Aqueous zinc ion battery negative electrode material with functional protection layer and preparation method and application thereof
By forming a functional protective coating on the negative electrode material of the aqueous zinc ion battery, problems such as dendrites are solved, the cycle stability and rate performance of the battery are improved, and more efficient electrochemical reactions are achieved.
Patent Information
- Application Number
- CN202410990977.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The negative electrode material of the aqueous zinc ion battery faces problems such as dendrite, deformation, hydrogen evolution and passivation, which limits the improvement of battery performance.
In-situ impregnation method is used to form a functional protective coating on the surface of zinc foil. Through the reaction of aminosilane coupling agent and glycidyl methacrylate, an ultra-thin micro-nano interface layer is formed to improve the mechanical properties and corrosion resistance of zinc foil. .
Effectively inhibit the growth of zinc dendrites, improve the cycle stability and rate performance of the battery, promote the uniform deposition of zinc ions and electrochemical reactions, and enhance the overall performance of the battery.
Smart Images

Figure CN118943272A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aqueous ion batteries, and in particular relates to an aqueous zinc ion battery negative electrode material with a functional protective layer, and a preparation method and application thereof. Background Art
[0002] With the rapid development of renewable energy and the promotion of energy transformation, efficient, safe and sustainable energy storage technology has become increasingly important. In this context, the research on aqueous zinc-ion batteries is of great significance. First, aqueous zinc-ion batteries have inherent safety. Compared with traditional organic solvent electrolytes, aqueous solutions as electrolytes have higher ionic conductivity and will not cause safety problems such as thermal runaway or flammable explosion caused by organic solvents. This makes aqueous zinc-ion batteries more reliable and safe when storing large-scale electrical energy. Secondly, aqueous zinc-ion batteries have higher energy and power density. Zinc as a negative electrode material has a low redox potential and fast kinetics, which can achieve efficient battery charge and discharge reactions. In alkaline systems, zinc obtains a higher ion transfer rate, thereby improving the energy and power density of the battery. This makes aqueous zinc-ion batteries an ideal choice for application scenarios requiring high power output. In addition, metallic zinc as a negative electrode material has the characteristics of abundant resources, low toxicity and easy handling. Compared with rare metals such as lithium, zinc resources are relatively abundant and low cost, which helps to reduce battery manufacturing costs and promote the commercialization and popularization of battery technology. At the same time, the use of zinc-ion batteries also avoids safety issues such as lithium metal accumulation that occur in traditional lithium-ion batteries. Therefore, the significance of studying the negative electrode of aqueous zinc-ion batteries is to promote the large-scale storage and utilization of renewable energy, and promote energy transformation and the realization of green energy.
[0003] At present, the research on aqueous ion batteries is mainly focused on developing new cathode materials and improving the performance of existing cathode materials. Researchers in this field are committed to finding strategies to improve battery performance. However, we cannot ignore the challenges faced by the negative electrode, such as dendrites, deformation, hydrogen evolution and passivation. In fact, these problems are the key factors limiting the performance improvement of aqueous ion batteries.
[0004] Therefore, proposing solutions for the preparation technology of negative electrode materials for aqueous ion batteries is of great significance for promoting the research and practical application of high-performance aqueous ion batteries. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and provide an aqueous zinc ion battery negative electrode material with a functional protective layer and a preparation method and application thereof.
[0006] To solve the technical problem, the solution of the present invention is:
[0007] Provided is a method for preparing an aqueous zinc ion battery negative electrode material having a functional protective coating, comprising the following steps:
[0008] Step 1, preparing a homogeneous solution I by adding appropriate amounts of anhydrous methanol, deionized water and silane coupling agent;
[0009] Step 2, grinding the zinc foil with sandpaper, cleaning it with ethanol and deionized water, drying it, and then immersing it in the homogeneous solution I prepared in step 1 for a suitable time;
[0010] Step 3, anhydrous methanol, deionized water and glycidyl methacrylate are mixed evenly, and glacial acetic acid is used as a catalyst, and stirred to form a homogeneous solution II;
[0011] Step 4: The zinc foil aminated in step 2 is transferred and immersed in the homogeneous solution II for an appropriate period of time to obtain an aqueous zinc ion battery negative electrode material with a functional protective coating.
[0012] As a preferred embodiment of the present invention, in step 1, the volume ratio of anhydrous methanol to deionized water is 9:1; the silane coupling agent includes one or more of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, and the amount thereof is 1-1000 μL.
[0013] As a preferred embodiment of the present invention, in step 2, one side of the cleaned and dried zinc foil is covered, so that the zinc foil is aminated on one side.
[0014] As a preferred embodiment of the present invention, in step 2, the immersion time is 0.1-48h.
[0015] As a preferred embodiment of the present invention, in step 3, the volume ratio of anhydrous methanol to deionized water is 9:1; the amount of glycidyl methacrylate is 1-1000 μL; and the amount of glacial acetic acid is 1-1000 μL.
[0016] As a preferred embodiment of the present invention, in step 4, the immersion time is 0.1-48h.
[0017] As a preferred embodiment of the present invention, the immersion time in step 2 is equal to that in step 4.
[0018] The present invention further provides an application method of the negative electrode material prepared by the aforementioned method in further preparing an aqueous zinc ion battery, which comprises slicing the negative electrode material having a functional protective coating to obtain an electrode sheet, which is used as the negative electrode of the aqueous zinc ion battery.
[0019] As a preferred solution of the present invention, the electrode sheet is a circular electrode sheet with a diameter of 1 to 19 mm.
[0020] As a preferred embodiment of the present invention, the aqueous zinc ion battery is prepared according to the following steps:
[0021] (1) Slicing the negative electrode material with the functional protective coating to obtain a circular electrode sheet as the negative electrode of the aqueous zinc ion battery;
[0022] (2) MnO2, Supper P and polyvinylidene fluoride (PVDF) are taken in a mass ratio of 7:2:1, dissolved in an appropriate amount of N-methylpyrrolidone (NMP), and mixed evenly to obtain a slurry; the slurry is coated on a Ti foil, dried at 60°C under vacuum conditions for 24 hours, and then cut into circular electrode sheets as the positive electrode of an aqueous zinc ion battery; the diameter of the positive electrode sheet is slightly smaller than that of the negative electrode sheet;
[0023] (3) preparing a 2M ZnSO4 aqueous solution as an electrolyte for an aqueous zinc ion battery; and using a cellulose diaphragm as a diaphragm for the aqueous zinc ion battery;
[0024] (4) 2025 battery positive electrode shell, negative electrode, cellulose separator, ZnSO4 electrolyte, negative electrode, nickel foam, and 2025 battery negative electrode shell are placed in order to assemble into a symmetrical battery; or,
[0025] The complete battery is assembled by placing the 2025 battery positive electrode shell, positive electrode, cellulose separator, ZnSO4 electrolyte, negative electrode, nickel foam and 2025 battery negative electrode shell in sequence.
[0026] Description of the principle of the present invention:
[0027] Aminosilane coupling agents are a class of silane compounds with amino functional groups. They contain silicon-amino bonds in their chemical structure. These coupling agents can establish chemical bonds between organic and inorganic materials, thereby improving the interfacial compatibility and bonding properties of the materials. Their main characteristics are: (1) Affinity with inorganic substances: The amino groups in aminosilane coupling agents can react with the hydroxyl or oxygen groups on the surface of inorganic substances to form stable silicon-oxygen-metal bonds, thereby improving the adhesion and compatibility of the interface; (2) Surface activity: Aminosilane coupling agents can introduce amino functional groups on the surface of materials, enhance surface activity and improve wettability, which is beneficial for applications such as coating and bonding; (3) Cross-linking properties: The silicon-amino bonds in aminosilane coupling agents can form cross-linked structures with other functional groups, thereby improving the mechanical properties and durability of materials. Glycidyl methacrylate is rich in olefin double bonds and epoxy groups, and can undergo free radical polymerization, which makes it have good polymerizability and cross-linking properties. It also has good solubility resistance to solvents such as water, acid, and alkali, which makes it have the advantage of anti-solvent in coatings, adhesives, and anti-corrosion materials. Therefore, when preparing zinc metal negative electrode materials, aminosilane coupling agents react with hydroxyl or oxygen groups on the surface of zinc foil to form chemical bonds, firmly connecting the gel layer to the surface of zinc foil. At the same time, glycidyl methacrylate undergoes polymerization or cross-linking in the reaction to form a stable gel structure, increasing the mechanical strength and stability of the gel layer. The formation of a gel layer can improve the performance of the zinc foil surface, improve its corrosion resistance, weather resistance, and chemical resistance, and can also provide a better basis for surface treatment and coating.
[0028] In order to achieve the above purpose, the present invention first immerses the metal zinc foil in a homogeneous solution of anhydrous methanol, deionized water and aminosilane coupling agent to perform preliminary surface amination on the zinc foil; then prepares a mixed solution of anhydrous methanol, deionized water and glycidyl methacrylate, and stirs with glacial acetic acid as a catalyst to form a homogeneous solution, and transfers the amination zinc foil to the homogeneous solution containing glycidyl methacrylate for subsequent crosslinking. After a certain period of immersion, an ultra-thin micro-nano interface layer grows on the surface of the zinc foil, which can be used as a functional protective coating to prepare the negative electrode material of aqueous zinc ion batteries and used as high-performance aqueous zinc ion batteries.
[0029] The in-situ impregnation method is also called the in-situ etching method. It is easy to operate. It only requires the electrode material to be directly immersed in the required solution without complicated equipment and steps. It has high controllability. By adjusting the concentration, temperature and immersion time of the impregnation solution and other parameters, the growth process of the negative electrode interface layer can be precisely controlled. In this way, the structure and performance of the interface layer can be finely controlled to meet the requirements of battery design. It has good uniformity. The in-situ impregnation method can achieve uniform distribution of the impregnation solution, so that the negative electrode interface layer grows uniformly on the electrode surface. This helps to improve the overall performance and cycle stability of the battery. It can be prepared on a large scale. The impregnation method is not limited to the size of the zinc metal substrate and can achieve large-scale preparation of zinc negative electrode materials.
[0030] The present invention utilizes the micro-nano structure modified by the gel interface obtained in step 4 to effectively shorten the transmission distance of electrons and ions. Secondly, the electric field distribution on the electrode surface is more uniform, which helps to improve the microscopic reaction uniformity and stability of the battery. At the same time, the highly zinc-affinity functional group can effectively adsorb Zn 2+ , achieving uniform surface ion distribution. This helps to reduce the nucleation barrier and nucleation overpotential, and inhibit the growth of zinc dendrites. Therefore, the negative electrode material prepared by this method is conducive to obtaining aqueous zinc ion batteries with good rate performance and long cycle stability.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The present invention adopts an in-situ impregnation method to form a uniform and ultra-thin gel interface protective layer on the surface of the metal zinc foil. The functional protective layer has a strong binding force with the zinc substrate, and the zinc-philic active groups on the surface can produce a strong electrostatic effect with zinc ions, thereby effectively adsorbing zinc ions in the solution and guiding them to deposit uniformly, effectively inhibiting the growth of zinc dendrites. In addition, these zinc-philic groups can also change the solvation structure of metal ions and form a hydrogen bond network with free water, thereby inhibiting water corrosion of zinc.
[0033] (2) The in-situ impregnation method on the metal substrate adopted by the present invention is universal and can be extended to copper foil, titanium foil, stainless steel foil and other metal substrates, and has the same or similar technical effects. At the same time, the method is not limited to the size of the zinc substrate and can be prepared on a large scale.
[0034] (3) The metal negative electrode with a functional protective coating prepared by the present invention has excellent performance, effectively inhibits the growth of negative electrode dendrites and the occurrence of side reactions, and the aqueous zinc ion battery prepared therefrom has high cycle stability and excellent rate performance, and is expected to accelerate the industrialization process of aqueous zinc ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1The surface morphologies of the pure metal zinc foil in the present invention and the negative electrodes prepared in Example 11 and Comparative Example 1; (a) is the surface morphology of the pure metal zinc foil (bare Zn) without a functional protective coating; (b) is the surface morphology of the negative electrode (SG@Zn) with a functional protective coating.
[0036] Figure 2 XPS high-resolution spectra of the pure metal zinc foil in the present invention and the negative electrodes prepared in Example 11 and Comparative Example 4; (a) Zn 2p, (b) O 1s, (c) Si 2p.
[0037] Figure 3 The performance test results of the symmetrical battery assembled with the pure metal zinc foil of the present invention and the negative electrode prepared in Example 11 and Comparative Example 1; (a) linear cyclic voltammetry curve, (b) it curve Figure 4 The electrochemical performance test results of the pure metal zinc foil and the negative electrode prepared in Example 11 and Comparative Example 1 assembled into a symmetrical cell and a Cu-Zn semi-symmetrical cell; (a) the bare Zn symmetrical cell at 2 mA cm -2 , 2mAh cm -2 Time-voltage curves of the SG@Zn symmetric battery at 2 mA cm -2 , 2mAh cm -2 The time-voltage curve below and the enlarged view of part (d).
[0038] Figure 5 The electrochemical performance of the full battery assembled with the pure metal zinc foil of the present invention and the negative electrode prepared in Example 4 and Comparative Example 4. (a) Self-discharge performance of bare Zn, (b) Self-discharge performance of SG@Zn, (c) Cycle curve at 1C rate (700 cycles). DETAILED DESCRIPTION
[0039] The technical solution of the present invention is further described below by specific implementation methods. The embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0040] Example 1
[0041] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0042] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly, and 1 μL of aminosilane coupling agent γ-aminopropyltriethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0043] (2) immersing the zinc foil polished and cleaned with sandpaper in the homogeneous solution described in (1) for 0.1 h to perform amino treatment on the surface of the zinc foil;
[0044] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 1 μL of glacial acetic acid and 1 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0045] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 0.1 h to finally obtain a negative electrode material with a functional protective coating.
[0046] 2. Example of application method for preparing symmetrical batteries:
[0047] (1) Slicing the negative electrode material with the functional protective coating to obtain a circular electrode sheet as the negative electrode of the aqueous zinc ion battery;
[0048] (2) MnO2, Supper P and polyvinylidene fluoride (PVDF) were taken in a mass ratio of 7:2:1, dissolved in an appropriate amount of N-methylpyrrolidone (NMP), and mixed evenly to obtain a slurry; the slurry was coated on a Ti foil, dried at 60°C under vacuum conditions for 24 hours, and then cut into circular electrode sheets as the positive electrode of an aqueous zinc ion battery;
[0049] The diameter of the negative electrode sheet can be selected to be 1 to 19 mm, and the diameter of the positive electrode sheet is slightly smaller than that of the negative electrode sheet;
[0050] (3) preparing a 2M ZnSO4 aqueous solution as an electrolyte for an aqueous zinc ion battery; and using a cellulose diaphragm as a diaphragm for the aqueous zinc ion battery;
[0051] (4) Place the 2025 battery positive electrode shell, negative electrode, cellulose separator, ZnSO4 electrolyte, negative electrode, nickel foam, and 2025 battery negative electrode shell in order to assemble into a symmetrical battery;
[0052] 3. Example of application method for preparing full battery:
[0053] (1) Prepare the battery components and prepare the electrolyte according to the steps in the method for preparing a symmetrical battery;
[0054] The difference is that the electrode on the positive side is a MnO2 electrode.
[0055] (2) Place the 2025 battery positive electrode shell, MnO2 positive electrode, cellulose separator, ZnSO4 electrolyte, negative electrode, nickel foam, and 2025 battery negative electrode shell in order to assemble a full battery.
[0056] Example 2
[0057] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0058] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly. 100 μL of aminosilane coupling agent γ-aminopropyltriethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0059] (2) immersing the zinc foil that has been sanded and cleaned in the homogeneous solution described in (1) for 2 hours to perform amino treatment on the surface of the zinc foil;
[0060] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 10 μL of glacial acetic acid and 10 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0061] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 2 hours to finally obtain a negative electrode material with a functional protective coating.
[0062] The application method of the negative electrode material refers to Example 1.
[0063] Example 3
[0064] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0065] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly, and 500 μL of aminosilane coupling agent γ-aminopropyltriethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0066] (2) immersing the zinc foil polished and cleaned with sandpaper in the homogeneous solution described in (1) for 5 hours to perform amino treatment on the surface of the zinc foil;
[0067] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 500 μL of glacial acetic acid and 500 μL of glycidyl methacrylate were added to the above solution and stirred continuously until the mixture was homogeneous;
[0068] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 5 hours to finally obtain a negative electrode material with a functional protective coating.
[0069] The application method of the negative electrode material refers to Example 1.
[0070] Example 4
[0071] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0072] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly, and 1000 μL of aminosilane coupling agent γ-aminopropyltriethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0073] (2) immersing the zinc foil polished and cleaned with sandpaper in the homogeneous solution described in (1) for 48 hours to perform amino treatment on the surface of the zinc foil;
[0074] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 1000 μL of glacial acetic acid and 1000 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0075] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 48 hours to finally obtain a negative electrode material with a functional protective coating.
[0076] The application method of the negative electrode material refers to Example 1.
[0077] Example 5
[0078] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0079] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly. 1 μL of aminosilane coupling agent γ-aminopropyltrimethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0080] (2) immersing the zinc foil polished and cleaned with sandpaper in the homogeneous solution described in (1) for 0.1 h to perform amino treatment on the surface of the zinc foil;
[0081] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 1 μL of glacial acetic acid and 1 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0082] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 0.1 h to finally obtain a negative electrode material with a functional protective coating.
[0083] The application method of the negative electrode material refers to Example 1.
[0084] Example 6
[0085] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0086] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly. 100 μL of aminosilane coupling agent γ-aminopropyltrimethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0087] (2) immersing the zinc foil that has been sanded and cleaned in the homogeneous solution described in (1) for 2 hours to perform amino treatment on the surface of the zinc foil;
[0088] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 10 μL of glacial acetic acid and 10 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0089] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 2 hours to finally obtain a negative electrode material with a functional protective coating.
[0090] The application method of the negative electrode material refers to Example 1.
[0091] Example 7
[0092] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0093] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly. 500 μL of aminosilane coupling agent γ-aminopropyltrimethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0094] (2) immersing the zinc foil polished and cleaned with sandpaper in the homogeneous solution described in (1) for 5 hours to perform amino treatment on the surface of the zinc foil;
[0095] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 50 μL of glacial acetic acid and 500 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0096] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 5 hours to finally obtain a negative electrode material with a functional protective coating.
[0097] The application method of the negative electrode material refers to Example 1.
[0098] Example 8
[0099] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0100] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly, and 1000 μL of aminosilane coupling agent γ-aminopropyltriethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0101] (2) immersing the zinc foil polished and cleaned with sandpaper in the homogeneous solution described in (1) for 48 hours to perform amino treatment on the surface of the zinc foil;
[0102] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 1000 μL of glacial acetic acid and 1000 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0103] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 48 hours to finally obtain a negative electrode material with a functional protective coating.
[0104] The application method of the negative electrode material refers to Example 1.
[0105] Example 9
[0106] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0107] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly. 1 μL of aminosilane coupling agent N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0108] (2) immersing the zinc foil polished and cleaned with sandpaper in the homogeneous solution described in (1) for 0.1 h to perform amino treatment on the surface of the zinc foil;
[0109] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 1 μL of glacial acetic acid and 1 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0110] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 0.1 h to finally obtain a negative electrode material with a functional protective coating.
[0111] The application method of the negative electrode material refers to Example 1.
[0112] Example 10
[0113] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0114] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly, and 100 μL of aminosilane coupling agent N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0115] (2) immersing the zinc foil that has been sanded and cleaned in the homogeneous solution described in (1) for 2 hours to perform amino treatment on the surface of the zinc foil;
[0116] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 10 μL of glacial acetic acid and 10 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0117] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 2 hours to finally obtain a negative electrode material with a functional protective coating.
[0118] The application method of the negative electrode material refers to Example 1.
[0119] Embodiment 11
[0120] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0121] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly, and 500 μL of aminosilane coupling agent N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0122] (2) immersing the zinc foil polished and cleaned with sandpaper in the homogeneous solution described in (1) for 5 hours to perform amino treatment on the surface of the zinc foil;
[0123] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 50 μL of glacial acetic acid and 500 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0124] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 5 hours to finally obtain a negative electrode material with a functional protective coating.
[0125] The application method of the negative electrode material refers to Example 1.
[0126] Example 12
[0127] 1. A method for preparing an aqueous zinc ion battery negative electrode material having a functional protective layer, comprising the following steps:
[0128] (1) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1 and stirred to mix evenly, and 1000 μL of aminosilane coupling agent N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane was measured and added to the above solution and stirred continuously until it became homogeneous;
[0129] (2) immersing the zinc foil polished and cleaned with sandpaper in the homogeneous solution described in (1) for 48 hours to perform amino treatment on the surface of the zinc foil;
[0130] (3) 45 mL of anhydrous methanol and 5 mL of deionized water were measured in a volume ratio of 9:1, and then 1000 μL of glacial acetic acid and 1000 μL of glycidyl methacrylate were added to the above solution and stirred continuously until homogeneous;
[0131] (4) The amination zinc foil in step (2) is transferred to the homogeneous solution in step (3) and immersed for 48 hours to finally obtain a negative electrode material with a functional protective coating.
[0132] The application method of the negative electrode material refers to Example 1.
[0133] Comparative Example 1
[0134] 1. Preparation of metal zinc foil negative electrode material without functional protective coating:
[0135] (1) After commercial metal zinc foil is polished with sandpaper, it is cleaned with ethanol and deionized water and dried to obtain a metal zinc foil negative electrode material without a functional protective coating.
[0136] 2. Example of application method for preparing symmetrical batteries:
[0137] (1) Slicing the negative electrode material without the functional protective coating to obtain a circular electrode sheet as the negative electrode of the aqueous zinc ion battery;
[0138] (2) MnO2, Supper P and polyvinylidene fluoride (PVDF) were taken in a mass ratio of 7:2:1, dissolved in an appropriate amount of N-methylpyrrolidone (NMP), and mixed evenly to obtain a slurry; the slurry was coated on a Ti foil, dried at 60°C under vacuum conditions for 24 hours, and then cut into circular electrode sheets as the positive electrode of an aqueous zinc ion battery;
[0139] The diameter of the negative electrode sheet can be selected to be 1 to 19 mm, and the diameter of the positive electrode sheet is slightly smaller than that of the negative electrode sheet;
[0140] (3) preparing a 2M ZnSO4 aqueous solution as an electrolyte for an aqueous zinc ion battery; and using a cellulose diaphragm as a diaphragm for the aqueous zinc ion battery;
[0141] (4) Place the 2025 battery positive electrode shell, negative electrode, cellulose separator, ZnSO4 electrolyte, negative electrode, nickel foam, and 2025 battery negative electrode shell in order to assemble into a symmetrical battery;
[0142] 3. Example of application method for preparing full battery:
[0143] (1) Prepare the battery components and prepare the electrolyte according to the steps in the method for preparing a symmetrical battery;
[0144] The difference is that the electrode on the positive side is a MnO2 electrode.
[0145] (2) Place the 2025 battery positive electrode shell, MnO2 positive electrode, cellulose separator, ZnSO4 electrolyte, negative electrode, nickel foam, and 2025 battery negative electrode shell in order to assemble a full battery.
[0146] Performance test and result evaluation:
[0147] 1. The following performance tests were performed on the negative electrode materials provided in Examples 1-12 and Comparative Example 1:
[0148] (1) Surface morphology characterization:
[0149] After being quenched by liquid nitrogen, the surface area is about 1cm 2 The test samples were freeze-dried and their surface morphology was observed by field emission scanning electron microscopy (FESEM).
[0150] (2) Analysis of surface elements and structures:
[0151] The metal zinc foil electrode with or without functional coating was cut into a surface area of about 1cm after being quenched with liquid nitrogen. 2 The test samples were freeze-dried and tested by X-ray photoelectron spectroscopy (XPS) to characterize their surface elements and structures.
[0152] (3) Electrochemical test:
[0153] Take the different electrode materials involved in each embodiment and comparative example, cut them into electrode sheets with a diameter of 14 mm, and test their linear voltammetric curves and it (time-voltage) curves under the three-electrode system. Then assemble them into symmetrical batteries, and test their cycle stability, i.e., time-voltage curve, on the Newwell battery test system. Then assemble them into full batteries, and test the self-discharge performance and cycle performance.
[0154] 2. Taking Example 11 and Comparative Example 1 as examples, Figure 1-Figure 5 The different performance test results of each product are shown in the table.
[0155] Figure 1is the surface morphology of the negative electrode; among them, (a) is the surface morphology of pure metal zinc foil (bare Zn) without functional protective coating; (b) is the surface morphology of the negative electrode (SG@Zn) with functional protective coating.
[0156] As can be seen from the figure, the surface of bare Zn is rough and uneven; the surface of SG@Zn has a dense and uniform micro-nanostructure coating.
[0157] Figure 2 High-resolution XPS spectrum of the negative electrode; among them, (a) Zn 2p, (b) O 1s, and (c) Si 2p.
[0158] As can be seen from the figure, the SG@Zn negative electrode is rich in zinc-philic functional groups C=O, and its binding energy is 532.8eV, which means that the SG@Zn negative electrode is conducive to more uniform adsorption of Zn 2+ , and the Si-O binding energy is 103.6eV. Its strong bonding effect proves that the coating has good bonding with the zinc substrate.
[0159] Figure 3 (a) Linear cyclic voltammetry curve and (b) IT curve measured for a symmetric battery.
[0160] As can be seen from the figure, (a) SG@Zn has a significant inhibitory effect on hydrogen evolution; (b) SG@Zn reaches the diffusion steady state in a faster time (130s), while the bare Zn negative electrode achieves steady state in a longer time (1000s), indicating that the SG@Zn negative electrode is conducive to promoting the uniform diffusion of zinc ions and the diffusion speed is faster.
[0161] Figure 4 Electrochemical performance of symmetrical cells assembled with negative electrodes; (a) bare Zn symmetrical cell at 2 mA cm -2 , 2mAh cm -2 Time-voltage curves of the SG@Zn symmetric battery at 2 mA cm -2 , 2mAh cm -2 The time-voltage curve below and the enlarged view of part (d).
[0162] from Figure 4 It can be seen that compared with (a) and (c), the voltage hysteresis of SG@Zn at the same time is about 40mV, which is much smaller than the voltage hysteresis of bare Zn negative electrode, indicating that it can more effectively inhibit dendrite growth. (b) and (d) further verify that SG@Zn battery has better cycle stability during the cycle process.
[0163] Figure 5The electrochemical performance of the full battery assembled with the negative electrode; among them, (a) the self-discharge performance of bare Zn, (b) the self-discharge performance of SG@Zn, and (c) the cycle curve at 1C rate (700 cycles).
[0164] As can be seen from the figure, compared with (a) and (b), after the SG@Zn electrode is charged to 1.8V, it is discharged to 0.8V after relaxation for 24h, and its coulombic efficiency is still as high as 97.2%, while the coulombic efficiency of the bare Zn negative electrode under the same conditions is only 76.5%, indicating that the reversibility of the SG@Zn full battery is better than that of pure metal zinc foil; (c) It can be seen that the first cycle capacity of the full battery of the SG@Zn electrode at 1C rate is 220mAh g -1 After 700 cycles, the capacity is about 194 mAh g -1 , the capacity retention rate is about 91.4%, which shows that the SG@Zn electrode has high capacity retention rate and good cycle stability.
[0165] Based on the above analysis, it can be seen that the negative electrode material with functional protective coating of the present invention is prepared by in-situ impregnation method, and the ultra-thin micro-nanostructure coating on the surface contains rich zinc-philic functional groups, which is conducive to the adsorption of zinc ions and can effectively promote the Zn 2+ The uniform nucleation and deposition of the negative electrode are beneficial to inhibiting the dendrite growth and the occurrence of side reactions such as corrosion and hydrogen evolution of the negative electrode. Therefore, it can be applied to the preparation of dendrite-free negative electrode and the performance improvement of its aqueous zinc-ion battery.
Claims
1. A method for preparing a negative electrode material for an aqueous zinc ion battery having a functional protective layer, characterized in that: The following steps are involved: Step 1, preparing a homogeneous solution I by adding appropriate amounts of anhydrous methanol, deionized water and silane coupling agent; Step 2, grinding the zinc foil with sandpaper, cleaning it with ethanol and deionized water, drying it, and then immersing it in the homogeneous solution I prepared in step 1 for a suitable time; Step 3, anhydrous methanol, deionized water and glycidyl methacrylate are mixed evenly, and glacial acetic acid is used as a catalyst, and stirred to form a homogeneous solution II; Step 4: The zinc foil aminated in step 2 is transferred and immersed in the homogeneous solution II for an appropriate period of time to obtain an aqueous zinc ion battery negative electrode material with a functional protective coating.
2. The preparation method according to claim 1, characterized in that: The volume ratio of anhydrous methanol to deionized water in step 1 is 9:
1.
3. The preparation method according to claim 1, characterized in that: The aminosilane coupling agent described in step 1 is one or more of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, and the amount used is 1-1000 μL.
4. The preparation method according to claim 1, characterized in that: The immersion time in step 2 is 0.1-48h.
5. The preparation method according to claim 1, characterized in that: In the step 3, the volume ratio of anhydrous methanol to deionized water is 9:1; the amount of glycidyl methacrylate is 1-1000 μL; and the amount of glacial acetic acid is 1-1000 μL.
6. The preparation method according to claim 1, characterized in that: In step 4, the immersion time is 0.1-48h.
7. The preparation method according to claim 1, characterized in that: The immersion time in step 2 and step 4 is equal.
8. An electrode sheet, characterized in that The electrode sheet is obtained by slicing the negative electrode material prepared by any one of claims 1 to 7.
9. An electrode sheet according to claim 8, characterized in that The electrode sheet is used as the negative electrode of an aqueous zinc ion battery.
10. A battery, characterized in that The battery comprises the electrode sheet according to claim 8.