Solid-state thick electrode, preparation method and solid-state battery
By using stacked electrolyte layers and composite positive electrode layers in solid-state thick electrodes, the design of gradually reducing the mass proportion of active substances is solved, and the problems of complex design of solid-state thick electrodes and difficulty in improving ionic conductivity are achieved, and the electrochemical performance is improved and process simplification.
Patent Information
- Application Number
- CN202411033670.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing solid-state thick electrodes have complex designs, and the ionic conductivity cannot be effectively improved. In the point-to-point contact mode of electrolytes, active substances, and conductive agents in all-solid lithium-ion batteries, the conductivity is not as good as that of liquid batteries.
The solid electrolyte layer and composite positive electrode layer are arranged stacked. The composite positive electrode layer includes multiple sub-layers. The mass proportion of active substances is gradually reduced, and the proportion of electrolytes and conductive agents is optimized. The thick electrode is formed by pressing, which simplifies the process flow and improves the active substances. utilization rate.
The process flow is simplified and the electrochemical performance is improved, especially under thick solid electrodes, which significantly improves the first discharge capacity, circulation capacity and capacity retention rate of the battery.
Smart Images

Figure CN118943291A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery electrode materials, and in particular relates to a solid thick electrode, a preparation method and a solid-state battery. Background Art
[0002] Increasing the thickness of the electrode is a relatively direct way to improve the energy density of the battery. However, there is a problem of limited ion / electron transfer kinetics in thick electrodes. Optimizing the design of thick electrodes is currently the key to improving the energy density of batteries. Although there have been some reports on the design of thick electrodes, they are basically the design methods of thick electrodes in traditional liquid lithium-ion batteries, such as: constructing a three-dimensional conductive network framework, designing a pore structure with low tortuosity, etc. However, there are very few designs for solid thick electrodes.
[0003] Nowadays, the development of all-solid-state lithium-ion batteries is extremely rapid. In terms of the structure of the two batteries, compared with traditional liquid lithium-ion batteries, the solid electrolyte in all-solid-state lithium-ion batteries replaces the role of electrolyte and diaphragm. In addition, unlike traditional liquid lithium-ion batteries, the electrolyte has wetting properties that can achieve good ion conductivity, while the active material, electrolyte, and conductive agent in the composite positive electrode of the solid-state battery are in point-to-point contact mode, and the conductivity is not as good as that of liquid batteries. Therefore, the electrode design of solid-state electrodes is completely different from that of liquid batteries.
[0004] At present, the research on solid-state thick electrodes mainly includes: 1. Trying to improve the ion transport performance of thick electrodes by improving the ionic conductivity of electrolytes; however, more and more electrolytes have reached 10 -2 The lithium ion conductivity level of S / cm is basically close to that of the electrolyte. It is no longer realistic to rely on improving the ion conductivity to improve the ion conduction of the electrode. 2. Design a porous and dense structural framework to increase the loading capacity; however, constructing a porous / dense structural framework to improve the dynamics of the composite electrode and then prepare a thick electrode has problems such as complex design, high process requirements, and high cost. Since solid-state batteries rely on external pressure to achieve good solid-solid contact, many frame structure designs have very small forces in solid-state batteries, so the design of the pores also needs to take into account the damage to the pores caused by pressure. Summary of the invention
[0005] In view of the above deficiencies in the prior art, the object of the present invention is to provide a solid thick electrode, a preparation method and a solid-state battery to solve the problems that the existing solid thick electrode has a complex design and the ion conductivity cannot be effectively improved.
[0006] To achieve the above object, the present invention is implemented through the following technical solutions: In a first aspect, the present invention provides a solid thick electrode, comprising a stacked solid electrolyte layer and a composite positive electrode layer; wherein the composite positive electrode layer comprises a plurality of sublayers stacked in sequence; away from the solid electrolyte layer, the mass proportion of active materials in the plurality of sublayers gradually decreases.
[0007] Preferably, the number of sublayers is n, the sublayer close to the solid electrolyte layer is recorded as the first layer, and the sublayer far from the solid electrolyte layer is recorded as the nth layer; From the first layer to the nth layer, the mass proportion of the active material in each sub-layer is recorded as X1, X2, X3, ...X n The mass proportion of the electrolyte in each sublayer is recorded as Y1, Y2, Y3, ...Y n ; Among them, X1>X2>X3>…>X n , Y1<Y2<Y3<…<Y n .
[0008] Preferably, the mass proportion of the conductive agent in the multiple sub-layers is the same.
[0009] Preferably, the composite positive electrode layer includes an active material, an electrolyte and a conductive agent; the mass proportion of the active material is 50-80%, the mass proportion of the electrolyte is 18-48%, and the rest is the conductive agent.
[0010] In the present invention, the active material used may be any positive electrode active material, including but not limited to one or more of commercial LCO, NCM111, NCM532, NCM622, NCM712, NCM811, NCA811, and NCM955.
[0011] Preferably, the electrolyte is a sulfide solid electrolyte.
[0012] Preferably, the sulfide solid electrolyte includes Li6PS5Cl, Li6PS5Br, Li6PS5I, Li 5.5 PS 4.5 Cl 1.5 、Li7P3S 11 、Li7P2S8I,Li3PS4,Li 10 SnP2S 12 , Li 10 GeP2S 12 One or more of .
[0013] Preferably, the conductive agent includes one or more of VGCF, CNT, Ketjen black, carbon black and graphite.
[0014] In a second aspect, the present invention provides a method for preparing a solid thick electrode, comprising the following steps: Active materials, electrolytes and conductive agents with different mass proportions are mixed and ground to obtain multiple positive electrode sub-layers; In the order of decreasing proportion of active material mass, multiple positive electrode layers are stacked on the surface of the solid electrolyte layer in sequence, and a solid thick electrode is obtained after pressing.
[0015] In a third aspect, the present invention further provides a solid-state battery, comprising the solid-state thick electrode as described in the first aspect.
[0016] The beneficial effects of the present invention are: The present invention obtains a solid thick electrode with a gradient distribution of active material content by arranging a positive electrode layer with a high active material load on the side close to the electrolyte layer and a positive electrode layer with a low active material load on the side away from the electrolyte layer. This not only simplifies the process flow, but also significantly improves the effective utilization rate of the active material, thereby achieving good electrochemical performance under the thick solid electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings of the embodiment are briefly introduced below.
[0018] Figure 1 is a schematic diagram of the structure of the solid thick electrode in Example 1; In the figure, 1, solid electrolyte layer; 2, composite positive electrode layer; 21, first positive electrode layer; 22, second positive electrode layer; 23, third positive electrode layer; Figure 2 Schematic diagram of the distribution of positive electrode active materials in solid thick electrodes of Example 1 and Comparative Examples 1-2; Figure 3 Capacity-voltage curves of solid thick electrodes prepared in Example 1 and Comparative Examples 1-2 after being assembled into batteries; Figure 4 The cycle performance diagram of the solid thick electrodes prepared in Example 1 and Comparative Examples 1-2 after being assembled into batteries; Figure 5 Capacity-voltage curves of solid thick electrodes prepared in Example 1 and Comparative Example 3 after being assembled into batteries; Figure 6 This is a cycle performance diagram of the solid thick electrodes prepared in Example 1 and Comparative Example 3 after being assembled into batteries. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1 A solid thick electrode, such as Figure 1 As shown, it includes a solid electrolyte layer 1 and a composite positive electrode layer 2 which are stacked; wherein the composite positive electrode layer 2 includes a plurality of sublayers which are stacked in sequence, for example, referring to Figure 1 The composite positive electrode layer 2 consists of three layers, namely a first positive electrode layer 21 , a second positive electrode layer 22 and a third positive electrode layer 23 .
[0021] The preparation method of the solid thick electrode is as follows: (1) LiNi, the positive electrode active material 0.6 Co 0.2 MnO2(NCM622),Li 5.5 PS 4.5 Cl 1.5 (LPSC) and conductive agent CNT were mixed manually in a mortar with a mortar rod for 30 minutes according to the proportions of composite positive electrode 1, composite positive electrode 2, and composite positive electrode 3 in Table 1, transferred to a ball mill, and ball milling beads with a ball-to-material ratio of 20:1 were added. The mixture was ball milled at a speed of 100 rpm to obtain the first composite positive electrode material, the second composite positive electrode material, and the third composite positive electrode material, respectively.
[0022] Table 1
[0023] (2) In a glove box, first, weigh 80 mg of solid electrolyte LPSC and press it into shape at a pressure of 50 MPa in a ceramic sleeve with a diameter of 10 mm. Then, press the first composite positive electrode material, the second composite positive electrode material, and the third composite positive electrode material layer by layer in the order of pressing, and each pressing is at a pressure of 350 MPa. That is, the first composite positive electrode material is placed on the surface of the solid electrolyte layer, and after pressing, the second composite positive electrode material is placed on the surface of the first composite positive electrode layer, and after pressing, the third composite positive electrode material is placed on the surface of the second composite positive electrode layer, and after pressing, a solid thick electrode is obtained.
[0024] Example 2 A solid thick electrode, the preparation method is as follows: (1) LiNi, the positive electrode active material 0.6 Co 0.2 MnO2(NCM622),Li 5.5 PS 4.5 Cl 1.5(LPSC) and conductive agent CNT were mixed manually in a mortar with a mortar rod for 30 minutes according to the proportions of composite positive electrode 1, composite positive electrode 2, and composite positive electrode 3 in Table 2, transferred to a ball mill, and ball milling beads with a ball-to-material ratio of 20:1 were added. The mixture was ball milled at a speed of 100 rpm to obtain the first composite positive electrode material, the second composite positive electrode material, and the third composite positive electrode material, respectively.
[0025] Table 2
[0026] (2) In a glove box, first, 80 mg of solid electrolyte LPSC was weighed and pressed into shape in a ceramic sleeve with a diameter of 10 mm at a pressure of 50 MPa. Subsequently, the first composite positive electrode material, the second composite positive electrode material, and the third composite positive electrode material were pressed layer by layer in the order of 350 MPa each time to obtain a solid thick electrode.
[0027] Comparative Example 1 A solid thick electrode, the preparation method is basically the same as that of Example 1, except that the active material in the composite positive electrode layer does not have a gradient distribution, and specifically comprises the following steps: (1) LiNi, the positive electrode active material 0.6 Co 0.2 MnO2(NCM622),Li 5.5 PS 4.5 Cl 1.5 (LPSC) and conductive agent CNT were mixed manually in a mortar with a mortar rod for 30 minutes according to the proportions of composite positive electrode 1, composite positive electrode 2, and composite positive electrode 3 in Table 3, transferred to a ball mill, and ball milling beads with a ball-to-material ratio of 20:1 were added. The mixture was ball milled at a speed of 100 rpm to obtain the first composite positive electrode material, the second composite positive electrode material, and the third composite positive electrode material, respectively.
[0028] Table 3
[0029] (2) In a glove box, first, 80 mg of solid electrolyte LPSC was weighed and pressed into shape in a ceramic sleeve with a diameter of 10 mm at a pressure of 50 MPa. Subsequently, the first composite positive electrode material, the second composite positive electrode material, and the third composite positive electrode material were pressed layer by layer in the order of 350 MPa each time to obtain a solid thick electrode.
[0030] Comparative Example 2 A solid thick electrode, the preparation method is basically the same as that of Example 1, except that the mass proportion of the active material in the composite positive electrode layer gradually increases in the direction away from the solid electrolyte layer. Specifically, the steps include: (1) LiNi, the positive electrode active material 0.6 Co 0.2 MnO2(NCM622),Li 5.5 PS 4.5 Cl 1.5 (LPSC) and conductive agent CNT were mixed manually in a mortar with a mortar rod for 30 minutes according to the proportions of composite positive electrode 1, composite positive electrode 2, and composite positive electrode 3 in Table 4, transferred to a ball mill, and ball milling beads with a ball-to-material ratio of 20:1 were added. The mixture was ball milled at a speed of 100 rpm to obtain the first composite positive electrode material, the second composite positive electrode material, and the third composite positive electrode material, respectively.
[0031] Table 4
[0032] (2) In a glove box, first, 80 mg of LPSC was weighed and pressed into shape in a ceramic sleeve with a diameter of 10 mm at a pressure of 50 MPa. Subsequently, the first composite positive electrode material, the second composite positive electrode material, and the third composite positive electrode material were pressed layer by layer in the order of 350 MPa each time to obtain a solid thick electrode.
[0033] Comparative Example 3 A solid thick electrode, the preparation method is basically the same as that of Example 1, except that the mass proportion of the conductive agent in the composite positive electrode layer gradually decreases in the direction away from the solid electrolyte layer. Specifically, the steps include: (1) LiNi, the positive electrode active material 0.6 Co 0.2 MnO2(NCM622),Li 5.5 PS 4.5 Cl 1.5 The (LPSC) and the conductive agent CNT were mixed manually in a mortar with a mortar rod for 30 minutes according to the proportions of composite positive electrode 1, composite positive electrode 2, and composite positive electrode 3 in Table 5, transferred to a ball mill, and ball milling beads with a ball-to-material ratio of 20:1 were added. The mixture was ball milled at a speed of 100 rpm to obtain the first composite positive electrode material, the second composite positive electrode material, and the third composite positive electrode material, respectively.
[0034] Table 5
[0035] (2) In a glove box, first, 80 mg of LPSC was weighed and pressed into shape in a ceramic sleeve with a diameter of 10 mm at a pressure of 50 MPa. Subsequently, the first composite positive electrode material, the second composite positive electrode material, and the third composite positive electrode material were pressed layer by layer in the order of 350 MPa each time to obtain a solid thick electrode.
[0036] Performance Testing In a glove box, the solid thick electrodes of Example 1 and Comparative Examples 1 to 3 were placed in a ceramic sleeve with a diameter of 10 mm, and then the lithium indium alloy negative electrode was attached to the side of the solid electrolyte layer away from the composite positive electrode layer, and pressed with a press at 150 MPa until good contact, and the battery mold was tightened to obtain an all-solid-state lithium ion battery. The obtained lithium ion battery was subjected to a performance test at a test temperature of 28°C. Figure 2 Schematic diagram of the distribution of positive electrode active materials in solid thick electrodes of Example 1 and Comparative Examples 1-2.
[0037] The test results are shown in Table 6 and Figures 3-5 As shown, the constant current charge and discharge measurements are performed in the range of 2.4~3.7V, and the charge and discharge current density is 0.1C.
[0038] Table 6
[0039] It can be seen from the above test data that the present invention achieves a significant improvement in the first discharge capacity, cycle capacity and capacity retention rate by constructing a gradient electrode on the side close to the solid electrolyte layer in the order of decreasing mass proportion of active materials.
[0040] The first discharge capacity, cycle capacity and capacity retention rate of Example 1 are all higher than those of Comparative Example 1, indicating that the performance of the battery with the gradient-distributed thick electrode is better than that of the battery without the gradient-distributed thick electrode.
[0041] Compared with Comparative Example 2, Example 1 has better electrochemical performance of the battery, indicating that the gradient electrode constructed in the order of increasing mass proportion of active material on the side close to the solid electrolyte layer cannot effectively improve the electrochemical performance of the battery.
[0042] Compared with Comparative Example 3, keeping the proportion of the conductive agent unchanged in Example 1 can improve the first cycle coulombic efficiency, the first specific capacity and the cycle capacity retention rate of the battery. This is because solid-state batteries do not have the wettability of electrolytes like liquid batteries. The electrolyte, active materials and conductive agents between the composite electrodes of solid-state batteries are in a point-to-point solid-solid contact form, and the conductive agent is the key to constructing the three-dimensional conductive network framework of the composite electrode. Too high a proportion will cause the decomposition of the electrolyte, and too low a proportion will cause poor electronic conductivity; especially in thick electrode systems, the adjustment of the conductive agent ratio has a great influence on the overall electrochemical performance of the battery.
[0043] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For details not described in individual embodiments, reference may be made to the description in other embodiments.
[0044] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A solid thick electrode, characterized in that: It comprises a stacked solid electrolyte layer and a composite positive electrode layer; wherein the composite positive electrode layer comprises a plurality of sublayers stacked in sequence; away from the solid electrolyte layer, the mass proportion of active materials in the plurality of sublayers gradually decreases.
2. The solid thick electrode according to claim 1, characterized in that: The number of sublayers is n, the sublayer close to the solid electrolyte layer is recorded as the first layer, and the sublayer far from the solid electrolyte layer is recorded as the nth layer; From the first layer to the nth layer, the mass proportion of the active material in each sub-layer is recorded as X1, X2, X3, ...X n The mass proportion of the electrolyte in each sublayer is recorded as Y1, Y2, Y3, ...Y n ; Among them, X1>X2>X3>…>X n , Y1<Y2<Y3<…<Y n .
3. The solid thick electrode according to claim 1, characterized in that: The mass proportion of the conductive agent in the multiple sub-layers is the same.
4. The solid thick electrode according to claim 1, characterized in that: The composite positive electrode layer includes an active material, an electrolyte and a conductive agent; the mass proportion of the active material is 50-80%, the mass proportion of the electrolyte is 18-48%, and the rest is the conductive agent.
5. The solid thick electrode according to claim 1, characterized in that: The active material includes one or more of LCO, NCM111, NCM532, NCM622, NCM712, NCM811, NCA811, and NCM955.
6. The solid thick electrode according to claim 4, characterized in that: The electrolyte is a sulfide solid electrolyte.
7. The solid thick electrode according to claim 6, characterized in that: The sulfide solid electrolyte includes Li6PS5Cl, Li6PS5Br, Li6PS5I, Li 5.5 PS 4.5 Cl 1.5 、Li7P3S 11 、Li7P2S8I,Li3PS4,Li 10 SnP2S 12 , Li 10 GeP2S 12 One or more of .
8. The solid thick electrode according to claim 4, characterized in that: The conductive agent includes one or more of VGCF, CNT, Ketjen black, carbon black and graphite.
9. A method for preparing a solid thick electrode as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: Active materials, electrolytes and conductive agents with different mass proportions are mixed and ground to obtain multiple positive electrode sub-layers; The plurality of positive electrode layers are stacked on the surface of the solid electrolyte layer in descending order of the mass proportion of the active material, and the solid thick electrode is obtained after pressing.
10. A solid-state battery, characterized in that: Comprising a solid thick electrode as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Pole piece, preparation method of pole piece, battery, battery module, battery pack and device
CN117352651A
All-solid-state double-layer composite positive electrode, preparation method thereof and lithium ion battery
CN118198335A