Preparation method of hollow core-shell nanometer silicon-carbon composite material for lithium ion battery negative electrode
Preparation of hollow core-shell nanosilicon carbon composite materials by double-layer in-situ growth method has solved the problem of poor cycle stability of nano-level silicon carbon materials in lithium-ion batteries, and achieved high capacity and excellent battery performance, especially at high current density long cycle performance.
Patent Information
- Application Number
- CN202411030286.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Nano-scale silicon-carbon anode materials have problems such as poor long cycle stability and easy destruction of silicon-carbon structure in lithium-ion batteries, resulting in a decline in electrode performance and rapid decline in capacity.
The hollow core-shell nano-silicon-carbon composite material is prepared by double-layer in situ growth method. By forming an outer carbon shell and an inner SiO2 layer on silicon particles, a stable hollow core-shell structure is formed to enhance electron and ion transport, and in lithium Provide stress buffer during the fusion process to prevent direct contact between silicon and electrolyte.
It significantly improves the conductivity and cyclic stability of silicon-based materials, ensures that the capacity retention rate of more than 85% is still maintained at high current density, and extends the cycle life of the electrode materials.
Smart Images

Figure CN118943332A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries. Background Art
[0002] The world is currently facing severe energy and environmental challenges, and there is an urgent need to develop and effectively utilize clean energy. The combination of electrochemical energy storage technology and clean energy is seen as an effective way to solve the time and space limitations of clean energy. As the most widely used electrochemical energy storage battery, the energy density of lithium-ion batteries is limited by the low capacity of electrode materials. Therefore, in order to improve the energy density of lithium-ion batteries, researchers from various countries are actively conducting research on high-capacity negative electrode materials.
[0003] Silicon is highly regarded as a promising alternative to graphite in lithium-ion batteries due to its extensive reserves, excellent theoretical capacity, and suitable voltage. However, silicon undergoes a large volume expansion (greater than 400%) during lithium storage and exhibits poor electronic and ionic conductivity. These inherent properties lead to safety issues such as electrode cracking, battery performance degradation, and rapid capacity loss. Therefore, the limitations brought about by these inherent characteristics of silicon-based anode materials hinder their practical application and their rapid development in the field of lithium-ion batteries.
[0004] According to existing literature, although various nano-scale silicon-carbon negative electrode materials are emerging, the lack of strong bonding between silicon and carbon makes the silicon-carbon structure unstable, which causes problems such as separation or shedding of silicon and carbon during the cycle of the material, affecting the long-term cycle stability of the material. Therefore, in order to solve this problem, it is very important to design a nano-silicon-carbon composite material with a stable structure and. Summary of the invention
[0005] The present invention aims to solve the problems that the existing nano-scale silicon-carbon negative electrode materials have poor long-cycle stability and the silicon-carbon structure is easily destroyed, and further provides a method for preparing a hollow core-shell nano-silicon-carbon composite material for lithium-ion battery negative electrode.
[0006] A method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery is carried out according to the following steps:
[0007] 1. Preparation of hollow core-shell-Si@C:
[0008] ① Add cobalt nitrate hexahydrate and 2-methylimidazole to methanol and mix by ultrasonic dispersion, then stir for 1 h to 12 h, age at room temperature, and finally collect the precipitate by centrifugation and washing to obtain ZIF-67;
[0009] ② Add ZIF-67 to ethanol and mix by ultrasonic dispersion, then add distilled water, tetraethyl orthosilicate and ammonia water and stir for 1h to 12h, finally collect the precipitate by centrifugation and washing to obtain ZIF-67 with in-situ growth of SiO2;
[0010] ③ Add the in-situ grown SiO2 ZIF-67 into ethanol and mix by ultrasonic dispersion, then add resorcinol, ammonia and formaldehyde and stir for 1h to 12h, finally collect the precipitate by centrifugation and washing to obtain the in-situ grown phenolic resin ZIF-67@SiO2;
[0011] ④ Add the ZIF-67@SiO2 grown in situ on phenolic resin into ethanol and disperse and mix by ultrasonication, then add hydrochloric acid and ultrasonicate, finally collect the precipitate by centrifugation and vacuum drying to obtain the hollow core-shell-SiO2@RF after etching the internal ZIF-67;
[0012] ⑤ In an Ar atmosphere at a temperature of 600°C to 800°C, the hollow core-shell-SiO2@RF after etching the internal ZIF-67 was calcined for 1h to 6h to obtain the hollow core-shell-SiO2@C;
[0013] ⑥ Mix the hollow core-shell-SiO2@C, Mg powder and NaCl, and pyrolyze them for 1h to 6h in an Ar / H2 atmosphere at a temperature of 600°C to 800°C to obtain a crude hollow core-shell-Si@C product;
[0014] 2. Treatment of Hollow Core-Shell-Si@C Crude Product:
[0015] The hollow core-shell-Si@C crude product was centrifuged with anhydrous ethanol, hydrochloric acid, deionized water, hydrofluoric acid and anhydrous ethanol in sequence, and finally dried to obtain a hollow core-shell-Si@C composite material.
[0016] The beneficial effects of the present invention are:
[0017] 1. Different from the general coating of traditional silicon-carbon materials, which will separate and fall off during the lithiation process, the present invention realizes a double-layer in-situ growth method to achieve a deeply integrated silicon-carbon composite material. The composite material synthesized by this method not only improves the conductivity of the silicon-based material, but also makes it difficult for silicon and carbon to separate during the lithiation process, thereby achieving cycle stability.
[0018] 2. The present invention designs a unique hollow core-shell silicon-carbon composite structure. The outer carbon shell is used to enhance electron and ion transmission and act as a stress buffer, and the internal silicon nanoparticles are firmly attached to the carbon shell, effectively preventing separation and crushing during lithiation and delithiation. This structure can protect the internal silicon nanodots from direct contact with the electrolyte and provide a closed space for the inward contraction of silicon during lithium storage, which is conducive to the formation of a stable SEI layer and effectively avoids the crushing of silicon particles.
[0019] 3. The material prepared by the present invention has excellent cycle stability due to its innovative preparation method and unique structure. After 250 cycles at a current density of 200 mA / g, its reversible capacity is 927.1 mAh g -1 After 800 cycles at a current density of 1000 mA / g, the reversible capacity is 883 mAh g -1 The ultra-long cycle performance under high current is a very important characteristic of electrode materials. After 3000 cycles at a high current density of 5000mA / g, the material of the present invention still maintains 713mAh g -l The reversible capacity and capacity retention rate reached over 85%, proving the excellent battery performance.
[0020] The main innovation of the present invention is that a negative electrode material with a unique hollow core-shell silicon-carbon composite structure is prepared through a double-layer in-situ growth method, and the material exhibits excellent cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The present invention is a flow chart for preparing the hollow core-shell nano silicon-carbon composite material for the negative electrode of the lithium ion battery;
[0022] Figure 2 The XRD pattern of the hollow core-shell-Si@C composite material prepared in step 2 of Example 1;
[0023] Figure 3 This is the full XPS spectrum of the hollow core-shell-Si@C composite material prepared in step 2 of Example 1;
[0024] Figure 4 This is a SEM image of the hollow core-shell-Si@C composite material prepared in step 2 of Example 1, with a scale of 500 nm;
[0025] Figure 5 This is a SEM image of the hollow core-shell-Si@C composite material prepared in step 2 of Example 1, with a scale of 100 nm;
[0026] Figure 6The cycle performance diagram of the button battery prepared by the hollow core-shell-Si@C composite material prepared in step 2 of Example 1 at a current density of 200 mA / g, 1 is charging, 2 is discharging;
[0027] Figure 7 The cycle performance diagram of the button battery prepared by the hollow core-shell-Si@C composite material prepared in step 2 of Example 1 at a current density of 1000 mA / g (the first three cycles were activated at 200 mA / g), 1 is charging, 2 is discharging;
[0028] Figure 8 This is a cycle performance diagram of a button battery prepared using the hollow core-shell-Si@C composite material prepared in step 2 of Example 1 at a current density of 5000 mA / g (the first three cycles were activated at 200 mA / g), 1 is charging, and 2 is discharging. DETAILED DESCRIPTION
[0029] Specific implementation method 1: This implementation method is a method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery, which is carried out according to the following steps:
[0030] 1. Preparation of hollow core-shell-Si@C:
[0031] ① Add cobalt nitrate hexahydrate and 2-methylimidazole to methanol and mix by ultrasonic dispersion, then stir for 1 h to 12 h, age at room temperature, and finally collect the precipitate by centrifugation and washing to obtain ZIF-67;
[0032] ② Add ZIF-67 to ethanol and mix by ultrasonic dispersion, then add distilled water, tetraethyl orthosilicate and ammonia water and stir for 1h to 12h, finally collect the precipitate by centrifugation and washing to obtain ZIF-67 with in-situ growth of SiO2;
[0033] ③ Add the in-situ grown SiO2 ZIF-67 into ethanol and mix by ultrasonic dispersion, then add resorcinol, ammonia and formaldehyde and stir for 1h to 12h, finally collect the precipitate by centrifugation and washing to obtain the in-situ grown phenolic resin ZIF-67@SiO2;
[0034] ④ Add the ZIF-67@SiO2 grown in situ on phenolic resin into ethanol and disperse and mix by ultrasonication, then add hydrochloric acid and ultrasonicate, finally collect the precipitate by centrifugation and vacuum drying to obtain the hollow core-shell-SiO2@RF after etching the internal ZIF-67;
[0035] ⑤ In an Ar atmosphere at a temperature of 600°C to 800°C, the hollow core-shell-SiO2@RF after etching the internal ZIF-67 was calcined for 1h to 6h to obtain the hollow core-shell-SiO2@C;
[0036] ⑥ Mix the hollow core-shell-SiO2@C, Mg powder and NaCl, and pyrolyze them for 1h to 6h in an Ar / H2 atmosphere at a temperature of 600°C to 800°C to obtain a crude hollow core-shell-Si@C product;
[0037] 2. Treatment of Hollow Core-Shell-Si@C Crude Product:
[0038] The hollow core-shell-Si@C crude product was centrifuged with anhydrous ethanol, hydrochloric acid, deionized water, hydrofluoric acid and anhydrous ethanol in sequence, and finally dried to obtain a hollow core-shell-Si@C composite material.
[0039] Figure 1 The preparation flow chart of the hollow core-shell nano silicon-carbon composite material for the negative electrode of the lithium-ion battery of the present invention is as follows: first, a certain amount of cobalt nitrate hexahydrate and 2-methylimidazole are stirred to synthesize size-controlled ZIF-67 as the core, giving each nanoparticle a dodecahedral structure. Then, by The process generates a silicon dioxide (SiO2) layer in situ on ZIF-67, and then generates a phenolic resin (RF) layer in situ on the silicon dioxide layer through the polycondensation reaction between resorcinol and formaldehyde to form ZIF-67@SiO2@RF. Then, the internal ZIF-67 core is etched with hydrochloric acid, and the phenolic resin layer is carbonized under argon protection to obtain a hollow dodecahedral structure of hollow core-shell-SiO2@C; finally, through magnesium thermal reaction:
[0040] 2Mg(g)+SiO2(s)=Si(s)+2MgO(s);
[0041] The silicon dioxide layer inside the reduction structure is then centrifuged using anhydrous ethanol, hydrochloric acid, deionized water, hydrofluoric acid and anhydrous ethanol in sequence, and dried to obtain the final product, a silicon-carbon composite material with a hollow core-shell structure.
[0042] The beneficial effects of this embodiment are:
[0043] 1. Different from the general coating of traditional silicon-carbon materials, which will separate and fall off during the lithiation process, this embodiment implements a double-layer in-situ growth method to achieve a deeply integrated silicon-carbon composite material. The composite material synthesized by this method not only improves the conductivity of the silicon-based material, but also makes it difficult for silicon and carbon to separate during the lithiation process, thereby achieving cycle stability.
[0044] 2. This embodiment designs a unique hollow core-shell silicon-carbon composite structure. The outer carbon shell is used to enhance electron and ion transmission and act as a stress buffer, and the internal silicon nanoparticles are firmly attached to the carbon shell, effectively preventing separation and crushing during lithiation and delithiation. This structure can protect the internal silicon nanodots from direct contact with the electrolyte and provide a closed space for the inward contraction of silicon during lithium storage, which is conducive to the formation of a stable SEI layer and effectively avoids the crushing of silicon particles.
[0045] 3. The material prepared in this embodiment has excellent cycle stability due to its innovative preparation method and unique structure. After 250 cycles at a current density of 200 mA / g, its reversible capacity is 927.1 mAh g -1 After 800 cycles at a current density of 1000 mA / g, the reversible capacity is 883 mAh g -1 , and ultra-long cycle performance under high current is a very important characteristic of electrode materials. After running 3000 cycles at a high current density of 5000mA / g, the material of this embodiment still maintains 713mAh g -l The reversible capacity and capacity retention rate reached over 85%, proving the excellent battery performance.
[0046] The main innovation of this embodiment is that a negative electrode material with a unique hollow core-shell silicon-carbon composite structure is prepared through a double-layer in-situ growth method, and the material exhibits excellent cycle stability.
[0047] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that: the mass ratio of cobalt nitrate hexahydrate to 2-methylimidazole described in step 1① is 1:(6-12); the mass ratio of cobalt nitrate hexahydrate described in step 1① to methanol is 1g:(90-100)mL; in step 1①, stirring is performed at a speed of 200rpm-600rpm for 1h-12h; in step 1①, aging is performed at room temperature for 12h-24h. Others are the same as specific implementation method 1.
[0048] Specific implementation method three: This implementation method is different from specific implementation method one or two in that: the volume ratio of the mass of ZIF-67 described in step 1 ② to ethanol is 1g: (40-60) mL; the volume ratio of the mass of ZIF-67 described in step 1 ② to distilled water is 1g: (1-5) mL; the volume ratio of the mass of ZIF-67 described in step 1 ② to tetraethyl orthosilicate is 1g: (1-5) mL; the volume ratio of the mass of ZIF-67 described in step 1 ② to ammonia water is 1g: (1-5) mL; the mass percentage of ammonia water described in step 1 ② is 20%-40%; in step 1 ②, stirring is performed for 1h-12h at a rotation speed of 200rpm-600rpm. Others are the same as specific implementation method one or two.
[0049] Specific embodiment 4: This embodiment is different from one of specific embodiments 1 to 3 in that: the mass ratio of the ZIF-67 of the in-situ growth SiO2 described in step 1 ③ to ethanol is 1g: (40-60) mL; the mass ratio of the ZIF-67 of the in-situ growth SiO2 described in step 1 ③ to resorcinol is 1: (0.02-0.08); the mass ratio of the ZIF-67 of the in-situ growth SiO2 described in step 1 ③ to ammonia water is 1g: (0.1-0.4) mL; the mass ratio of the ZIF-67 of the in-situ growth SiO2 described in step 1 ③ to formaldehyde is 1g: (0.02-0.08) mL; the mass percentage of ammonia water described in step 1 ③ is 20%-40%; in step 1 ③, stirring is performed for 1h-12h at a rotation speed of 200rpm-600rpm. Others are the same as specific embodiments 1 to 3.
[0050] Specific implementation mode 5: This implementation mode is different from any one of specific implementation modes 1 to 4 in that: the mass ratio of the ZIF-67@SiO2 of the in-situ growth phenolic resin to the volume ratio of ethanol is 1g:(40-60)mL in step 1④; the mass ratio of the ZIF-67@SiO2 of the in-situ growth phenolic resin to the volume ratio of hydrochloric acid is 1g:(1-2)mL in step 1④; the concentration of hydrochloric acid in step 1④ is 0.1M-0.5M; hydrochloric acid is added in step 1④, and ultrasonication is performed for 5min-10min under the condition of ultrasonic power density of 10W / L-20W / L; vacuum drying in step 1④ is specifically performed at a temperature of 40℃-80℃ for 1h-12h. The rest is the same as specific implementation modes 1 to 4.
[0051] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that the ultrasonic dispersion mixing described in steps 1 ① to ④ is carried out under the condition of ultrasonic power density of 10W / L to 20W / L for 5min to 10min. The rest is the same as specific embodiments 1 to 5.
[0052] Specific embodiment 7: This embodiment is different from Specific embodiments 1 to 6 in that the centrifugal washing and collecting precipitate described in steps 1 ① to ④ is carried out by centrifugal washing with ethanol for 4 min to 10 min at a rotation speed of 4000 rpm to 6000 rpm, and the centrifugal washing is repeated 1 to 6 times. The rest is the same as Specific embodiments 1 to 6.
[0053] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that: in step 1⑤, the temperature is raised to 600°C to 800°C at a heating rate of 2°C / min to 10°C / min under Ar atmosphere. The rest is the same as specific embodiments 1 to 7.
[0054] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that: the mass ratio of the hollow core-shell-SiO2@C to Mg powder in step 1 ⑥ is 1:(1 to 3); the mass ratio of the hollow core-shell-SiO2@C to NaCl in step 1 ⑥ is 1:(1 to 15); the volume percentage of Ar gas in the Ar / H2 atmosphere in step 1 ⑥ is 90% to 95%; in step 1 ⑥, the temperature is raised to 600℃ to 800℃ at a heating rate of 2℃ / min to 10℃ / min under Ar / H2 atmosphere. Others are the same as specific embodiments 1 to 8.
[0055] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: the concentration of the hydrochloric acid in step 2 is 0.1M to 0.5M; the concentration of the hydrofluoric acid in step 2 is 0.1M to 0.5M; the centrifugal treatment in step 2 is specifically centrifuged at a speed of 4000rpm to 6000rpm for 4min to 10min respectively. The rest is the same as specific embodiments 1 to 9.
[0056] The following examples are used to verify the beneficial effects of the present invention:
[0057] Embodiment 1:
[0058] A method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery is carried out according to the following steps:
[0059] 1. Preparation of hollow core-shell-Si@C:
[0060] ① Add cobalt nitrate hexahydrate and 2-methylimidazole to methanol, and ultrasonically disperse for 10 minutes at an ultrasonic power density of 15 W / L, then stir for 1 hour at a speed of 250 rpm, and then age at room temperature for 24 hours. Finally, centrifuge and wash with ethanol for 5 minutes at a speed of 4000 rpm, and repeat the centrifugation washing 3 times to collect the precipitate to obtain ZIF-67;
[0061] The mass ratio of the cobalt nitrate hexahydrate to 2-methylimidazole is 1:11; the mass ratio of the cobalt nitrate hexahydrate to methanol is 1 g:92 mL;
[0062] ② Add ZIF-67 to ethanol and disperse it ultrasonically for 10 minutes at an ultrasonic power density of 15 W / L, then add distilled water, tetraethyl orthosilicate and ammonia water, and stir for 6 hours at a speed of 250 rpm. Finally, centrifuge and wash with ethanol for 5 minutes at a speed of 4000 rpm, and repeat the centrifugation washing 3 times to collect the precipitate to obtain ZIF-67 with in situ growth of SiO2;
[0063] The mass ratio of ZIF-67 to ethanol is 1 g:50 mL; the mass ratio of ZIF-67 to distilled water is 1 g:1 mL; the mass ratio of ZIF-67 to tetraethyl orthosilicate is 1 g:1 mL; the mass ratio of ZIF-67 to ammonia water is 1 g:2 mL; the mass percentage of ammonia water is 27%;
[0064] ③ Add the in-situ grown SiO2 ZIF-67 to ethanol and disperse it ultrasonically for 10 minutes at an ultrasonic power of 15 W / L, then add resorcinol, ammonia water and formaldehyde, and stir for 12 hours at a speed of 250 rpm, and finally centrifuge and wash with ethanol for 5 minutes at a speed of 4000 rpm, and repeat the centrifugation washing for 3 times, collect the precipitate, and obtain the in-situ grown phenolic resin ZIF-67@SiO2;
[0065] The mass ratio of the in-situ grown SiO2 ZIF-67 to ethanol is 1 g:50 mL; the mass ratio of the in-situ grown SiO2 ZIF-67 to resorcinol is 1:0.05; the mass ratio of the in-situ grown SiO2 ZIF-67 to ammonia water is 1 g:0.2 mL; the mass ratio of the in-situ grown SiO2 ZIF-67 to formaldehyde is 1 g:0.05 mL; the mass percentage of ammonia water is 27%;
[0066] ④ Add the in-situ grown phenolic resin ZIF-67@SiO2 to ethanol and disperse it ultrasonically for 10 minutes at an ultrasonic power of 15 W / L, then add hydrochloric acid and ultrasonicate it for 10 minutes at an ultrasonic power of 15 W / L, then centrifuge and wash it with ethanol at a speed of 4000 rpm for 5 minutes, repeat the centrifugation washing 3 times, collect the precipitate, and finally vacuum dry it at 60 ° C for 12 hours to obtain the hollow core-shell-SiO2@RF after etching the internal ZIF-67;
[0067] The mass ratio of the in-situ grown phenolic resin ZIF-67@SiO2 to ethanol is 1 g:50 mL; the mass ratio of the in-situ grown phenolic resin ZIF-67@SiO2 to hydrochloric acid is 1 g:1 mL; the concentration of the hydrochloric acid is 0.1 M;
[0068] ⑤ In an Ar atmosphere, the temperature was raised to 700°C at a heating rate of 5°C / min. Under the conditions of an Ar atmosphere and a temperature of 700°C, the hollow core-shell-SiO2@RF after etching the internal ZIF-67 was calcined for 3 h to obtain a hollow core-shell-SiO2@C;
[0069] ⑥ The hollow core-shell-SiO2@C, Mg powder and NaCl were mixed, heated to 680°C at a heating rate of 5°C / min in an Ar / H2 atmosphere, and then pyrolyzed for 6 hours in an Ar / H2 atmosphere at a temperature of 680°C to obtain a crude hollow core-shell-Si@C product;
[0070] The mass ratio of the hollow core-shell-SiO2@C to Mg powder is 1:1.2; the mass ratio of the hollow core-shell-SiO2@C to NaCl is 1:14; the volume percentage of Ar gas in the Ar / H2 atmosphere is 95%;
[0071] 2. Treatment of Hollow Core-Shell-Si@C Crude Product:
[0072] The hollow core-shell-Si@C crude product is centrifuged and treated with anhydrous ethanol, hydrochloric acid, deionized water, hydrofluoric acid and anhydrous ethanol in sequence, and finally dried to obtain a hollow core-shell-Si@C composite material;
[0073] The concentration of the hydrochloric acid is 0.1 M; the concentration of the hydrofluoric acid is 0.1 M; the centrifugal treatment is specifically carried out at a rotation speed of 4000 rpm for 5 minutes.
[0074] Figure 2 This is the XRD pattern of the hollow core-shell-Si@C composite material prepared in step 2 of Example 1. According to the XRD pattern, all Si characteristic diffraction peaks at 28.3°, 47.3° and 56.2° can be observed, corresponding to the (111), (220) and (311) planes of Si, respectively, which indicates that silicon is successfully synthesized and has good crystallinity.
[0075] Figure 3 This is the full XPS spectrum of the hollow core-shell-Si@C composite material prepared in step 2 of Example 1. According to the XPS graph, obvious peaks corresponding to C1s, Si 2s and Si 2p are displayed, proving that the method successfully synthesized the silicon-carbon composite.
[0076] Figure 4 This is a SEM image of the hollow core-shell-Si@C composite material prepared in step 2 of Example 1, with a scale of 500 nm. As can be seen from the figure, the hollow core-shell-Si@C composite material maintains the integrity and uniform dispersion of the dodecahedron.
[0077] Figure 5 This is an SEM image of the hollow core-shell-Si@C composite material prepared in step 2 of Example 1, with a scale of 100 nm. As can be seen from the figure, a double-layer in-situ growth method is used to prepare a composite material with an obvious hollow core-shell structure, in which the silicon layer is the core and the amorphous carbon layer is the shell.
[0078] Electrochemical test (the instrument for electrochemical test is LANHE CT2001A battery test system produced by Wuhan Landian Company, and the test voltage range is 0.005V~3V):
[0079] First, 60% of active material, 20% of conductive agent and 20% of binder are placed in a ceramic crucible according to the mass fraction. Among them, the active material is the hollow core-shell-Si@C composite material prepared in step 2 of Example 1, acetylene black is used as a conductive agent, and sodium carboxymethyl cellulose (CMC) is a binder. After adding a few drops of water (H2O) to obtain a viscous liquid, the rotor is stirred for 40 minutes to obtain a battery negative electrode active material slurry; the mass percentage of active material in the battery negative electrode active material slurry is 60%; then the battery negative electrode active material slurry is scraped with a scraper with a uniform thickness on a copper foil wiped clean and flat with anhydrous ethanol, and dried in a vacuum drying oven at 60°C for 3 hours to obtain a dried electrode sheet, and the dried electrode sheet is cut into a circular sheet with a diameter of 12 mm by a cutting machine to obtain a negative electrode sheet.
[0080] The negative electrode sheet was sent into an argon glove box, and the negative electrode shell, metal lithium sheet (as the counter electrode), diaphragm (microporous polypropylene membrane), dried electrode sheet, gasket and spring were placed in order, and then the positive battery shell was covered (2-3 drops of electrolyte were added between the electrodes and the diaphragm on both sides), and after assembly, it was packaged with a hydraulic sealing machine to obtain a packaged CR2032 button battery, in which the electrolyte was prepared by fully compounding a secondary electrolyte (LB-002) with a volume percentage of 95% and FEC (fluoroethylene carbonate) with a volume percentage of 5%. The packaged CR2032 button battery was taken out of the argon glove box, and the subsequent electrochemical performance test was carried out at room temperature after standing for 12 hours.
[0081] Figure 6The cycle performance diagram of the button battery prepared by the hollow core-shell-Si@C composite material prepared in step 2 of Example 1 at a current density of 200 mA / g, 1 is charging, 2 is discharging. As can be seen from the figure, the initial discharge capacity and charging capacity at a current density of 200 mA / g are 2776 mAh g -1 and 1498mAh g -1 After 250 cycles, the reversible capacity is 927.1 mAh g -1 , traditional silicon materials undergo dramatic volume changes during the lithiation process, and silicon and carbon fall off or separate, causing the electrode to break. This continuous mechanical decomposition damages the integrity of the electrode structure, which ultimately manifests as a gradual decrease in battery capacity. The material prepared using the double-layer in-situ growth method not only improves the conductivity of Si, but also makes it difficult for silicon and carbon to separate during the lithiation process. The hollow core-shell structure adjusts the expansion of silicon to inward contraction, effectively reducing the impact of repeated expansion of nano-silicon on the physical integrity of the electrode and ensuring its stability.
[0082] Figure 7 The cycle performance diagram of the button battery prepared by the hollow core-shell-Si@C composite material prepared in step 2 of Example 1 at a current density of 1000 mA / g (the first three cycles were activated at 200 mA / g), 1 is charging, 2 is discharging. As can be seen from the figure, after 800 cycles at a current density of 1000 mA / g, its reversible capacity is 883 mAh g -1 , compared with the reversible capacity of 1142 mAh g in the fourth cycle. -1 , the capacity retention rate is 77%.
[0083] Figure 8 The cycle performance diagram of the button battery prepared by the hollow core-shell-Si@C composite material prepared in step 2 of Example 1 at a current density of 5000 mA / g (the first three cycles were activated at 200 mA / g), 1 is charging, 2 is discharging. It can be seen from the figure that after running 3000 cycles at a high current density of 5000 mA / g, the capacity is still 713 mAh g -l The reversible capacity of hollow core-shell-Si@C is 837 mAh g after 3000 cycles. -1 It can still be stable at more than 85%, proving to have excellent cycle stability. This is due to the hollow core-shell dodecahedral structure hollow core-shell-Si@C formed by the double-layer in-situ growth, which significantly improves the conductivity and structural stability and is an effective conductive scaffold. This configuration not only expands the availability of active sites for lithium ion interaction, but also significantly reduces the volume strain associated with the lithiation / delithiation process, thereby obtaining high capacity and excellent stability.
Claims
1. A method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery, characterized in that It is carried out in the following steps:
1. Preparation of hollow core-shell-Si@C: ① Add cobalt nitrate hexahydrate and 2-methylimidazole to methanol and mix by ultrasonic dispersion, then stir for 1 h to 12 h, age at room temperature, and finally collect the precipitate by centrifugation and washing to obtain ZIF-67; ② Add ZIF-67 to ethanol and mix by ultrasonic dispersion, then add distilled water, tetraethyl orthosilicate and ammonia water and stir for 1h to 12h, finally collect the precipitate by centrifugation and washing to obtain ZIF-67 with in-situ growth of SiO2; ③ Add the in-situ grown SiO2 ZIF-67 into ethanol and mix by ultrasonic dispersion, then add resorcinol, ammonia and formaldehyde and stir for 1h to 12h, finally collect the precipitate by centrifugation and washing to obtain the in-situ grown phenolic resin ZIF-67@SiO2; ④ Add the ZIF-67@SiO2 grown in situ on phenolic resin into ethanol and disperse and mix by ultrasonication, then add hydrochloric acid and ultrasonicate, finally collect the precipitate by centrifugation and vacuum drying to obtain the hollow core-shell-SiO2@RF after etching the internal ZIF-67; ⑤ In an Ar atmosphere at a temperature of 600°C to 800°C, the hollow core-shell-SiO2@RF after etching the internal ZIF-67 was calcined for 1h to 6h to obtain the hollow core-shell-SiO2@C; ⑥ Mix the hollow core-shell-SiO2@C, Mg powder and NaCl, and pyrolyze them for 1h to 6h in an Ar / H2 atmosphere at a temperature of 600°C to 800°C to obtain a crude hollow core-shell-Si@C product; 2. Treatment of Hollow Core-Shell-Si@C Crude Product: The hollow core-shell-Si@C crude product was centrifuged with anhydrous ethanol, hydrochloric acid, deionized water, hydrofluoric acid and anhydrous ethanol in sequence, and finally dried to obtain a hollow core-shell-Si@C composite material.
2. The method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery according to claim 1, characterized in that The mass ratio of the cobalt nitrate hexahydrate to 2-methylimidazole described in step 1① is 1:(6-12); the volume ratio of the cobalt nitrate hexahydrate described in step 1① to methanol is 1g:(90-100)mL; in step 1①, stirring is performed at a rotation speed of 200rpm-600rpm for 1h-12h; in step 1①, aging is performed at room temperature for 12h-24h.
3. The method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery according to claim 1, characterized in that The volume ratio of the ZIF-67 described in step 1② to ethanol is 1g:(40-60)mL; the volume ratio of the ZIF-67 described in step 1② to distilled water is 1g:(1-5)mL; the volume ratio of the ZIF-67 described in step 1② to tetraethyl orthosilicate is 1g:(1-5)mL; the volume ratio of the ZIF-67 described in step 1② to ammonia water is 1g:(1-5)mL; the mass percentage of ammonia water described in step 1② is 20%-40%; in step 1②, stirring is carried out at a rotation speed of 200rpm-600rpm for 1h-12h.
4. The method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery according to claim 1, characterized in that The volume ratio of the mass of the ZIF-67 in situ grown SiO2 described in step 1③ to ethanol is 1g:(40~60)mL; the mass ratio of the ZIF-67 in situ grown SiO2 described in step 1③ to resorcinol is 1:(0.02~0.08); the volume ratio of the mass of the ZIF-67 in situ grown SiO2 described in step 1③ to ammonia water is 1g:(0.1~0.4)mL; the volume ratio of the ZIF-67 in situ grown SiO2 described in step 1③ to formaldehyde is 1g:(0.02~0.08)mL; the mass percentage of ammonia water described in step 1③ is 20%~40%; in step 1③, stirring is carried out at a rotation speed of 200rpm~600rpm for 1h~12h.
5. The method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery according to claim 1, characterized in that The volume ratio of the mass of the ZIF-67@SiO2 in situ grown phenolic resin described in step 1④ to ethanol is 1g:(40~60)mL; the volume ratio of the mass of the ZIF-67@SiO2 in situ grown phenolic resin described in step 1④ to hydrochloric acid is 1g:(1~2)mL; the concentration of the hydrochloric acid described in step 1④ is 0.1M~0.5M; hydrochloric acid is added to step 1④, and ultrasonic power density is 10W / L~20W / L, and ultrasonic is carried out for 5min~10min; vacuum drying described in step 1④ is specifically vacuum drying at a temperature of 40℃~80℃ for 1h~12h.
6. The method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery according to claim 1, characterized in that The ultrasonic dispersion mixing described in step 1 ① to ④ is specifically carried out under the condition of ultrasonic power density of 10W / L to 20W / L, and ultrasonic dispersion is carried out for 5min to 10min.
7. The method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery according to claim 1, characterized in that The centrifugal washing and collection of the precipitate described in steps 1 to 4 is specifically carried out at a rotation speed of 4000 rpm to 6000 rpm, using ethanol for centrifugal washing for 4 min to 10 min, and repeating the centrifugal washing 1 to 6 times.
8. The method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery according to claim 1, characterized in that In step 1⑤, under Ar atmosphere, the temperature is increased to 600°C to 800°C at a heating rate of 2°C / min to 10°C / min.
9. The method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery according to claim 1, characterized in that The mass ratio of the hollow core-shell-SiO2@C described in step 1⑥ to Mg powder is 1:(1~3); the mass ratio of the hollow core-shell-SiO2@C described in step 1⑥ to NaCl is 1:(1~15); the volume percentage of Ar gas in the Ar / H2 atmosphere described in step 1⑥ is 90%~95%; in step 1⑥, under Ar / H2 atmosphere, the temperature is increased to 600℃~800℃ at a heating rate of 2℃ / min~10℃ / min.
10. The method for preparing a hollow core-shell nano silicon-carbon composite material for a negative electrode of a lithium ion battery according to claim 1, characterized in that The concentration of the hydrochloric acid in step 2 is 0.1M to 0.5M; the concentration of the hydrofluoric acid in step 2 is 0.1M to 0.5M; the centrifugal treatment in step 2 is specifically carried out at a rotation speed of 4000rpm to 6000rpm for 4min to 10min respectively.
Citation Information
Patent Citations
Carbon-silicon composite lithium ion battery cathode material and preparation method thereof
CN105006549A
Preparation method for negative electrode material with core-shell coated structure and for lithium ion battery
CN106941164A
Si@C lithium-ion battery negative electrode material of core-shell structure and preparation method thereof
CN107359326A
Preparation method of Si@TiO2 hollow core-shell composite material
CN111477858A
Lithium ion battery silicon-carbon negative electrode material with internal and external multistage core-shell structure and preparation method of lithium ion battery silicon-carbon negative electrode material
CN116207231A