Polyhedral Ge / C lithium ion battery composite negative electrode material and preparation method thereof
The polyhedral Ge/C composite anode material was synthesized by the sol-gel method, and the polyhedral structure and carbonization treatment of ZIF-67 were used to form carbon cage-covered germanium particles, which solved the performance problems caused by the volume changes of the negative electrode material of lithium-ion batteries, and achieved the High energy density and cycle stability reduce costs.
Patent Information
- Application Number
- CN202410986122.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing negative electrode material graphite theory is lower than that of the lithium-ion battery, which is difficult to meet the needs of high energy density and cycle life such as electric vehicles. Moreover, the Ge negative electrode material has a powdering material and a damage to the electrode structure due to volume changes during charging and discharging, which affects the Battery capacity and cycle life.
The sol-gel method is used to combine it with a tube furnace to form a composite negative electrode material of Ge/C lithium-ion battery. The polyhedral structure and carbonization treatment of ZIF-67 is used to form carbon cage-covered germanium particles to limit the volume expansion of the germanium electrode. Enhance conductivity and dispersion and improve electrochemical performance.
It achieves excellent cycle performance and charge and discharge rate performance of lithium-ion batteries, improves the energy density and cycle stability of the battery, and reduces material costs.
Smart Images

Figure CN118943322A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery negative electrode materials, and in particular relates to a polyhedral Ge / C lithium ion battery composite negative electrode material and a preparation method thereof. Background Art
[0002] In today's globalized world, energy issues have always been a topic of concern to all mankind. With the continuous reduction of fossil energy such as coal, oil and natural gas, the energy crisis has become more and more obvious. The environmental pollution and ecological damage caused by the excessive use of fossil fuels also threaten the sustainable development of mankind. Therefore, under the dual pressure of energy crisis and environmental problems, the development of renewable clean energy has become a hot topic of global concern. At present, clean energy such as wind energy, solar energy and tidal energy has great randomness and intermittency in time and region, so it is necessary to develop corresponding energy storage technology to effectively store electrical energy and improve its utilization rate.
[0003] Lithium-ion batteries are widely used as the main energy storage technology in consumer electronic products due to their many advantages such as high energy density, long cycle life and no memory effect. In recent years, with the rapid growth of the electric vehicle market, higher requirements have been put forward for the energy density, charge and discharge speed and cycle life of lithium-ion batteries. However, the existing commercial lithium-ion batteries use graphite as the negative electrode and have a low theoretical specific capacity (372mAh g -1 ), the energy storage characteristics are difficult to meet the demand, therefore, finding a negative electrode material with high specific capacity to replace traditional graphite is the key to improving the energy density of the battery.
[0004] Ge is an element of the IVA group and is in the same main group as Si. The two have similar physical and chemical properties and are both alloy-type negative electrode materials. The discharge products are Li 4.4 Si and Li 4.4 The theoretical specific capacity of Ge and Si is as high as 4200 mAh g -1 , while the theoretical specific capacity of Ge is about 1600 mAh g -1 , which is about 40% of Si, but the relative atomic mass of Ge is about 72 (about 2.7 times that of Si) and the density is 5.5g / cm 3 (about 2.36 times that of Si), therefore, the volumetric capacity of Ge and Si is basically the same, and, as the most common semiconductor material, the band gap width of Ge is 0.6eV, and the band gap width of Si is 1.1eV, so the conductivity of Ge is four orders of magnitude higher than that of Si, and the Ge electrode exhibits a lower volume change than Si during the charge and discharge process and a faster lithium ion diffusion rate than Si at room temperature (400 times faster than Si), which is more suitable for industrial high-power and high-current equipment.
[0005] However, there are also many problems in the actual application of Ge negative electrode materials. The fundamental reason comes from the large volume effect. The volume change of active materials during the charging and discharging process will cause material pulverization, electrode structure destruction, and loss of electrical contact with the current collector, which seriously restricts the battery capacity and cycle life. Summary of the invention
[0006] The purpose of the present invention is to provide a polyhedral Ge / C lithium ion battery composite negative electrode material and a preparation method thereof. The prepared lithium ion battery composite negative electrode material can give the lithium ion battery excellent cycle performance and charge and discharge rate performance.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing a polyhedral Ge / C lithium-ion battery composite negative electrode material comprises the following steps:
[0009] Step 1: 0.4-1 mmol of germanium and 0.03-0.05 mmol of hexadecyltrimethylammonium bromide are added to 30-40 mL of anhydrous methanol, and mixed thoroughly to obtain a mixture B. 4.6-5 mmol of cobalt nitrate hexahydrate is added to the mixture B and fully dissolved to obtain a solution C;
[0010] Step 2: Dissolve 0.01-0.03 mol of 2-methylimidazole in 30-40 mL of anhydrous methanol to obtain solution D, add solution D to solution C, mix well, and obtain a dark purple solution E;
[0011] Step 3: After centrifuging solution E, washing and vacuum drying are carried out in sequence to obtain Ge / ZIF-67;
[0012] Step 4: Place Ge / ZIF-67 in a tube furnace, heat it from room temperature to 600-800°C at a heating rate of 3-5°C / min in a protective atmosphere, keep it warm for 2-3 hours, and cool it naturally to room temperature to obtain a polyhedral Ge / C lithium-ion battery composite negative electrode material.
[0013] Furthermore, the germanium single substance is prepared by the following method:
[0014] Step 1.1: Add 0.01-0.02 mol of germanium dioxide to 30-40 mL of deionized water to obtain solution A;
[0015] Step 1.2: Add 5-15 mL of anhydrous ethylenediamine dropwise to solution A while stirring, continue stirring and heat to 75-85° C. After the solution evaporates to become a milky white colloid, stop stirring and freeze-dry the milky white colloid to obtain white solid particles;
[0016] Step 1.3: Grind the white solid particles, place them in a tube furnace, and heat them from room temperature to 750-850°C at a heating rate of 8-10°C / min in an argon atmosphere, and keep them warm for 2-3 hours to obtain germanium.
[0017] Furthermore, the freeze drying in step 1.2 is performed at -40 to -50°C for 10 to 12 hours.
[0018] Furthermore, the sufficient mixing in step 1 is carried out by ultrasonic dispersion for 25 to 35 minutes.
[0019] Furthermore, the thorough mixing in step 2 is performed by using a magnetic heating stirrer at 20 to 30° C. and a rotation speed of 250 to 350 r / min for 23 to 25 hours.
[0020] Furthermore, the cleaning in step three is performed by centrifugal washing with anhydrous methanol for 3 to 6 times.
[0021] Furthermore, the vacuum drying in step three is carried out in a vacuum drying oven at 50-70°C.
[0022] Furthermore, the protective atmosphere of step four is argon, or a mixed gas formed by mixing H2 and argon in a volume ratio of 5:95.
[0023] A polyhedral Ge / C lithium ion battery composite negative electrode material has a particle size of 400nm to 600nm and is in a polyhedral shape.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention adopts a sol-gel method and a tubular furnace calcination to synthesize a polyhedral Ge / C lithium ion battery composite negative electrode material, which has the advantages of simple preparation process and low cost.
[0026] (2) Through the sol-gel method, solid-phase sintering reaction and control of physical and chemical factors, the effects of the doping amount of the reactants and the temperature of different high-temperature calcination on the reaction products were explored. Finally, the most appropriate process parameters were selected to achieve organic-inorganic hybridization and modification, and a polyhedral Ge / C lithium-ion battery composite negative electrode material with excellent performance was prepared. Due to the polyhedral structure of ZIF-67 (cobalt-based zeolite imidazolate MOF) itself, it can maintain its original framework structure after high-temperature carbonization treatment and is an ideal carbon cage template. After ZIF-67 is composited with elemental germanium, a structure of carbon cage-coated germanium particles is formed, which can not only limit the huge volume expansion of the elemental germanium electrode during the charge and discharge process, but the presence of the carbon layer can also increase the conductivity of the electrode. In addition, the metal cobalt retained in ZIF-67 can form a germanium-cobalt alloy with the element under high-temperature calcination, which can also enhance the conductivity of the material. At the same time, it also improves the dispersion of elemental germanium particles, further improving the electrochemical performance of the electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 XRD diffraction spectrum of the polyhedral Ge / C lithium ion battery composite negative electrode material prepared in Example 2 of the present invention;
[0028] Figure 2 This is a Raman image of a polyhedral Ge / C lithium-ion battery composite negative electrode material prepared in Example 2 of the present invention;
[0029] Figure 3 This is a SEM image of a polyhedral Ge / C lithium-ion battery composite negative electrode material prepared in Example 2 of the present invention;
[0030] Figure 4 TEM image of the polyhedral Ge / C lithium ion battery composite negative electrode material prepared in Example 2 of the present invention;
[0031] Figure 5 The lithium ion battery assembled with the Ge / C composite negative electrode material prepared in Example 2 of the present invention is -1 Cycling performance diagram at different current densities. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0033] Example 1
[0034] Step 1: Add 0.01 mol of germanium dioxide into 30 mL of deionized water to obtain solution A;
[0035] Step 2: Using a magnetic heating stirrer, add 5 mL of anhydrous ethylenediamine solution dropwise into solution A while stirring, continue stirring and heat to 75°C, and stop stirring after the solution evaporates to become a milky white colloid, freeze-dry the milky white colloid at -40°C for 10 hours to obtain white solid particles;
[0036] Step 3: Grind the white solid particles, place them in a tube furnace, and heat them from room temperature to 750°C at a heating rate of 8°C / min in an argon atmosphere, and keep them warm for 3 hours to obtain germanium;
[0037] Step 4: 0.4 mmol of germanium and 0.03 mmol of hexadecyltrimethylammonium bromide were added to 30 mL of anhydrous methanol, and ultrasonically dispersed for 25 min to fully mix to obtain a mixture B. 4.6 mmol of cobalt nitrate hexahydrate was added to the mixture B, and stirred for 25 min to obtain a solution C;
[0038] Step 5: Dissolve 0.01 mol of 2-methylimidazole in 30 mL of anhydrous methanol, and stir for 23 h at 250 r / min at 20°C using a magnetic heating stirrer to obtain solution D, and quickly add solution D to solution C and mix thoroughly to obtain a dark purple solution E;
[0039] Step 6: After centrifuging solution E, wash it three times with anhydrous methanol, and then put it into a vacuum oven at 60°C for drying to obtain Ge / ZIF-67;
[0040] Step 7: Place Ge / ZIF-67 in a tube furnace, heat from room temperature to 600°C at a heating rate of 3°C / min in a H2 / Ar mixed gas atmosphere with a volume ratio of 5:95, keep warm for 3 hours, and cool naturally to room temperature to obtain a polyhedral Ge / C lithium-ion battery composite negative electrode material.
[0041] Example 2
[0042] Step 1: Add 0.02 mol of germanium dioxide into 30 mL of deionized water to obtain solution A;
[0043] Step 2: Using a magnetic heating stirrer, add 10 mL of ethylenediamine solution dropwise into solution A while stirring, continue stirring and heat to 80°C, stop stirring after the solution evaporates to become a milky white colloid, freeze-dry the milky white colloid at -45°C for 12 hours to obtain white solid particles;
[0044] Step 3: Grind the white solid particles, place them in a tube furnace, and calcine them to 800°C at a heating rate of 10°C / min in an argon atmosphere, and keep them warm for 3 hours to obtain germanium;
[0045] Step 4: 0.7 mmol of germanium and 0.04 mmol of hexadecyltrimethylammonium bromide were added to 35 mL of anhydrous methanol, and ultrasonically dispersed for 30 min to fully mix to obtain a mixture B. 4.8 mmol of cobalt nitrate hexahydrate was added to the mixture B, and stirred for 30 min to obtain a solution C;
[0046] Step 5: Dissolve 0.02 mol of 2-methylimidazole in 35 mL of anhydrous methanol, and stir for 24 h at 300 r / min at 25°C using a magnetic heating stirrer to obtain solution D, and quickly add solution D to solution C and mix thoroughly to obtain a dark purple solution E;
[0047] Step 6: After centrifuging solution E, wash it six times with anhydrous methanol, and then put it into a vacuum oven at 50°C for drying to obtain Ge / ZIF-67;
[0048] Step 7: Place Ge / ZIF-67 in a tube furnace, heat from room temperature to 700°C at a heating rate of 3°C / min in a H2 / Ar mixed gas atmosphere with a volume ratio of 5:95, keep warm for 3 hours, and cool naturally to room temperature to obtain a polyhedral Ge / C lithium-ion battery composite negative electrode material.
[0049] from Figure 1 It can be seen that the composite negative electrode prepared in Example 2 corresponds to the standard card XRD pattern and the standard diffraction patterns of cubic phase Ge (JCPDS card number 04-0545) and CoGe2 (JCPDS card number 07-0162), which have good crystallinity. The formation of CoGe2 is because Ge forms an alloy with cobalt in the raw material hexahydrate of cobalt nitrate for preparing ZIF-67 during high-temperature calcination. According to literature reports, CoGe2 can provide additional capacity, so that the electrode material has excellent structural stability and energy storage efficiency; in addition, since the Ge (111) peak at 27.3° coincides with the diffraction peak of carbon, the diffraction peak of carbon cannot be observed in the figure.
[0050] from Figure 2 It can be seen that at 298cm -1 The Raman peak at 1351 cm is the characteristic peak of crystalline germanium, corresponding to the vibration of Ge-Ge bond. -1 and 1596cm -1 The two peaks at correspond to the D band peak and G band peak of carbon materials. After calculation, the I D / I G The value is 1.01, indicating that the carbon in the composite negative electrode material mainly exists in the form of amorphous carbon.
[0051] from Figure 3It can be seen that the composite negative electrode material prepared in Example 2 has a novel morphology, is polyhedral, and has a particle size of 400nm to 600nm.
[0052] from Figure 4 (a) It can be seen that the ZIF-67 derived carbon cage framework covers the polyhedral structure of germanium. The continuous amorphous carbon shell formed by carbonization is also doped with uniformly dispersed metal Co particles, which plays an important role in enhancing the conductivity of the material and improving the dispersion of germanium particles. Figure 4 (b) The high-resolution TEM image shows lattice fringes with a crystal plane spacing of 0.20 nm, corresponding to the (220) crystal plane of germanium. The surrounding area without obvious lattice fringes is the amorphous carbon layer derived from the high-temperature carbonization of ZIF-67.
[0053] from Figure 5 It can be seen that the lithium-ion battery assembled using the sample prepared in Example 2 as the negative electrode has a high -1 The initial discharge capacity at the current density is 1241.9 mAh g -1 The initial charge capacity is 795.6 mAh g -1 The coulombic efficiency of the first cycle is 64.1%, and the initial discharge capacity of Ge is 1562.5 mAh g -1 The initial charge capacity is 912.6 mAh g -1 The coulombic efficiency of the first cycle is 58.4%. Although the initial charge and discharge capacity is lower than that of the lithium-ion battery assembled with Ge single-electrode, the coulombic efficiency of the first cycle is improved. After 100 cycles, the discharge specific capacity is 754.1 mAh g -1 The capacity retention rate is 60.7%. However, the capacity of the lithium battery assembled with single-element Ge electrode is greatly reduced due to the huge volume expansion during the charge and discharge process. After 100 cycles, the discharge capacity is only 222 mAh g -1 The capacity retention rate is only 14.2%, which is enough to prove that the multi-faceted Ge / C composite electrode can give lithium batteries better cycle stability than the Ge single electrode.
[0054] Example 3
[0055] Step 1: Add 0.01 mol of germanium dioxide into 35 mL of deionized water to obtain solution A;
[0056] Step 2: Using a magnetic heating stirrer, add 15 mL of ethylenediamine solution dropwise into solution A while stirring, continue stirring and heat to 80°C, stop stirring after the solution evaporates to become a milky white colloid, freeze-dry the milky white colloid at -50°C for 12 hours to obtain white solid particles;
[0057] Step 3: Grind the white solid particles, place them in a tube furnace, and heat them from room temperature to 850°C at a heating rate of 10°C / min in an argon atmosphere, and keep them warm for 2 hours to obtain germanium;
[0058] Step 4: 1 mmol of germanium and 0.04 mmol of hexadecyltrimethylammonium bromide were added to 35 mL of anhydrous methanol, and ultrasonically dispersed for 30 min to obtain a mixture B. 5 mmol of cobalt nitrate hexahydrate was added to the mixture B, and stirred for 30 min to obtain a solution C.
[0059] Step 5: Dissolve 0.02 mol of 2-methylimidazole in 35 mL of anhydrous methanol, stir for 24 h at 25 °C and 300 r / min using a magnetic heating stirrer to obtain solution D, quickly add solution D to solution C, mix thoroughly, and obtain a dark purple solution E;
[0060] Step 6: After centrifuging solution E, wash it five times with anhydrous methanol, and then put it into a vacuum oven at 60°C for drying to obtain Ge / ZIF-67;
[0061] Step 7: Place Ge / ZIF-67 in a tube furnace, heat from room temperature to 800°C at a heating rate of 4°C / min in a H2 / Ar mixed gas atmosphere with a volume ratio of 5:95, keep warm for 3 hours and naturally cool to room temperature to obtain a polyhedral Ge / C lithium-ion battery composite negative electrode material.
[0062] Example 4
[0063] Step 1: Add 0.01 mol of germanium dioxide into 30 mL of deionized water to obtain solution A;
[0064] Step 2: Using a magnetic heating stirrer, add 10 mL of ethylenediamine solution dropwise into solution A while stirring, continue stirring and heat to 80°C, stop stirring after the solution evaporates to become a milky white colloid, freeze-dry the milky white colloid at -40°C for 11 hours to obtain white solid particles;
[0065] Step 3: Grind the white solid particles, place them in a tube furnace, and heat them from room temperature to 800°C at a heating rate of 10°C / min in an argon atmosphere, and keep them warm for 3 hours to obtain germanium;
[0066] Step 4: 0.8 mmol of germanium and 0.04 mmol of hexadecyltrimethylammonium bromide were added to 40 mL of anhydrous methanol, and ultrasonically dispersed for 35 min to obtain a mixture B. 4.9 mmol of cobalt nitrate hexahydrate was added to the mixture B, and stirred for 35 min to obtain a solution C.
[0067] Step 5: Dissolve 0.02 mol of 2-methylimidazole in 40 mL of anhydrous methanol, and stir for 24 h at 350 r / min at 25°C using a magnetic heating stirrer to obtain solution D, and quickly add solution D to solution C and mix thoroughly to obtain a dark purple solution E;
[0068] Step 6: After centrifuging solution E, wash it 4 times with anhydrous methanol, and then put it into a vacuum oven at 70°C for drying to obtain Ge / ZIF-67;
[0069] Step 7: Place Ge / ZIF-67 in a tube furnace, and heat it from room temperature to 650°C at a heating rate of 5°C / min in an Ar atmosphere, keep it warm for 2 hours, and cool it naturally to room temperature to obtain a polyhedral Ge / C lithium-ion battery composite negative electrode material.
[0070] Example 5
[0071] Step 1: Add 0.02 mol of germanium dioxide into 40 mL of deionized water to obtain solution A;
[0072] Step 2: Using a magnetic heating stirrer, add 15 mL of ethylenediamine solution dropwise into solution A while stirring, continue stirring and heat to 85°C, stop stirring after the solution evaporates to become a milky white colloid, freeze-dry the milky white colloid at -50°C for 10 hours to obtain white solid particles;
[0073] Step 3: Grind the white solid particles, place them in a tube furnace, and heat them from room temperature to 800°C at a heating rate of 8°C / min in an argon atmosphere, and keep them warm for 2.5 hours to obtain germanium;
[0074] Step 4: Add 0.5 mmol of germanium and 0.03 mmol of hexadecyltrimethylammonium bromide into 30 mL of anhydrous methanol, and disperse by ultrasonic for 30 min to obtain a mixture B. Add 4.7 mmol of cobalt nitrate hexahydrate into the mixture B, and stir for 30 min to obtain a solution C.
[0075] Step 5: Dissolve 0.02 mol of 2-methylimidazole in 30 mL of anhydrous methanol, stir for 25 h at 30°C and 350 r / min using a magnetic heating stirrer to obtain solution D, quickly add solution D to solution C, mix thoroughly, and obtain a dark purple solution E;
[0076] Step 6: After centrifuging solution E, wash it three times with anhydrous methanol, and then put it into a vacuum oven at 50°C for drying to obtain Ge / ZIF-67;
[0077] Step 7: Place Ge / ZIF-67 in a tube furnace, and heat it from room temperature to 750°C at a heating rate of 3°C / min in an Ar atmosphere, keep it warm for 2.5 hours, and cool it naturally to room temperature to obtain a polyhedral Ge / C lithium-ion battery composite negative electrode material.
[0078] Example 6
[0079] Step 1: Add 0.015 mol of germanium dioxide into 35 mL of deionized water to obtain solution A;
[0080] Step 2: Using a magnetic heating stirrer, add 10 mL of ethylenediamine solution dropwise into solution A while stirring, continue stirring and heat to 80°C, stop stirring after the solution evaporates to become a milky white colloid, freeze-dry the milky white colloid at -40°C for 11 hours to obtain white solid particles;
[0081] Step 3: Grind the white solid particles, place them in a tube furnace, and heat them from room temperature to 850°C at a heating rate of 8°C / min in an argon atmosphere, and keep them warm for 2 hours to obtain germanium;
[0082] Step 4: 0.9 mmol of germanium and 0.05 mmol of hexadecyltrimethylammonium bromide were added to 40 mL of anhydrous methanol, and ultrasonically dispersed for 35 min to obtain a mixture B. 5 mmol of cobalt nitrate hexahydrate was added to the mixture B and stirred for 30 min to obtain a solution C.
[0083] Step 5: Dissolve 0.025 mol of 2-methylimidazole in 40 mL of anhydrous methanol, stir for 23 h at 250 r / min at 20°C using a magnetic heating stirrer to obtain solution D, quickly add solution D to solution C, mix thoroughly, and obtain a dark purple solution E;
[0084] Step 6: After centrifuging solution E, wash it 4 times with anhydrous methanol, and then put it into a vacuum oven at 70°C for drying to obtain Ge / ZIF-67;
[0085] Step 7: Place Ge / ZIF-67 in a tube furnace, and heat it from room temperature to 750°C at a heating rate of 5°C / min in an Ar atmosphere, keep it warm for 2 hours, and naturally cool it to room temperature to obtain a polyhedral Ge / C lithium-ion battery composite negative electrode material.
Claims
1. A method for preparing a polyhedral Ge / C lithium-ion battery composite negative electrode material, characterized in that: The following steps are involved: Step 1: 0.4-1 mmol of germanium and 0.03-0.05 mmol of hexadecyltrimethylammonium bromide are added to 30-40 mL of anhydrous methanol, and mixed thoroughly to obtain a mixture B. 4.6-5 mmol of cobalt nitrate hexahydrate is added to the mixture B and fully dissolved to obtain a solution C; Step 2: Dissolve 0.01-0.03 mol of 2-methylimidazole in 30-40 mL of anhydrous methanol to obtain solution D, add solution D to solution C, mix well, and obtain a dark purple solution E; Step 3: After centrifuging solution E, washing and vacuum drying are carried out in sequence to obtain Ge / ZIF-67; Step 4: Place Ge / ZIF-67 in a tube furnace, heat it from room temperature to 600-800°C at a heating rate of 3-5°C / min in a protective atmosphere, keep it warm for 2-3 hours, and cool it naturally to room temperature to obtain a polyhedral Ge / C lithium-ion battery composite negative electrode material.
2. The method for preparing the polyhedral Ge / C lithium ion battery composite negative electrode material according to claim 1, characterized in that: The germanium element is prepared by the following method: Step 1.1: Add 0.01-0.02 mol of germanium dioxide to 30-40 mL of deionized water to obtain solution A; Step 1.2: Add 5-15 mL of anhydrous ethylenediamine dropwise to solution A while stirring, continue stirring and heat to 75-85° C. After the solution evaporates to become a milky white colloid, stop stirring and freeze-dry the milky white colloid to obtain white solid particles; Step 1.3: Grind the white solid particles, place them in a tube furnace, and heat them from room temperature to 750-850°C at a heating rate of 8-10°C / min in an argon atmosphere, and keep them warm for 2-3 hours to obtain germanium.
3. The method for preparing the polyhedral Ge / C lithium ion battery composite negative electrode material according to claim 2, characterized in that: The freeze drying in step 1.2 is performed at -40 to -50°C for 10 to 12 hours.
4. The method for preparing a polyhedral Ge / C lithium-ion battery composite negative electrode material according to claim 1, characterized in that: The sufficient mixing in step 1 is carried out by ultrasonic dispersion for 25 to 35 minutes.
5. The method for preparing a polyhedral Ge / C lithium-ion battery composite negative electrode material according to claim 1, characterized in that: The thorough mixing in step 2 is performed by using a magnetic heating stirrer at 20 to 30° C. and a rotation speed of 250 to 350 r / min for 23 to 25 hours.
6. The method for preparing a polyhedral Ge / C lithium-ion battery composite negative electrode material according to claim 1, characterized in that: The cleaning in step three is performed by centrifugation washing with anhydrous methanol for 3 to 6 times.
7. The method for preparing a polyhedral Ge / C lithium-ion battery composite negative electrode material according to claim 1, characterized in that: The vacuum drying in step three is carried out in a vacuum drying oven at 50-70°C.
8. The method for preparing a polyhedral Ge / C lithium-ion battery composite negative electrode material according to claim 1, characterized in that: The protective atmosphere of step 4 is argon, or a mixed gas of H2 and argon in a volume ratio of 5:
95.
9. A polyhedral Ge / C lithium ion battery composite negative electrode material prepared according to any one of claims 1 to 8, characterized in that: The particle size is 400nm to 600nm and the shape is polyhedral.