Modified high-nickel ternary positive electrode material and preparation method thereof
The high-nickel ternary cathode material is coated through gamma ray co-irradiation grafting reaction and electrospinning technology, which solves the material's conductivity and cyclic stability problems, and improves the electrochemical performance and battery life.
Patent Information
- Application Number
- CN202411135446.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
AI Technical Summary
During the charging and discharging process, high-nickel ternary cathode materials are prone to cause cation mixing, lithium ion transmission rate is reduced, electronic conductivity is low, cycle stability is poor, and sensitive to moisture and carbon dioxide, resulting in a reduced battery cycle life.
2-acrylamide-2-methylpropanesulfonic acid is grafted with gel polymer by gamma ray co-irradiation grafting reaction to form a lithiated single-ion conductor polymer, and coated with high nickel through electrospinning technology The surface of the ternary positive electrode material forms a uniform cladding layer.
It improves the conductivity and cyclic stability of the material, enhances the electrochemical performance under high current density, and extends the cycle life of the battery.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the field of preparation of cathode materials for lithium-ion batteries, and in particular, to a single-ion conductor polymer-coated high-nickel ternary cathode material and a preparation method thereof. Background Art
[0002] With the development of the new energy industry, people have put forward higher requirements for the cruising range of new energy vehicles. Using cathode materials with higher specific capacity is an effective way to improve the cruising ability. High-nickel ternary materials with a nickel content of more than 80% (LiNi 1-x-y Co x Mn y O2, 0 < x + y ≤ 0.2) are currently known ultra-high specific capacity cathode materials that can meet the long cruising range requirements of new energy vehicles.
[0003] Although high-nickel ternary materials have advantages such as high theoretical specific capacity and low cost, with the increase of nickel content, the material is prone to cation mixing during charge and discharge, resulting in a decrease in the lithium ion transmission rate and ionic conductivity; at the same time, the ternary material belongs to transition metal oxides and has problems such as low bulk electronic conductivity. Therefore, during charge and discharge at a large current density, low ionic and electronic conductivities will lead to capacity loss. Another major problem restricting the commercial application of high-nickel ternary materials is poor cycle stability. High-nickel ternary materials are very sensitive to moisture and carbon dioxide in the air and are prone to form surface residual alkali. During the battery cycle, the organic electrolyte contacts the cathode material for a long time, resulting in the decomposition of the electrolyte and the dissolution of metals in the cathode material, leading to a reduction in the cycle life of the battery.
[0004] These instability problems of high-nickel ternary materials need to be solved urgently. Surface modification is regarded as an effective method. The current mainstream coating method is solid-phase coating, and the coating materials are mainly oxides, fluorides, phosphates, etc. However, most of these coating materials are electrochemically inert substances, which will reduce the ionic conductivity of the material. At the same time, the coating materials agglomerate on the surface of the material, resulting in uneven coating and even reducing the capacity performance of the material. How to coat the high-nickel ternary material to effectively improve the conductivity, rate performance and cycle stability of the material while improving the conductivity of the material has become a technical problem that needs to be solved urgently. Summary of the Invention
[0005] The purpose of the present invention is to provide a modified high-nickel ternary cathode material and a preparation method thereof. The modified high-nickel ternary cathode material can not only improve the conductivity of the material but also block the direct contact between the cathode material body and the electrolyte, effectively improving the rate performance and cycle stability of the material, and can solve the problems of capacity attenuation and poor cycle stability of the high-nickel ternary cathode material in the prior art at a large current density.
[0006] To achieve the above object, the present invention adopts the following technical solution: In a first aspect, the present invention provides a method for preparing a modified high-nickel ternary positive electrode material, comprising the following steps: S1. Under irradiation of gamma rays, 2-acrylamide-2-methylpropanesulfonic acid and a gel polymer are subjected to a co-irradiation grafting reaction in a solvent under an inert atmosphere to obtain a grafted polymer; The gel polymer is one or more of polyvinylidene fluoride-hexafluoropropylene, polyethylene oxide, polyvinyl chloride, polyvinylidene fluoride, and polymethyl acrylate; S2, immersing the graft polymer in an aqueous solution of a lithium salt for lithiation to obtain a lithiated graft polymer; S3. Coating the lithiated graft polymer on the surface of the high-nickel ternary positive electrode material to obtain the positive electrode material.
[0007] Based on the above technical scheme, the present invention first grafts 2-acrylamide-2-methylpropanesulfonic acid (AMPS) onto gel polymers such as polyvinylidene fluoride-hexafluoropropylene, polyethylene oxide, polyvinyl chloride, polyvinylidene fluoride, and polymethyl acrylate, and then lithifies to obtain a single ion conductor polymer with high ionic conductivity, and finally coats it on a high-nickel ternary positive electrode material. Among them, the coating on the high-nickel ternary positive electrode material is a single ion conductor polymer, which has a wide electrochemical window, can effectively promote the conduction of lithium ions, and improve the rate performance and cycle stability of the material.
[0008] In the above-mentioned method for preparing the modified high-nickel ternary positive electrode material, the mass of the gel polymer is 20% to 40% of the mass of the 2-acrylamide-2-methylpropanesulfonic acid, such as 20%, 30% or 40%; The 2-acrylamide-2-methylpropanesulfonic acid accounts for 30% to 50% of the total mass of (2-acrylamide-2-methylpropanesulfonic acid + solvent), such as 50%, 40% or 30%; The solvent is an aqueous solution of ethanol, preferably composed of ethanol and water in a volume ratio of 2:1; The gamma ray is Co 60 Source gamma rays; The irradiation dose is 40-60 kGy, such as 40 kGy, 50 kGy or 60 kGy.
[0009] In the above-mentioned method for preparing the modified high-nickel ternary positive electrode material, the co-irradiation grafting reaction is carried out in the presence of a 2-acrylamide-2-methylpropanesulfonic acid monomer self-polymerization inhibitor; Preferably, the monomer inhibitor is preferably copper sulfate, and its concentration in the co-irradiation grafting system is 0.002 - 0.006 mol / L (final concentration of copper sulfate), such as 0.002 mol / L, 0.004 mol / L or 0.006 mol / L.
[0010] In the above preparation method of the modified high-nickel ternary cathode material, the method further includes the following steps in step S1: after the co-irradiation grafting reaction is completed, wash the generated solid powder, centrifuge and dry it. The detergent consists of ethanol and water with a volume ratio of 1:2. The drying temperature is 60 - 80 °C, and the drying time is 4 - 6 h, such as drying for 6 h at 60 °C, drying for 5 h at 70 °C or drying for 4 h at 80 °C.
[0011] In the above preparation method of the modified high-nickel ternary cathode material, the concentration of the aqueous solution of the lithium salt is 1 - 3 mol / L, such as 1 mol / L, 2 mol / L or 3 mol / L; The lithium salt is one or more of lithium hydroxide, lithium carbonate, lithium acetate and lithium oxide; Every 1 g of the grafted polymer is immersed in 10 - 20 mL of the aqueous solution of the lithium salt, such as 10 mL, 15 mL, 20 mL; The immersion time is 24 - 28 h, such as 24 h, 28 h or 26 h; The method further includes the following steps in step S2: after the immersion is completed, wash to remove the residual lithium. The detergent consists of ethanol and water with a volume ratio of 1:2.
[0012] In the above preparation method of the modified high-nickel ternary cathode material, the high-nickel ternary cathode material is LiNi 1-x- y Co x Mn y O2, where 0 < x + y ≤ 0.2, such as LiNi 0.83 Co 0.06 Mn 0.11 O2, LiNi 0.88 Co 0.07 Mn 0.05 O2 or LiNi 0.93 Co 0.06 Mn 0.01 O2.
[0013] In the above preparation method of the modified high-nickel ternary cathode material, the coating step is as follows: dissolve the lithiated grafted polymer in an organic solvent as a spinning solution, and spray the spinning solution onto the surface of the high-nickel ternary cathode material by electrospinning, and dry it after spinning.
[0014] Compared with the dry ball milling mixing coating method, electrospinning is more conducive to the uniformity of the coating layer. At the same time, it can effectively control the thickness of the coating layer and further improve the electrochemical performance and cycle stability of high nickel ternary materials at higher current density.
[0015] Furthermore, in the electrospinning step, the lithiated grafted polymer accounts for 0.1% to 0.5% of the total mass of the high-nickel ternary material, such as 0.1%, 0.3% or 0.5%; The mass percentage of the lithiated graft polymer in the organic solvent is 12% to 20%, such as 12%, 16% or 20%; The conditions for the electrospinning are as follows: the spinning voltage is 12-16 kV, the spinning distance is 14-18 cm, and the spinning solution flow rate is 3.4-3.8 μL / min; exemplarily, the spinning voltage is 12 kV, the spinning distance is 14 cm, and the spinning solution flow rate is 3.4 μL / min; or, the spinning voltage is 14 kV, the spinning distance is 16 cm, and the spinning solution flow rate is 3.6 μL / min; or, the spinning voltage is 16 kV, the spinning distance is 18 cm, and the spinning solution flow rate is 3.8 μL / min.
[0016] The drying temperature is 60-100° C., and the drying time is 8-12 hours, such as drying at 60° C. for 12 hours, drying at 80° C. for 10 hours, or drying at 100° C. for 8 hours.
[0017] In a second aspect, the present invention provides a modified high-nickel ternary positive electrode material obtained by any of the preparation methods described above.
[0018] In a third aspect, the present invention provides a lithium-ion battery comprising the modified high-nickel ternary positive electrode material.
[0019] In the test example of the present invention, the lithium-ion battery is a button cell, metallic lithium is the counter electrode, the electrolyte is 1 mol / L LiPF6, and the solvent is a mixed solvent of EC, DEC and DMC in a volume ratio of 1:1:1.
[0020] The present invention has the following beneficial effects: The technical solution of the present invention is applied. First, the double-bond monomer AMPS with a lithiated sulfonic acid group is grafted onto a stable organic polymer skeleton using a co-radiation grafting technique, followed by lithiation to obtain a single-ion conductor polymer with high ionic conductivity, and finally coated on a high-nickel ternary positive electrode material by an electrostatic spinning technique. The synthesized single-ion conductor polymer has a wide electrochemical window and can effectively promote the conduction of lithium ions. Due to the ultra-high energy of ionizing radiation, the grafting process does not require harsh reaction conditions, nor does it require additional initiators or catalysts; compared with traditional atom transfer radical polymerization reactions, irradiation grafting is more convenient and controllable, and has a wide range of industrial application potential. At the same time, the electrostatic spinning technology can effectively control the thickness of the coating layer to form a thin and dense coating layer, improve the problem of low solid-phase diffusion efficiency of lithium ions at high rates, and improve the electrochemical performance and cycle stability of high-nickel ternary materials at higher current densities. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings: Figure 1 The SEM image of the single ion conductor polymer-coated high-nickel ternary positive electrode material prepared according to Example 1 of the present invention is shown.
[0022] Figure 2 The first cycle charge and discharge curve of the single ion conductor polymer-coated high nickel ternary positive electrode material prepared according to Example 1 of the present invention is shown. DETAILED DESCRIPTION
[0023] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.
[0024] The methods used in the following examples, unless otherwise specified, are all conventional methods, carried out according to the techniques or conditions described in the literature in the art or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources.
[0025] Example 1 This embodiment provides an AMPS Li-g-PVDF-HFP coated LiNi 0.83 Co 0.06 Mn 0.11 The preparation method of O2 ternary positive electrode material, the specific steps are as follows: (1) Weigh 3 g of 2-acrylamide-2-methylpropanesulfonic acid (AMPS) and dissolve it in 3 g of ethanol-water solution (the volume ratio of ethanol to water is 2:1), then add 0.6 g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) (molecular weight 500000), fully disperse by ultrasonication, and then add copper sulfate solution to control the final concentration of copper sulfate to 0.002 mol / L; send the above mixed solution into Co 60 The grafting was carried out by co-irradiation in a source γ-ray irradiation chamber. The grafting process was carried out in an argon atmosphere with a radiation dose of 40 kGy to obtain AMPS-grafted PVDF-HFP powder, which was recorded as AMPS-g-PVDF-HFP. The AMPS-g-PVDF-HFP powder was then washed three times in a water-ethanol solution (the volume ratio of ethanol to water was 1:2), centrifuged, and dried at 60 °C for 6 h; (2) The AMPS-g-PVDF-HFP powder was immersed in a 1 mol / L lithium hydroxide solution (1 g powder / 20 mL lithium hydroxide solution) for 28 h for lithiation, then rinsed three times with a water-ethanol solution (the volume ratio of water to ethanol was 2:1) and dried, and recorded as AMPS Li-g-PVDF-HFP; (3) Weigh 0.2 g AMPS Li-g-PVDF-HFP powder and dissolve it in 1.67 g NMP as the spinning solution. Transfer it to the needle tube and add 200 g LiNi 0.83 Co 0.06 Mn 0.11 The O2 ternary cathode material was spread on aluminum foil, the spinning voltage was set to 12 kV, the spinning distance was 14 cm, the spinning solution flow rate was 3.4 μL / min, the spinning solution was evenly spun on the ternary cathode material, and after spinning, it was transferred to an oven and dried at 60 ° C for 12 h to obtain AMPS Li-g-PVDF-HFP coated LiNi 0.83 Co 0.06 Mn 0.11 O2 ternary positive electrode material.
[0026] The obtained AMPS Li-g-PVDF-HFP coated LiNi 0.83 Co 0.06 Mn 0.11 The scanning electron microscopy results of O2 ternary cathode materials are as follows Figure 1 As shown, a uniform coating layer is formed on the surface of the material.
[0027] Example 2 This embodiment provides an AMPS Li-g-PEO coated LiNi 0.88 Co 0.07 Mn 0.05 The preparation method of O2 ternary positive electrode material, the specific steps are as follows: (1) Weigh 3 g of 2-acrylamide-2-methylpropanesulfonic acid (AMPS) and dissolve it in 4.5 g of ethanol-water solution (the volume ratio of ethanol to water is 2:1), then add 0.9 g of polyethylene oxide (PEO) (molecular weight 2000000), fully disperse by ultrasonication, and then add copper sulfate solution to control the final concentration of copper sulfate to 0.004 mol / L; send the above mixed solution into Co 60 The grafting was carried out by co-irradiation in a source γ-ray irradiation chamber. The grafting process was carried out in an argon atmosphere with a radiation dose of 50 kGy to obtain AMPS-grafted PEO powder, which was recorded as AMPS-g-PEO. The AMPS-g-PEO powder was then washed three times in a water-ethanol solution, centrifuged, and dried at 70 °C for 5 h. (2) The AMPS-g-PEO powder was immersed in a 2 mol / L lithium hydroxide solution (1 g powder / 15 mL lithium hydroxide solution) for 26 h for lithiation, then rinsed three times with a water-ethanol solution (the volume ratio of water to ethanol was 2:1) and dried, and recorded as AMPS Li-g-PEO; (3) Weigh 0.2 g AMPS Li-g-PEO powder and dissolve it in 1.23 g NMP as the spinning solution. Transfer it to the needle tube and add 66.67 g LiNi 0.88 Co 0.07 Mn 0.05 The O2 ternary cathode material was spread on aluminum foil, the spinning voltage was set to 14 kV, the spinning distance was 16 cm, the spinning solution flow rate was 3.6 μL / min, the spinning solution was evenly spun on the ternary cathode material, and after spinning, it was transferred to an oven and dried at 80 ° C for 10 h to obtain AMPS Li-g-PEO-coated LiNi 0.88 Co 0.07 Mn 0.05 O2 ternary positive electrode material.
[0028] Example 3 This embodiment provides an AMPS Li-g-PVC coated LiNi 0.93 Co 0.06 Mn 0.01 The preparation method of O2 ternary positive electrode material, the specific steps are as follows: (1) Weigh 3 g of 2-acrylamide-2-methylpropanesulfonic acid (AMPS) and dissolve it in 7 g of ethanol-water solution (the volume ratio of ethanol to water is 2:1), then add 1.2 g of polyvinyl chloride (PVC) (molecular weight 95000), fully disperse by ultrasonication, and then add copper sulfate solution to control the final concentration of copper sulfate to 0.006 mol / L; send the above mixed solution into Co 60The grafting was carried out by co-irradiation in a source γ-ray irradiation chamber. The grafting process was carried out in an argon atmosphere with a radiation dose of 60 kGy to obtain AMPS-grafted PVC powder, which was recorded as AMPS-g-PVC. The AMPS-g-PVC powder was then washed three times in a water-ethanol solution (the volume ratio of ethanol to water was 1:2), centrifuged, and dried at 80 °C for 4 h. (2) The AMPS-g-PVC powder was immersed in a 3 mol / L lithium hydroxide solution (1 g powder / 20 mL lithium hydroxide solution) for 24 h for lithiation, then rinsed three times with a water-ethanol solution (the volume ratio of water to ethanol was 2:1) and dried, and recorded as AMPS Li-g-PVC; (3) Weigh 0.2 g AMPS Li-g-PVC powder and dissolve it in 1.05 g NMP as the spinning solution. Transfer it to the needle tube and add 40 g LiNi 0.93 Co 0.06 Mn 0.01 The O2 ternary cathode material was spread on aluminum foil, the spinning voltage was set to 16 kV, the spinning distance was 18 cm, the spinning solution flow rate was 3.8 μL / mi, the spinning solution was evenly spun on the ternary cathode material, and after spinning, it was transferred to an oven and dried at 100 ° C for 8 h to obtain AMPS Li-g-PVC coated LiNi 0.93 Co 0.06 Mn 0.01 O2 ternary positive electrode material.
[0029] Comparative Example 1 Comparative Example 1 Compared with Example 1, the LiNi 0.83 Co 0.06 Mn 0.11 O2 ternary positive electrode material without any subsequent processing.
[0030] Comparative Example 2 Comparative Example 2 Compared with Example 1, the same raw materials as in Example 1 were used, and PVDF-HFP was not grafted with AMPS. Only PVDF-HFP was used for spinning and coating LiNi 0.83 Co 0.06 Mn 0.11 O2 ternary material, that is, 0.2g PVDF-HFP powder was weighed and dissolved in 1.67g NMP as the spinning solution, transferred to the needle tube, and 200g LiNi 0.83 Co 0.06 Mn 0.11The O2 ternary cathode material was spread on aluminum foil, the spinning voltage was set to 12 kV, the spinning distance was 14 cm, the spinning solution flow rate was 3.4 μL / min, the spinning solution was evenly spun on the ternary cathode material, and after spinning, it was transferred to an oven and dried at 60 ° C for 12 h to obtain PVDF-HFP-coated LiNi 0.83 Co 0.06 Mn 0.11 O2 ternary positive electrode material.
[0031] Comparative Example 3 Comparative Example 3 Compared with Example 1, the preparation method of AMPS-g-PVDF-HFP is consistent with that of Example 1, and the coating method adopts solid phase mixing of planetary ball mill, that is, AMPS-g-PVDF-HFP and LiNi 0.83 Co 0.06 Mn 0.11 The O2 ternary material was added to the ball mill, and zirconium balls were added at a ball-to-material ratio of 1:1. The materials were mixed at a frequency of 30 Hz for 3 h to obtain AMPS-g-PVDF-HFP coated LiNi 0.83 Co 0.06 Mn 0.11 O2 ternary material, subsequent treatment is the same as in Example 1.
[0032] Test Case Electrochemical performance characterization: The high nickel ternary cathode materials before and after coating modification were made into button batteries (the button battery model is CR2032, with metal lithium as the counter electrode, the conductive agent is Super P, the binder is PVDF, and the mass ratio of active material, conductive agent and binder is 90:5:5, the electrolyte is 1 mol / L LiPF6, and the solvent is a mixed solvent of EC, DEC and DMC with a volume ratio of 1:1:1), and the test voltage range is 2.8-4.35V. The first round of charge and discharge curves were tested at 0.2C, and the cycle curves were obtained at 1C charging and 1C discharging.
[0033] The electrochemical properties of the battery positive electrode products of Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Table 1.
[0034] The first charge-discharge curve of the modified high-nickel ternary cathode material prepared in Example 1 is as follows: Figure 2 shown.
[0035] Table 1 Electrochemical performance test results
[0036] It can be seen from the above that the high-nickel ternary material coated with a single-ion conductor polymer obtained in the embodiment of the present invention has a good coating effect, which can effectively improve the rate performance and cycle stability of the high-nickel ternary material. Compared with the embodiment, Comparative Example 1 did not undergo any coating modification, and the high-nickel ternary material body was directly in contact with the electrolyte during the cycle, with a low capacity and poor cycle; Comparative Example 2 only performed PVDF-HFP electrospinning coating treatment, which can isolate the material body from direct contact with the electrolyte, so the cycle performance is better than that of Comparative Example 1, but because AMPS with high ionic conductivity is not grafted, the rate performance is worse than that of Example 1; In Comparative Example 3, AMPS-g-PVDF-HFP coating only uses dry ball milling mixing, and the mixing effect is uneven, resulting in failure to completely cover the surface of the high-nickel ternary material, and the uniformity of the coating layer is slightly worse than that of Example 1, but it can still improve the electrochemical properties of the material.
[0037] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, can implement the present invention in a wider range under equivalent parameters, concentrations and conditions. Although the present invention provides specific embodiments, it should be understood that the present invention can be further improved. In a word, according to the principle of the present invention, the application is intended to include any changes, uses or improvements to the present invention, including departing from the disclosed scope in the application and the changes made with conventional techniques known in the art.
Claims
1. A method for preparing a modified high-nickel ternary positive electrode material, It is characterized in that The steps include: S1. Under irradiation of gamma rays, 2-acrylamide-2-methylpropanesulfonic acid and a gel polymer are subjected to a co-irradiation grafting reaction in a solvent under an inert atmosphere to obtain a grafted polymer; The gel polymer is one or more of polyvinylidene fluoride-hexafluoropropylene, polyethylene oxide, polyvinyl chloride, polyvinylidene fluoride, and polymethyl acrylate; S2, immersing the graft polymer in an aqueous solution of a lithium salt for lithiation to obtain a lithiated graft polymer; S3. Coating the lithiated graft polymer on the surface of the high-nickel ternary positive electrode material to obtain the modified high-nickel ternary positive electrode material.
2. The method for preparing the modified high-nickel ternary positive electrode material according to claim 1, Features: The mass of the gel polymer is 20% to 40% of the mass of the 2-acrylamide-2-methylpropanesulfonic acid; The 2-acrylamide-2-methylpropanesulfonic acid accounts for 30% to 50% of the total mass of (2-acrylamide-2-methylpropanesulfonic acid + solvent); The solvent is an aqueous solution of ethanol, preferably composed of ethanol and water in a volume ratio of 2:1; The gamma ray is Co 60 Source gamma rays; The irradiation dose is 40-60 kGy.
3. The method for preparing the modified high-nickel ternary positive electrode material according to claim 1, Features: The co-irradiation grafting reaction is carried out in the presence of a 2-acrylamide-2-methylpropanesulfonic acid monomer self-polymerization inhibitor; Preferably, the monomer self-polymerization inhibitor is copper sulfate, and its concentration in the co-irradiation grafting system is 0.002-0.006 mol / L.
4. The method for preparing the modified high-nickel ternary positive electrode material according to claim 1, Features: The method further comprises the following steps in step S1: after the co-irradiation grafting reaction is completed, washing the generated solid powder, centrifuging and drying, the detergent is composed of ethanol and water in a volume ratio of 1:2, the drying temperature is 60-80°C, and the drying time is 4-6h.
5. The method for preparing the modified high-nickel ternary positive electrode material according to claim 1, Features: The concentration of the aqueous solution of the lithium salt is 1 to 3 mol / L; The lithium salt is one or more of lithium hydroxide, lithium carbonate, lithium acetate and lithium oxide; Each 1g of the grafted polymer is immersed in 10-20mL of the aqueous solution of the lithium salt; The soaking time is 24 to 28 hours; The method further comprises the following steps in step S2: after the soaking is completed, washing to remove residual lithium, wherein the washing agent is composed of ethanol and water in a volume ratio of 1:
2.
6. The method for preparing the modified high-nickel ternary positive electrode material according to claim 1, Features: The high nickel ternary positive electrode material is LiNi 1-x-y Co x Mn y O 2 , where 0 <x+y≤0.2。 7. The method for preparing the modified high-nickel ternary positive electrode material according to claim 1, Features: The coating step is as follows: dissolving the lithiated graft polymer in an organic solvent as a spinning solution, spraying the spinning solution onto the surface of the high-nickel ternary positive electrode material by electrostatic spinning, and drying after spinning.
8. The method for preparing the modified high-nickel ternary positive electrode material according to claim 7, Features: In the electrospinning step, the lithiated grafted polymer accounts for 0.1% to 0.5% of the total mass of the high-nickel ternary material; The mass percentage of the lithiated graft polymer in the organic solvent is 12% to 20%; The electrospinning conditions are as follows: the spinning voltage is 12-16 kV, the spinning distance is 14-18 cm, and the spinning solution flow rate is 3.4-3.8 μL / min; The drying temperature is 60-100° C., and the drying time is 8-12 hours.
9. The modified high-nickel ternary positive electrode material obtained by the preparation method according to any one of claims 1 to 8.
10. A lithium ion battery comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, Features: The positive electrode plate includes the modified high-nickel ternary positive electrode material according to claim 9.
Citation Information
Patent Citations
Positive electrode material with low internal resistance for solid state lithium battery and preparation method of positive electrode material
CN108232138A
Blended polymer coated high-nickel ternary positive electrode material and preparation method thereof
CN110429269A
Lithium ion battery membrane, preparation method thereof and lithium ion battery
CN112635907A
Conductive coating, coating method and application
CN112864398A
Carbon-coated aluminum foil and preparation method thereof and lithium ion battery
CN112952106A