. The method for preparing a solar cell according to claim 1, characterized in that: The material of the electron transport layer is a metal compound, and the metal is at least one of molybdenum, nickel and titanium.

3. The method for preparing a solar cell according to claim 2, characterized in that: The material of the electron transport layer is metal nitride.

4. The method for preparing a solar cell according to claim 3, characterized in that: The material of the electron transport layer is titanium nitride, the metal silicon compound alloy layer is a titanium silicon alloy layer, and the annealing temperature is 350°C to 950°C.

5. The method for preparing a solar cell according to claim 1, characterized in that: The thickness of the electron transport layer is greater than 1 nm.

6. The method for preparing a solar cell according to claim 1, characterized in that: The orthographic projection of the electrode on the substrate is located within the orthographic projection of the electron transport layer on the substrate.

7. The method for preparing a solar cell according to claim 1, characterized in that: The preparation method further comprises: The second surface of the substrate is doped to form a doping layer, and a third passivation layer and a fourth passivation layer are sequentially formed on the doping layer.

8. The method for preparing a solar cell according to claim 1, characterized in that: The polysilicon layer includes a first polysilicon layer of a first doping type and a second polysilicon layer of a second doping type, wherein the first polysilicon layer and the second polysilicon layer are insulated from each other; The electron transport layer is formed on the first polysilicon layer and the second polysilicon layer.

9. A solar cell, characterized in that: include: substrate; A first passivation layer, a polysilicon layer, a metal silicon compound alloy layer, an electron transport layer, and a second passivation layer are sequentially disposed on a first surface of the substrate, wherein the metal silicon compound alloy layer is located within the polysilicon layer; An electrode is extended from a surface of the second passivation layer to between the electron transport layer and the first passivation layer, and an ohmic contact is formed between the electrode and the metal silicide.

10. The solar cell according to claim 9, characterized in that: The polysilicon layer and the substrate are of a first doping type, the second surface of the substrate has a doping layer of a second doping type, and a third passivation layer and a fourth passivation layer are sequentially arranged on a side of the doping layer away from the substrate; or, The polysilicon layer includes a first polysilicon layer and a second polysilicon layer which are insulated from each other, the first polysilicon layer and the second polysilicon layer have opposite doping types, and the metal silicon compound alloy layer is disposed in both the first polysilicon layer and the second polysilicon layer.

11. The solar cell according to claim 9 or 10, characterized in that: The orthographic projection of the electrode on the substrate is located within the orthographic projection of the electron transport layer on the substrate; or, The thickness of the electron transport layer is greater than 1 nm.

Citation Information

Patent Citations

  • Crystalline silicon solar cell

    CN113629155A

  • Electron selective passivation contact structure, solar cell and preparation method

    CN114678430A

  • Preparation process of solar cell, solar cell, assembly and system

    CN116565062A

  • Solar cell and photovoltaic module

    CN117059690A

  • Solar cell, preparation method thereof and photovoltaic module

    CN117525179A