TBC solar cell and preparation method thereof
By forming a tunneling oxide layer and an intrinsic polysilicon layer on the substrate of the TBC solar cell, and using laser doping technology to form an isolation zone, the complex problem of TBC solar cell preparation process is solved, process simplification and cost reduction are achieved, and the improvement of photoelectric conversion efficiency.
Patent Information
- Application Number
- CN202411024574.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
The preparation process of TBC solar cells is complicated, resulting in high production costs.
The tunneling oxide layer and the intrinsic polysilicon layer are formed on the substrate in turn, and the first and second doped layers are formed by doping. The laser doping technology is used to form an isolation region in the intrinsic polysilicon layer, which simplifies the process flow and Reduce energy consumption.
The preparation process of TBC solar cells is simplified, production costs are reduced, process time is shortened, and photoelectric conversion efficiency is improved.
Smart Images

Figure CN118943245A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and specifically provides a TBC solar cell and a preparation method thereof. Background Art
[0002] Traditional solar cells have electrode grid lines on both sides, which will block part of the battery. The part of the battery blocked by the electrode grid lines cannot receive sunlight and cannot generate photogenerated electrons and holes, thus affecting the photoelectric conversion efficiency of the battery. In particular, the electrode grid lines arranged on the front side of the battery, which is the light-facing side, have a greater impact on the photoelectric conversion efficiency of the battery. In addition, as the efficiency of conventional batteries (such as TOPCon batteries) gradually approaches the theoretical limit, people have begun to explore more advanced battery structures. Therefore, back contact batteries have gradually begun to develop. Among them, the back contact technology is combined with the TOPCon battery to form a TBC (TOPCon back contact structure, TOPCon back contact) battery, that is, a solar cell with a back tunneling passivation structure.
[0003] The current TBC solar cell preparation method has a complex preparation process and a high production cost. Therefore, a TBC solar cell and a preparation method are urgently needed to solve the problem of the complex preparation process of the existing TBC solar cell. Summary of the invention
[0004] The present invention aims to solve the above technical problem, that is, to solve the problem of complex preparation process of existing TBC solar cells.
[0005] In a first aspect, the present invention provides a method for preparing a TBC solar cell, comprising: providing a substrate, the substrate comprising a first surface; sequentially forming a tunneling oxide layer and an intrinsic polysilicon layer on the first surface; performing doping on the intrinsic polysilicon layer to form a first doping layer; performing laser doping on the intrinsic polysilicon layer to form a second doping layer, the first doping layer and the second doping layer having opposite doping types; and providing an isolation region formed by the undoped intrinsic polysilicon layer between the first doping layer and the second doping layer to isolate the first doping layer from the second doping layer.
[0006] In some exemplary embodiments, laser doping is controlled to form a laser scanning region of the second doping layer, so that the isolation region is formed between the laser scanning region and the first doping layer.
[0007] In some exemplary embodiments, the width of the isolation region is 30 micrometers to 90 micrometers.
[0008] In some exemplary embodiments, doping is performed on the intrinsic polysilicon layer to form a first doped layer, comprising: forming a first slurry layer on the intrinsic polysilicon layer; patterning the first slurry layer; and doping dopant ions in the first slurry layer into the intrinsic polysilicon layer to form the first doped layer.
[0009] In some exemplary embodiments, patterning the first slurry layer includes: patterning the first slurry layer using a picosecond laser.
[0010] In some exemplary embodiments, doping the doping ions in the first slurry layer into the intrinsic polysilicon layer to form a first doping layer includes: placing the substrate into a diffusion furnace and heating it up, so that the doping ions in the first slurry layer are diffused and doped into the intrinsic polysilicon layer to form a first doping layer.
[0011] In some exemplary embodiments, laser doping is performed on the intrinsic polysilicon layer to form a second doped layer, including: forming a second slurry layer on the entire intrinsic polysilicon layer; irradiating a portion of the second slurry layer with a laser so that doping ions in the second slurry layer are doped into the intrinsic polysilicon layer to form the second doped layer; and removing the second slurry layer.
[0012] In some exemplary embodiments, the first slurry layer is removed simultaneously with the removal of the second slurry layer.
[0013] In some exemplary embodiments, the laser is nanosecond green light, with a pulse width of 50 ns to 150 ns, a frequency of 5 kHz to 20 kHz, and a laser beam width of 240 μm to 420 μm.
[0014] In some exemplary embodiments, the method further includes: forming a first anti-reflection layer on the first doping layer, the second doping layer and the isolation region; and / or forming a first electrode and a second electrode insulated from each other, the first electrode being electrically connected to the first doping layer, and the second electrode being electrically connected to the second doping layer.
[0015] In a second aspect, the present invention also provides a TBC solar cell, comprising: a substrate, comprising a first surface; a tunneling oxide layer and a polysilicon layer sequentially formed on the first surface, the polysilicon layer comprising a first doped layer, a second doped layer and an isolation region between the first doped layer and the second doped layer, the first doped layer and the second doped layer having opposite doping types, and the isolation region being intrinsic polysilicon.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The preparation method of the TBC solar cell provided by the present invention comprises: providing a substrate, the substrate comprising a first surface; sequentially forming a tunneling oxide layer and an intrinsic polysilicon layer on the first surface; performing doping on the intrinsic polysilicon layer to form a first doping layer; performing laser doping on the intrinsic polysilicon layer to form a second doping layer, the doping types of the first doping layer and the second doping layer are opposite, and an isolation region formed by an undoped intrinsic polysilicon layer is provided between the first doping layer and the second doping layer to isolate the first doping layer from the second doping layer. The present invention uses laser doping to scan a partial area of the second slurry layer to form a second doped layer in a partial area of the intrinsic polysilicon layer. The intrinsic polysilicon layer only needs to be deposited once, and the first doped layer and the second doped layer are formed in the same intrinsic polysilicon layer, which can shorten the process time and reduce energy consumption. At the same time, the second doped layer is formed by laser doping, and the diffusion speed of the doped ions is slow and the diffusion range is small, that is, the diffusion range to the isolation area is small. Compared with the high-temperature doping method, it helps to ensure that the isolation area can isolate the first doped layer and the second doped layer. Therefore, there is no need to remove the intrinsic polysilicon layer located in the isolation area, thereby simplifying the preparation process of the TBC solar cell.
[0018] Furthermore, by controlling the laser scanning area, a portion of the intrinsic polysilicon layer is reserved between the second doping layer and the first doping layer as an isolation region to isolate the first doping layer from the second doping layer.
[0019] Furthermore, the first slurry layer and the second slurry layer are both formed as a whole layer, and the first slurry layer is patterned using a picosecond laser, and no mask is required during the process, thereby simplifying the preparation process of the TBC solar cell.
[0020] Furthermore, the first doping layer is formed by high-temperature doping, which can reduce the damage to the intrinsic polysilicon layer, the tunneling oxide layer and the substrate during the process of patterning the first slurry layer by laser.
[0021] Furthermore, the first slurry layer and the second slurry layer are removed simultaneously by one chain pickling, thereby simplifying the preparation process of the TBC solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings, in which:
[0023] Figure 1 is a flow chart of the TBC solar cell preparation method provided by the present disclosure;
[0024] Figures 2A to 2G It is a cross-sectional view of the TBC solar cell disclosed in the present invention during the preparation process.
[0025] Description of reference numerals:
[0026] 1. Substrate; 11. First surface; 12. Second surface; 2. Tunneling oxide layer; 3. Intrinsic polysilicon layer; 31. First doping layer; 32. Second doping layer; 33. Isolation region; 4. First slurry layer; 41. Opening; 5. Second slurry layer; 6. First anti-reflection layer; 71. First electrode; 72. Second electrode; 8. Passivation layer; 9. Second anti-reflection layer. DETAILED DESCRIPTION
[0027] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0028] It should be noted that in the description of the present invention, the terms "upper", "lower", "left", "right", "inner", "outer" and the like indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings, which are only for the convenience of description, and do not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0029] Figure 1 It is a flow chart of the TBC solar cell preparation method provided by the present disclosure.
[0030] In order to solve the problem of complex preparation process of existing TBC solar cells, such as Figure 1 As shown, the present disclosure provides a method for preparing a TBC solar cell, comprising: providing a substrate, the substrate comprising a first surface; sequentially forming a tunneling oxide layer and an intrinsic polysilicon layer on the first surface; performing doping on the intrinsic polysilicon layer to form a first doped layer; performing laser doping on the intrinsic polysilicon layer to form a second doped layer, the doping types of the first doped layer and the second doped layer are opposite, and an isolation region formed by an undoped intrinsic polysilicon layer is provided between the first doped layer and the second doped layer to isolate the first doped layer from the second doped layer.
[0031] Next, the method for preparing the solar cell provided by the embodiment of the present disclosure is introduced.
[0032] Figures 2A to 2G is a cross-sectional view of the TBC solar cell disclosed in the present invention during the preparation process,
[0033] First, if Figure 2AAs shown, a substrate 1 is provided, and the substrate 1 has a first surface 11 and a second surface 12 opposite to the first surface 11, wherein the second surface 12 is a light-facing surface. The substrate 1 is an N-type silicon substrate, or a P-type silicon substrate. For example, the first surface 11 and the second surface 12 of the substrate 1 are textured; or, the second surface 12 of the substrate 1 is textured, and the first surface 11 of the substrate 1 is polished. After the second surface 12 is textured, the surface area of the second surface 12 and the surface complexity can be increased, thereby increasing the diffuse reflection effect of the second surface 12 on light.
[0034] For example, the substrate 1 is an N-type substrate 1, and the N-type substrate 1 is immersed in a KOH or NaOH solution with a temperature of 60°C to 80°C and a mass fraction of 1% to 3% for texturing, and the texturing time is controlled to be 15 minutes to 25 minutes.
[0035] A passivation layer 8 and a second anti-reflection layer 9 are sequentially formed on the second surface 12 of the substrate 1, and a tunneling oxide layer 2 and an intrinsic polysilicon layer 3 are sequentially formed on the first surface 11 of the substrate 1. For example, the tunneling oxide layer 2 and the intrinsic polysilicon layer 3 are generated by LPCVD (Low Pressure Chemical Vapor Deposition). For example, the material of the tunneling oxide layer can be any one of silicon oxide, aluminum oxide, tantalum oxide, zirconium oxide, and titanium dioxide, the material of the passivation layer 8 is aluminum oxide, and the material of the second anti-reflection layer 9 is silicon nitride (SiNx). After the second surface 12 is textured, the passivation layer 8 and the second anti-reflection layer 9 formed on the second surface 12 can have a more complex surface, and light can be diffusely reflected after being irradiated to the passivation layer 8, and then reflected by the second anti-reflection layer 9, which can improve the absorption efficiency of light, thereby improving the conversion efficiency of solar cells.
[0036] Combination Figure 2B and Figure 2C As shown, the intrinsic polysilicon layer 3 is doped to form a first doping layer 31, which specifically includes:
[0037] like Figure 2B As shown, a first slurry layer 4 is formed on the intrinsic polysilicon layer 3. For example, the first slurry layer 4 is formed by CVD (Chemical Vapor Deposition). The first slurry layer 4 can be BSG (boron-silicate glass) or PSG (phosphorus-silicate glass). The thickness of the first slurry layer 4 is 30nm to 80nm.
[0038] like Figure 2CAs shown, the first slurry layer 4 is patterned, and the patterned first slurry layer 4 covers a portion of the intrinsic polysilicon layer 3. After the first slurry layer 4 is patterned, an opening 41 is formed, and the width of the opening 41 is 400μm to 500μm. For example, a picosecond laser is used to pattern the first slurry layer 4. The duration of the picosecond laser beam emitted by the picosecond laser is short, and the material is heated slowly. The temperature rise is not large during the removal of the first slurry layer 4, and the doped ions in the first slurry layer 4 irradiated by the laser will not be doped into the intrinsic polysilicon layer 3. In this way, there is no need to prepare a mask during the patterning of the first slurry layer 4, thereby simplifying the preparation process of preparing TBC solar cells.
[0039] The doping ions in the first slurry layer 4 are doped into the intrinsic polysilicon layer 3 covered by the first slurry layer 4 to form the first doping layer 31. For example, the first doping layer 31 is formed by high-temperature diffusion. Specifically, the substrate 1 is placed in a diffusion furnace and heated up, so that the doping ions in the first slurry layer 4 are doped into the intrinsic polysilicon layer 3 covered by the first slurry layer 4 to form the first doping layer 31. At the same time, the formation of the first doping layer 31 by high-temperature diffusion can also reduce the damage to the intrinsic polysilicon layer 3, the tunneling oxide layer 2 and the substrate 1 in the process of patterning the first slurry layer 4 by laser. Of course, in other examples, other methods can also be used to dope the doping ions in the first slurry layer 4 into the intrinsic polysilicon layer 3 covered by the first slurry layer 4 to form the first doping layer 31, such as by laser doping.
[0040] Combination Figure 2D and Figure 2E As shown, doping is performed on the intrinsic polysilicon layer 3 to form a second doping layer 32 of a second doping type, which specifically includes:
[0041] like Figure 2D As shown, a second slurry layer 5 is formed on the intrinsic polysilicon layer 3, and the second slurry layer 5 covers the first slurry layer 4. For example, the second slurry layer 5 is formed by CVD (Chemical Vapor Deposition). When the first slurry layer 4 is BSG (boron-silicate glass), the second slurry layer 5 is PSG (phosphorus-silicate glass); when the first slurry layer 4 is PSG, the second slurry layer 5 is BSG.
[0042] The doping ions in the second slurry layer 5 are doped into the intrinsic polysilicon layer 3 by laser doping to form a second doping layer 32, and the doping type of the second doping layer 32 is opposite to that of the first doping layer 31. The laser irradiated portion of the second slurry layer 5 is specifically a portion of the second slurry layer 5 located in the opening 41, so that the second doping layer 32 is formed in a portion of the intrinsic passivation layer 8 exposed at the opening 41.
[0043] During the process of laser doping to form the second doped layer 32, the area scanned by the laser determines the area where the second doped layer 32 is located. By controlling the laser scanning area, an isolation region 33 can be formed between the second doped layer 32 and the first doped layer 31, and the isolation region 33 specifically includes an undoped intrinsic polysilicon layer 3. The isolation region 33 can isolate the first doped layer 31 and the second doped layer 32, and prevent the first doped layer 31 and the second doped layer 32 from forming an electron flow and short circuit.
[0044] Of course, in other examples, the intrinsic polysilicon in the isolation region 33 may be removed by laser to form an isolation groove to isolate the first doping layer 31 and the second doping layer 32 .
[0045] For example, the laser used for laser doping is nanosecond green light, with a pulse width of 50ns to 150ns, a frequency of 5kHz to 20kHz, and a laser beam width of 240μm to 420μm. The laser beam of the nanosecond laser has a long duration, and the second slurry layer 5 scanned and irradiated by the nanosecond laser can be rapidly heated up, so that the doping ions in the second slurry layer 5 are doped into the intrinsic polysilicon layer 3 to form the second doping layer 32; the second slurry layer 5 not scanned and irradiated by the nanosecond laser will not be heated up, so that the area of the second doping layer 32 can be controlled by controlling the scanning range of the nanosecond laser. In addition, during the laser doping process, the area irradiated by the laser scanning is locally heated up rapidly for doping, and the heat is dissipated quickly, which can minimize the diffusion speed and diffusion range of the doped ions, reduce the diffusion speed and diffusion range of the doped ions in the second doped layer 32 to the isolation region 33, and ensure that the isolation region 33 can isolate the first doped layer 31 and the second doped layer 32, thereby eliminating the need to remove the intrinsic polysilicon layer 3 on the isolation region 33 to isolate the first doped layer 31 and the second doped layer 32, thereby simplifying the preparation process of the TBC solar cell.
[0046] For example, the width of the isolation region 33 is 30 micrometers to 90 micrometers, preferably 40 micrometers to 80 micrometers, to ensure that the isolation region 33 has a sufficient width to isolate the first doping layer 31 and the second doping layer 32 .
[0047] like Figure 2E As shown, the second slurry layer 5 is removed, for example, by chain pickling to remove the second slurry layer 5. The first slurry layer 4 can be removed at the same time as the second slurry layer 5 is removed, so as to simplify the preparation process of the TBC solar cell.
[0048] like Figure 2FAs shown, a first anti-reflection layer 6 is formed on the first doping layer 31, the second doping layer 32 and the isolation region 33. For example, the material of the first anti-reflection layer 6 is silicon nitride (SiNx), and the thickness of the first anti-reflection layer 6 is 40nm to 90nm. The first anti-reflection layer 6 can increase the passivation characteristics of the surface of the solar cell, and the first anti-reflection layer 6 can reflect the sunlight incident on the solar cell, thereby increasing the light absorption efficiency.
[0049] like Figure 2G As shown, a first electrode 71 and a second electrode 72 are formed to be insulated from each other, the first electrode 71 is electrically connected to the first doping layer 31, and the second electrode 72 is electrically connected to the second doping layer 32. Specifically, an electrode material layer is formed on the first anti-reflection layer 6 by screen printing, and then the electrode material layer is heated. After the electrode material layer is melted by heat, it can corrode the first anti-reflection layer 6, so that the electrode material layer is electrically connected to the first doping layer 31 and the second doping layer 32. Among them, the electrode material layer electrically connected to the first doping layer 31 is the first electrode 71, and the electrode material layer electrically connected to the second doping layer 32 is the second electrode 72.
[0050] In summary, the method for preparing a TBC solar cell provided by the present disclosure has at least the following advantages:
[0051] (1) Scanning a partial area of the second slurry layer 5 by laser doping to form a second doped layer 32 in a partial area of the intrinsic polysilicon layer 3, and reserving a portion of the intrinsic polysilicon layer 3 as an isolation region 33 between the second doped layer 32 and the first doped layer 31 by controlling the laser scanning area to isolate the first doped layer 31 from the second doped layer 32; at the same time, the second doped layer 32 is formed by laser doping, and the diffusion speed of the doped ions is slow and the diffusion range is small, that is, the diffusion range to the isolation region 33 is small. Compared with the high-temperature doping method, it helps to ensure that the isolation region 33 can isolate the first doped layer 31 from the second doped layer 32. Therefore, there is no need to remove the intrinsic polysilicon layer 3 located in the isolation region 33, thereby simplifying the preparation process of the TBC solar cell;
[0052] (2) The first slurry layer 4 and the second slurry layer 5 are both formed as a whole layer, and the first slurry layer 4 is patterned by a picosecond laser, and no mask is required during the process, thereby simplifying the preparation process of the TBC solar cell;
[0053] (3) The first doping layer 31 is formed by high-temperature doping, which can reduce the damage to the intrinsic polysilicon layer 3, the tunneling oxide layer 2 and the substrate 1 during the process of patterning the first slurry layer 4 by laser;
[0054] (4) The intrinsic polysilicon layer 3 only needs to be deposited once, and the first doped layer 31 and the second doped layer 32 are formed in the same intrinsic polysilicon layer 3, which can shorten the process time and reduce energy consumption;
[0055] (5) The first slurry layer 4 and the second slurry layer 5 are removed simultaneously by one chain pickling, thereby simplifying the preparation process of the TBC solar cell.
[0056] Some embodiments of the present disclosure also provide a TBC solar cell, comprising: a substrate, comprising a first surface; a tunneling oxide layer and a polysilicon layer sequentially formed on the first surface, the polysilicon layer comprising a first doping layer of a first doping type, a second doping layer of a second doping type, and an isolation region between the first doping layer and the second doping layer, the isolation region being intrinsic polysilicon, and the first doping type and the second doping type being opposite.
[0057] The following is Figure 2G The examples shown illustrate solar cells of some embodiments of the present disclosure.
[0058] like Figure 2G As shown, in at least one example of the present invention, the solar cell includes a substrate 1, the substrate 1 having a first surface 11 and a second surface 12 opposite to the first surface 11, wherein the second surface 12 is a light-facing surface. The substrate 1 is an N-type silicon substrate or a P-type silicon substrate.
[0059] The second surface 12 of the substrate 1 is provided with a passivation layer 8 and a second anti-reflection layer 9 in sequence. Sunlight enters the substrate 1 from the passivation layer 8 and the second anti-reflection layer 9, and the sunlight reflected by the substrate 1 can be reflected by the passivation layer 8 and the second anti-reflection layer 9 and then be emitted to the substrate 1 again, thereby improving the light absorption efficiency of the solar cell. The material of the passivation layer 8 is aluminum oxide, and the material of the second anti-reflection layer 9 is silicon nitride (SiNx).
[0060] The first surface 11 of the substrate 1 is provided with a tunneling oxide layer 2 and a polysilicon layer in sequence. The polysilicon layer includes a first doping layer 31, a second doping layer 32, and an isolation region 33 located between the first doping layer 31 and the second doping layer 32. The doping types of the first doping layer 31 and the second doping layer 32 are opposite, for example, the first doping layer 31 is P-type doped, and the second doping layer 32 is N-type doped. The polysilicon layer in the isolation region 33 is intrinsic polysilicon, so that the first doping layer 31 and the second doping layer 32 are isolated by the polysilicon layer in the isolation region 33.
[0061] The material of the tunneling oxide layer can be any one of silicon oxide, aluminum oxide, tantalum oxide, zirconium oxide, and titanium dioxide.
[0062] The polysilicon layer is provided with a first anti-reflection layer 6. The first anti-reflection layer 6 can increase the passivation characteristics of the surface of the solar cell, and the first anti-reflection layer 6 can reflect the sunlight incident on the solar cell, thereby increasing the light absorption efficiency.
[0063] The TBC solar cell also includes a first electrode 71 and a second electrode 72 insulated from each other, the first electrode 71 is electrically connected to the first doping layer 31, and the second electrode 72 is electrically connected to the second doping layer 32. Specifically, an electrode material layer is formed on the first anti-reflection layer 6 by screen printing, and then the electrode material layer is heated. After the electrode material layer is melted by heat, it can corrode the first anti-reflection layer 6, so that the electrode material layer is electrically connected to the first doping layer 31 and the second doping layer 32. Among them, the electrode material layer electrically connected to the first doping layer 31 is the first electrode 71, and the electrode material layer electrically connected to the second doping layer 32 is the second electrode 72.
[0064] There are a few points to note:
[0065] (1) The drawings of the embodiments of the present disclosure only relate to the structures related to the embodiments of the present disclosure, and other structures may refer to the general design.
[0066] (2) For the sake of clarity, in the drawings used to describe the embodiments of the present disclosure, the thickness of layers or regions is enlarged or reduced, that is, these drawings are not drawn according to the actual scale.
[0067] (3) In the absence of conflict, the embodiments of the present disclosure and the features therein may be combined with each other to obtain new embodiments.
[0068] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
Claims
1. A method for preparing a TBC solar cell, characterized in that: include: Providing a substrate (1), wherein the substrate (1) comprises a first surface (11); forming a tunneling oxide layer (2) and an intrinsic polysilicon layer (3) in sequence on the first surface (11); Performing doping on the intrinsic polysilicon layer (3) to form a first doping layer (31); Performing laser doping on the intrinsic polysilicon layer (3) to form a second doping layer (32), wherein the first doping layer (31) and the second doping layer (32) have opposite doping types; An isolation region (33) formed by the undoped intrinsic polysilicon layer (3) is provided between the first doped layer (31) and the second doped layer (32) to isolate the first doped layer (31) and the second doped layer (32).
2. The method for preparing a TBC solar cell according to claim 1, characterized in that: Laser doping is controlled to form a laser scanning area of the second doping layer (32), so that the isolation area (33) is formed between the laser scanning area and the first doping layer (31).
3. The method for preparing a TBC solar cell according to claim 1, characterized in that: The width of the isolation region (33) is 30 micrometers to 90 micrometers.
4. The method for preparing a TBC solar cell according to claim 1, characterized in that: Doping is performed on the intrinsic polysilicon layer (3) to form a first doping layer (31), comprising: forming a first slurry layer (4) on the intrinsic polysilicon layer (3); patterning the first slurry layer (4); The doping ions in the first slurry layer (4) are doped into the intrinsic polysilicon layer (3) to form a first doping layer (31).
5. The method for preparing a TBC solar cell according to claim 4, characterized in that: Patterning the first slurry layer (4), comprising: The first slurry layer (4) is patterned using a picosecond laser.
6. The method for preparing a TBC solar cell according to claim 4, characterized in that: Doping the doping ions in the first slurry layer (4) into the intrinsic polysilicon layer (3) to form a first doping layer (31), comprising: The substrate (1) is placed in a diffusion furnace and heated, so that the doping ions in the first slurry layer (4) are diffused and doped into the intrinsic polysilicon layer (3) to form a first doping layer (31).
7. The method for preparing a TBC solar cell according to claim 4, characterized in that: Laser doping is performed on the intrinsic polysilicon layer (3) to form a second doping layer (32), comprising: forming a second slurry layer (5) entirely on the intrinsic polysilicon layer (3); irradiating a portion of the second slurry layer (5) with laser light, so that the doping ions in the second slurry layer (5) are doped into the intrinsic polysilicon layer (3) to form the second doping layer (32); The second slurry layer (5) is removed.
8. The method for preparing a TBC solar cell according to claim 7, characterized in that: The first slurry layer (4) is removed while the second slurry layer (5) is removed.
9. The method for preparing a TBC solar cell according to claim 7, characterized in that: The laser is nanosecond green light, with a pulse width of 50ns to 150ns, a frequency of 5kHz to 20kHz, and a laser beam width of 240μm to 420μm.
10. The method for preparing a TBC solar cell according to claim 1, characterized in that: The method further comprises: forming a first anti-reflection layer (6) on the first doping layer (31), the second doping layer (32) and the isolation region (33); and / or, A first electrode (71) and a second electrode (72) insulated from each other are formed, wherein the first electrode (71) is electrically connected to the first doping layer (31), and the second electrode (72) is electrically connected to the second doping layer (32).
11. A TBC solar cell, characterized in that: include: A substrate (1) comprising a first surface (11); A tunneling oxide layer (2) and a polysilicon layer are sequentially formed on the first surface (11), the polysilicon layer comprising a first doping layer (31), a second doping layer (31), and an isolation region (33) located between the first doping layer (31) and the second doping layer (32), the first doping layer (31) and the second doping layer (31) having opposite doping types, and the isolation region (33) being intrinsic polysilicon.
Citation Information
Cited By
TBC battery and preparation method thereof
CN120786956A
TBC solar cell and preparation method and application thereof
CN121194552A
Back contact battery, battery assembly and photovoltaic system
CN122054747A
A back contact cell, cell assembly and photovoltaic system
CN122054747B