CoTAP / CoPc / AC catalytic flexible electrode, preparation method thereof and lithium / thionyl chloride soft package battery
Through the preparation of CoTAP/CoPc/AC catalytic flexible electrode, the problems of poor reversibility and short cycle life of lithium/thionyl chloride batteries are solved, high cycle life and stability are achieved, and the application field of lithium/thionyl chloride batteries is broadened. .
Patent Information
- Application Number
- CN202410987895.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing lithium/thionyl chloride batteries have poor reversibility, short cycle life and low safety, especially under the shuttle effect of chlorine, resulting in anode corrosion and reduced battery capacity. There are few researches on rechargeable lithium/thionyl chloride batteries, lacking stability Soft-pack battery with charge and discharge cycle capability.
The preparation method of CoTAP/CoPc/AC catalytic flexible electrode is adopted to form a porous structure by synthesizing activated carbon-supported cobalt phthalocyanine composite material rich in oxygen functional groups and tetrapyridoporphyrin/cobalt phthalocyanine/carbon composite catalytic material combined with acetylene black. Improve catalytic activity and cycling performance, and prepare flexible electrodes by roll pressing to enhance the stability and breadth of the battery.
It significantly improves the cycle life, reversible capacity and cycle stability of lithium/thionyl chloride batteries, reduces the internal resistance of the battery, enhances the reversibility of the charging reaction and the decomposition efficiency of the product, and fills the soft-packed lithium/thionyl chloride batteries. The technology gap has broadened the application field.
Smart Images

Figure CN118943277A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rechargeable lithium / thionyl chloride batteries, and specifically relates to a CoTAP / CoPc / AC catalytic flexible electrode and a preparation method thereof, and a lithium / thionyl chloride soft-pack battery. Background Art
[0002] With the rapid development of mobile devices, wearable technology and other applications, the demand for high-performance rechargeable batteries is becoming increasingly urgent. Lithium / thionyl chloride batteries have a discharge voltage platform of about 3.5V and a wide operating temperature range of -40 to 150°C, a high energy density of 710Wh / kg, and a storage life of up to 5-10 years. They can be used in special fields such as military, aerospace, and oil exploration. Among them: the existing lithium / chlorine battery based on thionyl chloride electrolyte adopts a high specific surface area and high pore positive electrode structure to achieve the storage of Cl2 in the reversible redox reaction for cyclic discharge (Zhu G, et al. Nature. 2021, 596 (7873), 525-530), however, chlorine is in gaseous state at room temperature, which increases the explosion hazard caused by the increase of internal voltage of the battery, and the safety performance is relatively low. In addition, the shuttle effect of chlorine corrodes the anode and reduces the battery capacity; in addition, due to the adsorption of Cl2 by porous carbon, the conversion of Cl2 to SOCl2 is severely reduced (Cl2 + S → SCl2, Cl2 + SO2 → SO2Cl2, SCl2 + SO2Cl2 → SOCl2) (Chen G, et al. J. Am. Chem. Soc. 2023, 145 (40), 22158-22167), which makes the rechargeable lithium / thionyl chloride battery reversible and limits the battery's cyclic application.
[0003] In addition, most of the existing research on lithium / thionyl chloride batteries is aimed at primary batteries, which have high operating costs and great environmental hazards, while research on rechargeable lithium / thionyl chloride batteries is rare; in addition, soft-pack batteries can provide larger capacity storage and can be applied to more scenarios through series and parallel connection. For example, soft-pack batteries can have a higher output voltage through series connection, so they can be used to power engines. Therefore, they are widely used in mobile devices and electric vehicles.
[0004] However, there are currently few reports on rechargeable lithium / thionyl chloride soft-pack batteries. Therefore, preparing a rechargeable lithium / thionyl chloride soft-pack battery that can undergo stable charge and discharge cycles will have great practical application value and has become a key difficulty in current research. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a flexible CoTAP / CoPc / AC catalytic electrode and a preparation method thereof and a lithium / thionyl chloride soft-pack battery, which improves the cycle life, reversible capacity and cycle stability of the lithium / thionyl chloride battery and broadens its application field.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The preparation method of CoTAP / CoPc / AC catalytic flexible electrode comprises the following steps:
[0008] Step 1, according to the mass ratio of (0.1-0.5):(1.2-4.1):(4.3-9.8):(1.5-4.3):(0.8-1.2), pyroasphalt activated carbon, phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate are mixed and ground to obtain a mixture A;
[0009] Step 2, placing the mixture A in a crucible and placing it in a muffle furnace, heating from room temperature to 130-150°C at a heating rate of 5-10°C / min in an air atmosphere, keeping warm for 0.5-1h, then heating to 260-280°C at a heating rate of 5-10°C / min, keeping warm for 2-4h, naturally cooling to room temperature, grinding, soaking, washing and drying in sequence to obtain an activated carbon-supported cobalt phthalocyanine composite material, recorded as CoPc / AC;
[0010] Step 3: Grind CoPc / AC, 2,3-pyridinedicarboxylic acid, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of (4.7-5.8):(0.9-3.8):(4.1-8.9):(0.9-4.6):(1.2-1.8) to obtain a mixture B;
[0011] Step 4, placing the mixture B in a crucible and placing it in a muffle furnace, heating from room temperature to 130-150°C at a heating rate of 5-10°C / min in an air atmosphere, keeping warm for 0.5-1h, then heating to 260-280°C at a heating rate of 5-10°C / min, keeping warm for 2-4h, naturally cooling to room temperature, grinding, soaking, washing and drying in sequence to obtain a tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalytic material, recorded as CoTAP / CoPc / AC;
[0012] Step 5, mixing a polytetrafluoroethylene emulsion having a solid content of 60% and deionized water in a mass ratio of (0.01-0.08):(1.2-3.0), stirring evenly, and obtaining a polytetrafluoroethylene dilution solution;
[0013] Step 6, acetylene black and CoTAP / CoPc / AC are mixed in a mass ratio of (6-10):(0.5-3), and stirred evenly in a dry powder state to obtain a mixture C, and then a polytetrafluoroethylene diluent is added to the mixture C in a mass ratio of 1:10, and then a trace amount of ethanol is added, and then ground evenly and dried to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;
[0014] Step 7: Soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol, take it out, gradually roll-press it, and dry it to obtain a CoTAP / CoPc / AC catalytic flexible electrode.
[0015] Furthermore, the soaking in step 2 and step 4 is to first soak in deionized water for at least 12 hours, then pour out the upper suspension, and then soak in new water, and repeat this process 3 times.
[0016] Furthermore, the cleaning in step 2 and step 4 is firstly cleaned with anhydrous ethanol for 2 to 4 times, and then cleaned with deionized water for 1 to 5 times.
[0017] Furthermore, the drying in step 2 and step 4 is carried out at 60-150° C. for 12-24 hours.
[0018] Furthermore, the drying in step 6 is performed by using a muffle furnace or an oven, heating from room temperature to 160-200° C. at a heating rate of 5-10° C. / min, and drying for 4-24 hours.
[0019] Furthermore, the step-by-step rolling process of step 7 is as follows: first, anhydrous ethanol is extruded with a small pressure using a roller press, then cut, and then pressed in sequence with working thicknesses of 1.75-2.0 mm, 1.25-1.5 mm, 0.75-1.0 mm, and 0.25-0.75 mm to obtain a CoTAP / CoPc / AC catalytic flexible electrode with a thickness of 0.25-0.75 mm.
[0020] Furthermore, the drying in step 7 is carried out at 50-130° C. for 2-24 hours.
[0021] A CoTAP / CoPc / AC catalytic flexible electrode.
[0022] A lithium / thionyl chloride soft-pack battery with a CoTAP / CoPc / AC catalytic flexible electrode as the positive electrode.
[0023] A lithium / thionyl chloride soft pack battery is assembled by the following method:
[0024] S1. First, use a roller press to press the CoTAP / CoPc / AC catalytic flexible electrode onto one side of the positive electrode current collector, connect the positive electrode metal tab to the upper end of the positive electrode current collector, and then place the positive electrode insulating separator onto the other side of the positive electrode current collector;
[0025] S2, using a metal lithium sheet as the negative electrode, placing the negative electrode current collector in close contact with one side of the metal lithium sheet, connecting a negative electrode metal tab to the upper end of the negative electrode current collector, and then placing a negative electrode insulating separator in close contact with the surface of the negative electrode current collector;
[0026] S3, covering the surface of the CoTAP / CoPc / AC catalytic flexible electrode with a battery separator, dripping electrolyte to soak the separator, and then placing the other side of the metal lithium sheet close to the separator, and then using a PTFE film to wrap around the periphery of the positive electrode insulating separator and the negative electrode insulating separator to obtain a battery core;
[0027] S4. Encapsulate the battery core in an aluminum-plastic shell to obtain a lithium / thionyl chloride soft-pack battery.
[0028] Compared with the prior art, the present invention has the following technical effects:
[0029] The present invention adopts a two-step method to synthesize the CoTAP / CoPc / AC catalytic material. The surface of the pitch coke activated carbon is rich in oxygen-containing functional groups, so that the catalytic materials CoPc and CoTAP can grow on the AC surface. On the one hand, CoTAP and CoPc have a conjugated effect, which significantly enhances the delocalization characteristics of the central ring π electrons, enhances the electron transfer performance, and has higher catalytic activity and longer cycle performance. On the other hand, the pyro-pitch activated carbon with high specific surface area and high pore structure increases the contact area between the catalytic material and SOCl2, so that the catalytic performance is fully released and participates in the chemical reaction during the battery charging and discharging process, so that the SOCl2 reaction is more sufficient. Therefore, the catalytic material CoTAP / CoPc / AC is combined with acetylene black with a conductive network, which not only reduces the internal resistance of the battery, significantly enhances the electron transmission capacity, but also enhances the decomposition efficiency of the chloride in the carbon coating in the charging reaction and the reversibility of the product, thereby improving the reversible capacity and cycle life of the battery.
[0030] The present invention prepares CoTAP / CoPc / AC catalytic flexible electrodes by rolling, which not only has the advantages of simple preparation, good stability, good uniformity, high yield, low energy consumption and good repeatability, but also solves the problem of uneven catalyst mixing caused by the existing slurry titration method for preparing the positive electrode of a rechargeable lithium thionyl chloride battery, so that the catalyst and the electrolyte can be fully in contact, thereby improving the average coulombic efficiency and cycle stability of the battery; in addition, the prepared flexible electrode can not only alleviate the potential danger of Cl2 causing the battery volume expansion during the charging and discharging process, but also is more suitable for various bending and folding shape changes. Compared with rigid electrodes, the application field is wider.
[0031] The lithium / thionyl chloride soft-pack battery assembled by the present invention using the CoTAP / CoPc / AC catalytic flexible electrode as the positive electrode not only has a high cycle life, a high reversible capacity and good cycle stability, but also fills the technical gap of soft-pack lithium / thionyl chloride batteries and further broadens the application field of lithium / thionyl chloride batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The technical roadmap for synthesizing the tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalytic material CoTAP / CoPc / AC of the present invention;
[0033] Figure 2 This is a physical photo of the CoTAP / CoPc / AC catalytic flexible electrode prepared in Example 1 of the present invention;
[0034] Figure 3 This is a physical photo of the lithium / thionyl chloride soft-pack battery assembled in Example 6 of the present invention;
[0035] Figure 4 This is a microscopic scanning image of the CoTAP / CoPc / AC catalytic flexible electrode prepared in Example 1 of the present invention;
[0036] Figure 5 This is a SEM electron microscope image of CoTAP / CoPc / AC prepared in Example 1 of the present invention;
[0037] Figure 6 FT-IR image of CoTAP / CoPc / AC prepared in Example 1 of the present invention;
[0038] Figure 7 This is a cycle performance diagram of the lithium / thionyl chloride soft-pack battery assembled in Example 6 of the present invention;
[0039] Figure 8 The charge and discharge curves of the lithium / thionyl chloride soft-pack battery assembled in Example 6 of the present invention;
[0040] Fig. 9 This is a schematic diagram of the structure of the lithium / thionyl chloride soft-pack battery assembled in Example 6 of the present invention. DETAILED DESCRIPTION
[0041] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.
[0042] In Examples 1 to 5, the technical route for synthesizing tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalyst CoTAP / CoPc / AC in Steps 1 to 4 is as follows: Figure 1 shown.
[0043] Example 1
[0044] A method for preparing a CoTAP / CoPc / AC catalytic flexible electrode comprises the following steps:
[0045] Step 1, mixing and grinding pyroasphalt activated carbon, phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate according to a mass ratio of 0.1:1.2:4.3:1.5:0.8 to obtain a mixture A;
[0046] Step 2, the mixture A is placed in a crucible and placed in a muffle furnace. In an air atmosphere, the temperature is increased from room temperature to 140°C at a heating rate of 10°C / min, and the mixture is kept warm for 0.5h. The temperature is then increased to 270°C at a heating rate of 10°C / min, and the mixture is kept warm for 2h. After naturally cooling to room temperature, the mixture is first ground, and then soaked in deionized water for at least 12h. The upper suspension is poured out, and the mixture is soaked in water again. This is repeated 3 times, followed by washing with anhydrous ethanol 3 times, and then washing with deionized water 3 times. Finally, the mixture is dried at 105°C for 12h to obtain an activated carbon-supported cobalt phthalocyanine composite material, recorded as CoPc / AC;
[0047] Step 3: Grind CoPc / AC, 2,3-pyridinedicarboxylic acid, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of 4.7:0.9:4.1:0.9:1.2 to obtain a mixture B;
[0048] Step 4, the mixture B is placed in a crucible and placed in a muffle furnace. In an air atmosphere, the temperature is increased from room temperature to 140°C at a heating rate of 10°C / min, and the temperature is kept for 0.5h. Then, the temperature is increased to 270°C at a heating rate of 10°C / min, and the temperature is kept for 2h. After naturally cooling to room temperature, the mixture is first ground into powder, and then soaked in deionized water for at least 12h, the upper suspension is poured out, and the water is changed again for soaking. This is repeated 3 times, followed by washing with anhydrous ethanol 3 times, and then washing with deionized water 3 times, and finally dried at 105°C for 12h to obtain a tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalytic material, recorded as CoTAP / CoPc / AC;
[0049] Step 5, mixing a polytetrafluoroethylene emulsion having a solid content of 60% and deionized water in a mass ratio of 0.0213:1.267, and stirring for 30 minutes to obtain a polytetrafluoroethylene dilution solution;
[0050] Step 6, according to a mass ratio of 9:1, acetylene black and CoTAP / CoPc / AC are put into a mortar, and stirred evenly in a dry powder state to obtain a mixture C, and then a polytetrafluoroethylene diluent is added to the mixture C according to a mass ratio of 1:10, and then a trace amount of ethanol is added to make the acetylene black and CoTAP / CoPc / AC bond faster, and after being ground into a mass, the mixture is transferred to a crucible, and the crucible is placed in a muffle furnace, and the temperature is increased from room temperature to 180°C at a heating rate of 10°C / min, and dried for 24 hours to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;
[0051] Step 7. Soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol for 10 minutes to make it sticky and not easy to disperse. After taking it out, wrap it with plastic wrap first, use a roller press to extrude the anhydrous ethanol with a small pressure, then cut it, and then remove the plastic wrap. Press it with a working thickness of 1.75mm, 1.25mm, 0.75mm and 0.25mm in turn, and dry it at 70°C for 24h to obtain a CoTAP / CoPc / AC catalytic flexible electrode with a thickness of 0.25mm.
[0052] Figure 4 The SEM image of the CoTAP / CoPc / AC catalytic flexible electrode prepared in Example 1 shows a porous structure composed of acetylene black nanoparticles and CoTAP / CoPc / AC catalytic materials, mainly composed of medium pores with a size of about 20nm to 2μm, in addition to a small number of small pores with a size of 2 to 10nm and large pores with a size of >2μm. The loose porous structure is conducive to the penetration of the electrolyte; in addition, the carbon nanoparticles are intertwined with each other to form a self-supporting structure. This stable porous self-supporting structure can not only allow the deposition and oxidation of LiCl during discharge and charge, but also ensure the stability of the electrode structure during the cycle.
[0053] Figure 5The SEM electron microscope image of the tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalytic material CoTAP / CoPc / AC prepared in Example 1 shows that the thin sheet of activated carbon AC is used as a growth substrate, and the rod-shaped cobalt phthalocyanine CoPc grows in situ on its surface. The surface of the activated carbon has rich oxygen-containing functional groups, which have a coordination effect on the cobalt phthalocyanine Co, N, O atoms, etc., and realizes the induced growth of CoPc. In addition, the in-situ grown CoPc has a nanoscale size. The template effect of the activated carbon makes the cobalt phthalocyanine catalytic material nanosized, increases its surface area, and provides more active sites, thereby realizing the catalytic Performance improvement; in addition, the micro-nano block-shaped CoTAP is gathered around the rod-shaped CoPc and AC, and is connected to the rod-shaped CoPc, and grows together on the activated carbon substrate. This is because the conjugated ring in the center of the CoTAP molecular structure produces a conjugated effect with the CoPc molecular macrocycle and the AC surface. This double conjugated molecular macrocycle structure can not only increase the delocalization characteristics of the π electrons in the center of the metal phthalocyanine molecular ring, but also has a more stable structure, which enhances the electron transfer ability of the catalytic material. Therefore, the CoTAP / CoPc / AC catalytic material has good structural stability and catalytic performance.
[0054] Figure 6 FT-IR image of the tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalyst CoTAP / CoPc / AC prepared in Example 1. -1 、1089cm -1 and 1390cm -1 The vibration peak at 1519 cm belongs to the conjugated phthalocyanine ring of CoTAP / CoPc / AC molecule. -1 Belongs to C=N stretching vibration, 1623cm -1 Belongs to C=C stretching vibration, 3415cm -1 It is attributed to the -OH group that absorbs water molecules. It proves that the CoTAP / CoPc / AC catalytic material was successfully synthesized.
[0055] The CoTAP / CoPc / AC catalytic flexible electrode prepared in Example 1 was cut into squares with a side length of 3 to 5 cm for assembly as follows: Figure 3 Lithium / thionyl chloride pouch cell shown.
[0056] Example 2
[0057] A method for preparing a CoTAP / CoPc / AC catalytic flexible electrode comprises the following steps:
[0058] Step 1, mixing and grinding pyroasphalt activated carbon, phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate according to a mass ratio of 0.21:1.9:5.6:2.2:0.9 to obtain a mixture A;
[0059] Step 2, the mixture A is placed in a crucible and placed in a muffle furnace, and in an air atmosphere, the temperature is increased from room temperature to 130°C at a heating rate of 5°C / min, and the temperature is kept for 1.0h, and then the temperature is increased to 280°C at a heating rate of 10°C / min, and the temperature is kept for 3h. After naturally cooling to room temperature, it is first ground, and then soaked in deionized water for at least 12h, the upper suspension is poured out, and the water is changed again for soaking, and this is repeated 3 times, followed by washing with anhydrous ethanol 3 times, and then washing with deionized water 2 times, and finally drying at 60°C for 18h to obtain an activated carbon-supported cobalt phthalocyanine composite material, recorded as CoPc / AC;
[0060] Step 3: Grind CoPc / AC, 2,3-pyridinedicarboxylic acid, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of 5.0:1.6:5.3:1.8:1.3 to obtain a mixture B;
[0061] Step 4, the mixture B is placed in a crucible and placed in a muffle furnace. In an air atmosphere, the temperature is increased from room temperature to 130°C at a heating rate of 5°C / min, and the temperature is kept for 1.0h. Then, the temperature is increased to 280°C at a heating rate of 10°C / min, and the temperature is kept for 3h. After naturally cooling to room temperature, the mixture is first ground into powder, and then soaked in deionized water for at least 12h, the upper suspension is poured out, and the water is changed again for soaking. This is repeated 3 times, followed by washing with anhydrous ethanol 3 times, and then washing with deionized water 2 times, and finally drying at 60°C for 18h to obtain a tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalytic material, recorded as CoTAP / CoPc / AC;
[0062] Step 5, mixing a polytetrafluoroethylene emulsion having a solid content of 60% and deionized water in a mass ratio of 0.03:1.5, and stirring for 30 minutes to obtain a polytetrafluoroethylene dilution solution;
[0063] Step 6, according to the mass ratio of 8.8:1.2, acetylene black and CoTAP / CoPc / AC were put into a mortar, and stirred evenly in a dry powder state to obtain a mixture C, and then a polytetrafluoroethylene diluent was added to the mixture C according to the mass ratio of 1:10, and then a trace amount of ethanol was added to make the acetylene black and CoTAP / CoPc / AC bond faster, and after being ground into a mass, the mixture was transferred to a crucible, and the crucible was placed in a muffle furnace, and the temperature was raised from room temperature to 190°C at a heating rate of 5°C / min, and dried for 20 hours to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;
[0064] Step 7. Soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol for 6 hours to make it sticky and not easy to disperse. After taking it out, wrap it with plastic wrap first, use a roller press to extrude the anhydrous ethanol with a small pressure, then cut it, and then remove the plastic wrap. Press it with a working thickness of 2.0 mm, 1.5 mm, 1.0 mm and 0.75 mm in turn, and dry it at 50°C for 24 hours to obtain a CoTAP / CoPc / AC catalytic flexible electrode with a thickness of 0.75 mm.
[0065] Example 3
[0066] A method for preparing a CoTAP / CoPc / AC catalytic flexible electrode comprises the following steps:
[0067] Step 1, mixing and grinding pyroasphalt activated carbon, phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate according to a mass ratio of 0.3:2.7:7.0:2.9:1.0 to obtain a mixture A;
[0068] Step 2, placing the mixture A in a crucible and placing it in a muffle furnace, heating from room temperature to 150°C at a heating rate of 5°C / min in an air atmosphere, keeping warm for 0.5h, and then heating to 260°C at a heating rate of 5°C / min, keeping warm for 4h, naturally cooling to room temperature, first grinding, then soaking in deionized water for at least 12h, pouring out the upper suspension, and re-immersing in water, repeating this 3 times, then washing with anhydrous ethanol 2 times, then washing with deionized water 5 times, and finally drying at 150°C for 12h to obtain an activated carbon-supported cobalt phthalocyanine composite material, recorded as CoPc / AC;
[0069] Step 3, according to the mass ratio of 5.3:2.4:6.5:2.8:1.5, CoPc / AC, 2,3-pyridinedicarboxylic acid, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate were fully ground to obtain a mixture B;
[0070] Step 4, the mixture B is placed in a crucible and placed in a muffle furnace. In an air atmosphere, the temperature is increased from room temperature to 150°C at a heating rate of 5°C / min, and the mixture is kept warm for 0.5h. The temperature is then increased to 260°C at a heating rate of 5°C / min, and the mixture is kept warm for 4h. After naturally cooling to room temperature, the mixture is first ground into powder, and then soaked in deionized water for at least 12h. The upper suspension is poured out, and the mixture is soaked in water again. This is repeated 3 times, followed by washing with anhydrous ethanol 2 times, and then washing with deionized water 5 times. Finally, the mixture is dried at 150°C for 12h to obtain a tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalytic material, recorded as CoTAP / CoPc / AC;
[0071] Step 5, mixing a polytetrafluoroethylene emulsion having a solid content of 60% and deionized water in a mass ratio of 0.01:1.8, and stirring for 30 minutes to obtain a polytetrafluoroethylene dilution solution;
[0072] Step 6, according to the mass ratio of 6:0.5, acetylene black and CoTAP / CoPc / AC were put into a mortar, and stirred evenly in a dry powder state to obtain a mixture C, and then a polytetrafluoroethylene diluent was added to the mixture C according to the mass ratio of 1:10, and then a trace amount of ethanol was added to make the acetylene black and CoTAP / CoPc / AC bond faster, and after being ground into a mass, the mixture was transferred to a crucible, and the crucible was placed in an oven, and the temperature was raised from room temperature to 160°C at a heating rate of 8°C / min, and dried for 18 hours to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;
[0073] Step 7. Soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol for 12 hours to make it sticky and not easy to disperse. After taking it out, wrap it with plastic wrap first, use a roller press to extrude the anhydrous ethanol with a small pressure, then cut it, and then remove the plastic wrap. Press it with a working thickness of 1.75 mm, 1.5 mm, 1.0 mm and 0.75 mm in turn, and dry it at 100 ° C for 10 hours to obtain a CoTAP / CoPc / AC catalytic flexible electrode with a thickness of 0.75 mm.
[0074] Example 4
[0075] A method for preparing a CoTAP / CoPc / AC catalytic flexible electrode comprises the following steps:
[0076] Step 1, mixing and grinding pyroasphalt activated carbon, phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of 0.4:3.5:8.5:3.5:1.1 to obtain a mixture A;
[0077] Step 2, the mixture A is placed in a crucible and placed in a muffle furnace, and in an air atmosphere, the temperature is increased from room temperature to 140°C at a heating rate of 8°C / min, and the temperature is kept for 1.0h, and then the temperature is increased to 280°C at a heating rate of 8°C / min, and the temperature is kept for 3h. After naturally cooling to room temperature, it is first ground, and then soaked in deionized water for at least 12h, the upper suspension is poured out, and the water is changed again for soaking, and this is repeated 3 times, followed by washing with anhydrous ethanol 4 times, and then washing with deionized water once, and finally drying at 80°C for 24h to obtain an activated carbon-supported cobalt phthalocyanine composite material, recorded as CoPc / AC;
[0078] Step 3: Grind CoPc / AC, 2,3-pyridinedicarboxylic acid, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of 5.5:3.0:7.5:3.5:1.6 to obtain a mixture B;
[0079] Step 4, the mixture B is placed in a crucible and placed in a muffle furnace. In an air atmosphere, the temperature is increased from room temperature to 140°C at a heating rate of 8°C / min, and the temperature is kept for 1.0h. Then, the temperature is increased to 280°C at a heating rate of 8°C / min, and the temperature is kept for 3h. After naturally cooling to room temperature, the mixture is first ground into powder, and then soaked in deionized water for at least 12h, the upper suspension is poured out, and the water is changed again for soaking. This is repeated 3 times, followed by washing with anhydrous ethanol 4 times, and then washing with deionized water once, and finally drying at 80°C for 24h to obtain a tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalytic material, recorded as CoTAP / CoPc / AC;
[0080] Step 5, mixing a polytetrafluoroethylene emulsion having a solid content of 60% and deionized water in a mass ratio of (0.01-0.08):(1.2-3.0), stirring for 30 minutes, and obtaining a polytetrafluoroethylene dilution solution;
[0081] Step 6, according to a mass ratio of 7:2, acetylene black and CoTAP / CoPc / AC are put into a mortar, and stirred evenly in a dry powder state to obtain a mixture C, and then a polytetrafluoroethylene diluent is added to the mixture C according to a mass ratio of 1:10, and then a trace amount of ethanol is added to make the acetylene black and CoTAP / CoPc / AC bond faster, and after being ground into a mass, the mixture is transferred to a crucible, and the crucible is placed in an oven, and the temperature is increased from room temperature to 170°C at a heating rate of 10°C / min, and dried for 10 hours to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;
[0082] Step 7. Soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol for 18 hours to make it sticky and not easy to disperse. After taking it out, wrap it with plastic wrap first, use a roller press to extrude the anhydrous ethanol with a small pressure, then cut it, and then remove the plastic wrap. Press it with a working thickness of 2.0 mm, 1.5 mm, 1.0 mm and 0.75 mm in turn, and dry it at 130°C for 2 hours to obtain a CoTAP / CoPc / AC catalytic flexible electrode with a thickness of 0.75 mm.
[0083] Example 5
[0084] A method for preparing a CoTAP / CoPc / AC catalytic flexible electrode comprises the following steps:
[0085] Step 1, mixing and grinding pyroasphalt activated carbon, phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate according to a mass ratio of 0.5:4.1:9.8:4.3:1.2 to obtain a mixture A;
[0086] Step 2, the mixture A is placed in a crucible and placed in a muffle furnace, and in an air atmosphere, the temperature is increased from room temperature to 150°C at a heating rate of 6°C / min, and the temperature is kept for 1.0h, and then the temperature is increased to 270°C at a heating rate of 6°C / min, and the temperature is kept for 2h. After naturally cooling to room temperature, it is first ground, and then soaked in deionized water for at least 12h, the upper suspension is poured out, and the water is changed again for soaking, and this is repeated 3 times, followed by washing with anhydrous ethanol 2 times, and then washing with deionized water 4 times, and finally dried at 120°C for 20h to obtain an activated carbon-supported cobalt phthalocyanine composite material, recorded as CoPc / AC;
[0087] Step 3, according to the mass ratio of 5.8:3.8:8.9:4.6:1.8, CoPc / AC, 2,3-pyridinedicarboxylic acid, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate were fully ground to obtain a mixture B;
[0088] Step 4, the mixture B is placed in a crucible and placed in a muffle furnace. In an air atmosphere, the temperature is increased from room temperature to 150°C at a heating rate of 6°C / min, and the mixture is kept warm for 1.0h. The temperature is then increased to 270°C at a heating rate of 6°C / min, and the mixture is kept warm for 2h. After naturally cooling to room temperature, the mixture is first ground into powder, and then soaked in deionized water for at least 12h. The upper suspension is poured out, and the mixture is soaked in water again. This is repeated 3 times, and then the mixture is washed with anhydrous ethanol twice, and then washed with deionized water 4 times. Finally, the mixture is dried at 120°C for 20h to obtain a tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalytic material, recorded as CoTAP / CoPc / AC;
[0089] Step 5, mixing a polytetrafluoroethylene emulsion having a solid content of 60% and deionized water in a mass ratio of 0.08:3.0, stirring for 30 minutes, to obtain a polytetrafluoroethylene dilution solution;
[0090] Step 6, according to the mass ratio of 10:3, acetylene black and CoTAP / CoPc / AC are put into a mortar, and stirred evenly in a dry powder state to obtain a mixture C, and then a polytetrafluoroethylene diluent is added to the mixture C according to the mass ratio of 1:10, and then a trace amount of ethanol is added to make the acetylene black and CoTAP / CoPc / AC bond faster, and after being ground into a mass, the mixture is transferred to a crucible, and the crucible is placed in an oven, and the temperature is increased from room temperature to 170°C at a heating rate of 10°C / min, and dried for 10 hours to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture;
[0091] Step 7. Soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol for 24 hours to make it sticky and not easy to disperse. After taking it out, wrap it with plastic wrap first, use a roller press to extrude the anhydrous ethanol with a small pressure, then cut it, and then remove the plastic wrap. Press it with a working thickness of 1.75mm, 1.25mm, 0.75mm and 0.5mm in turn, and dry it at 80°C for 18 hours to obtain a CoTAP / CoPc / AC catalytic flexible electrode with a thickness of 0.5mm.
[0092] Example 6
[0093] like Fig. 9 As shown, a method for assembling a lithium / thionyl chloride soft-pack battery comprises the following steps:
[0094] S1. Select two square nickel foam sheets with a side length of 4 cm as the positive electrode current collector and the negative electrode current collector respectively, and select two long strip nickel foam sheets as the positive electrode metal tab and the negative electrode metal tab respectively;
[0095] S2. Cut the square CoTAP / CoPc / AC catalytic flexible electrode prepared in Example 1 into Figure 2 The square with a side length of 4 cm shown is used to press the CoTAP / CoPc / AC catalytic flexible electrode with a side length of 4 cm onto the surface of one side of the positive electrode current collector using a roller press to obtain a positive electrode sheet with a thickness of 1 to 2 mm. The positive electrode nickel tab is externally connected to the upper end of the positive electrode current collector, and then the PEFE insulating separator is pressed onto the surface of the other side of the positive electrode current collector as a barrier to reduce the corrosion of the electrolyte to the battery;
[0096] S3, using a metal lithium sheet with a side length of 4 cm as the negative electrode, placing the negative electrode current collector close to one side of the metal lithium sheet, connecting the negative electrode nickel tab to the upper end of the negative electrode current collector, and then pressing the PEFE insulating separator to the surface of the negative electrode current collector;
[0097] S4. A square glass fiber separator with a side length of 5 cm is used as a battery separator. Two pieces of battery separators are covered on the surface of the CoTAP / CoPc / AC catalytic flexible electrode, and the electrolyte is dripped to infiltrate the separator. Then, the other side of the metal lithium sheet is placed close to the battery separator. Then, a PTFE film is used to wrap around the periphery of the positive electrode insulating separator and the negative electrode insulating separator to prevent the electrolyte from volatilizing and corroding the inside of the battery, thereby obtaining a battery core.
[0098] S5, aligning two square pieces of aluminum-plastic paper with a side length of 7 cm, and using a plastic sealing machine to seal three sides thereof, leaving the remaining side open, to obtain an aluminum-plastic shell for encapsulating the battery core;
[0099] S6, encapsulate the battery core in the aluminum-plastic shell to obtain Figure 3Lithium / thionyl chloride pouch cell shown.
[0100] In the process of assembling lithium / thionyl chloride soft-pack batteries, the metal sheets used as positive electrode current collectors and negative electrode current collectors include but are not limited to foam nickel sheets, and can also be aluminum sheets or copper sheets, and the material of the positive electrode metal tabs includes but is not limited to nickel, and can also be aluminum or copper.
[0101] In addition, the dimensions of the positive electrode current collector, square CoTAP / CoPc / AC catalytic flexible electrode, metal lithium sheet, cathode current collector, battery separator and aluminum-plastic casing can be designed according to actual needs.
[0102] Figure 7 The cycle performance diagram of the lithium / thionyl chloride soft-pack battery assembled in Example 6 shows that the lithium / thionyl chloride soft-pack battery assembled with CoTAP / CoPc / AC catalytic flexible electrode can achieve 10 stable cycles and has a stable coulombic efficiency. The initial low coulombic efficiency may be due to the activation process of the battery in the initial stage. After the activation stage, the battery coulombic efficiency begins to stabilize. Since CoTAP / CoPc / AC improves electron transfer, the battery can achieve 10 stable cycles at 1 mA cm -2 Under high current density, the battery and electrodes remain intact during the charge and discharge process and are able to cycle stably, with an average coulombic efficiency of >93.5%, providing a cumulative reversible capacity of more than 90 mAh.
[0103] Figure 8 The charge and discharge curves of the lithium / thionyl chloride soft-pack battery assembled in Example 6 show that the main charging platform voltage of the lithium / thionyl chloride soft-pack battery assembled using CoTAP / CoPc / AC catalytic flexible electrodes is 3.95 V, corresponding to the partial oxidation of LiCl during the charging process, and the charging terminal voltage rises to 4.05 V, which is related to the occurrence of additional oxidation; the main discharge voltage platform of the lithium / thionyl chloride soft-pack battery is 3.5 V, corresponding to the reduction of SOCl2, indicating that the lithium / thionyl chloride soft-pack battery assembled in Example 6 can effectively reduce the corrosion of the electrolyte to the inside of the battery and has a stable charging and discharging curve platform.
Claims
1. A method for preparing a CoTAP / CoPc / AC catalytic flexible electrode, characterized in that: The steps include: Step 1, according to the mass ratio of (0.1-0.5):(1.2-4.1):(4.3-9.8):(1.5-4.3):(0.8-1.2), pyroasphalt activated carbon, phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate are mixed and ground to obtain a mixture A; Step 2, placing the mixture A in a crucible and placing it in a muffle furnace, heating from room temperature to 130-150°C at a heating rate of 5-10°C / min in an air atmosphere, keeping warm for 0.5-1h, then heating to 260-280°C at a heating rate of 5-10°C / min, keeping warm for 2-4h, naturally cooling to room temperature, grinding, soaking, washing and drying in sequence to obtain an activated carbon-supported cobalt phthalocyanine composite material, recorded as CoPc / AC; Step 3: Grind CoPc / AC, 2,3-pyridinedicarboxylic acid, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of (4.7-5.8):(0.9-3.8):(4.1-8.9):(0.9-4.6):(1.2-1.8) to obtain a mixture B; Step 4, placing the mixture B in a crucible and placing it in a muffle furnace, heating from room temperature to 130-150°C at a heating rate of 5-10°C / min in an air atmosphere, keeping warm for 0.5-1h, then heating to 260-280°C at a heating rate of 5-10°C / min, keeping warm for 2-4h, naturally cooling to room temperature, grinding, soaking, washing and drying in sequence to obtain a tetrapyridoporphyrin / cobalt phthalocyanine / carbon composite catalytic material, recorded as CoTAP / CoPc / AC; Step 5, according to the mass ratio of (0.01-0.08): (1.2-3.0), a polytetrafluoroethylene emulsion with a solid content of 60% and deionized water are mixed and stirred evenly to obtain a polytetrafluoroethylene dilution solution; Step 6, acetylene black and CoTAP / CoPc / AC are mixed in a mass ratio of (6-10):(0.5-3), and stirred evenly in a dry powder state to obtain a mixture C, and then a polytetrafluoroethylene diluent is added to the mixture C in a mass ratio of 1:10, and then a trace amount of ethanol is added, and then ground evenly and dried to obtain a polytetrafluoroethylene cross-linked composite carbon cathode mixture; Step 7: Soak the polytetrafluoroethylene cross-linked composite carbon cathode mixture in anhydrous ethanol, take it out, gradually roll-press it, and dry it to obtain a CoTAP / CoPc / AC catalytic flexible electrode.
2. The method for preparing the CoTAP / CoPc / AC catalytic flexible electrode according to claim 1, characterized in that: The soaking in step 2 and step 4 is to first soak in deionized water for at least 12 hours, then pour out the upper suspension, and then soak in new water, and repeat this process 3 times.
3. The method for preparing the CoTAP / CoPc / AC catalytic flexible electrode according to claim 1, characterized in that: The cleaning in step 2 and step 4 is firstly cleaning with anhydrous ethanol for 2 to 4 times, and then cleaning with deionized water for 1 to 5 times.
4. The method for preparing the CoTAP / CoPc / AC catalytic flexible electrode according to claim 1, characterized in that: The drying in step 2 and step 4 is carried out at 60-150° C. for 12-24 hours.
5. The method for preparing the CoTAP / CoPc / AC catalytic flexible electrode according to claim 1, characterized in that: The drying in step 6 is performed by using a muffle furnace or an oven, heating from room temperature to 160-200° C. at a heating rate of 5-10° C. / min, and drying for 4-24 hours.
6. The method for preparing the CoTAP / CoPc / AC catalytic flexible electrode according to claim 1, characterized in that: The step-by-step rolling process of step 7 is as follows: first, anhydrous ethanol is extruded with a small pressure using a roller press, then cut, and then pressed in sequence with working thicknesses of 1.75-2.0 mm, 1.25-1.5 mm, 0.75-1.0 mm, and 0.25-0.75 mm to obtain a CoTAP / CoPc / AC catalytic flexible electrode with a thickness of 0.25-0.75 mm.
7. The method for preparing the CoTAP / CoPc / AC catalytic flexible electrode according to claim 1, characterized in that: The drying in step 7 is performed at 50-130° C. for 2-24 hours.
8. A CoTAP / CoPc / AC catalytic flexible electrode prepared by the method of any one of claims 1 to 7.
9. A lithium / thionyl chloride soft pack battery, characterized in that: The CoTAP / CoPc / AC catalytic flexible electrode described in claim 8 is used as the positive electrode.
10. The lithium / thionyl chloride soft pack battery according to claim 9, characterized in that: Assembled by the following method: S1. First, use a roller press to press the CoTAP / CoPc / AC catalytic flexible electrode onto one side of the positive electrode current collector, connect the positive electrode metal tab to the upper end of the positive electrode current collector, and then place the positive electrode insulating separator onto the other side of the positive electrode current collector; S2, using a metal lithium sheet as the negative electrode, placing the negative electrode current collector in close contact with one side of the metal lithium sheet, connecting a negative electrode metal tab to the upper end of the negative electrode current collector, and then placing a negative electrode insulating separator in close contact with the surface of the negative electrode current collector; S3, covering the surface of the CoTAP / CoPc / AC catalytic flexible electrode with a battery separator, dripping electrolyte to soak the separator, and then placing the other side of the metal lithium sheet close to the separator, and then using a PTFE film to wrap around the periphery of the positive electrode insulating separator and the negative electrode insulating separator to obtain a battery core; S4. Encapsulate the battery core in an aluminum-plastic shell to obtain a lithium / thionyl chloride soft-pack battery.