Single crystal type sodium ion battery positive electrode material and preparation method thereof

By pre-grinding the particle size of iron phosphate slurry and controlling pH value, combined with sintering treatment, a high-purity single-crystalline sodium ion battery positive electrode material was prepared, which solved the problem of low energy density of the sodium ion battery positive electrode material, significantly improving its Electrochemical properties.

CN118943336APending Publication Date: 2024-11-12ZHUHAI KECHUANG SODIUM ELECTRIC TECH CO LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202411187947.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The crystal phase purity and electrical properties of the positive electrode material of sodium ion battery are poor, resulting in low energy density.

Method used

By grinding the iron phosphate slurry to D90≤0.5 μm and mixing it with supplementary phosphorus source, sodium source, carbon source and deionized water to form a precursor slurry with a solid content of 15-60 wt%. The pH value is controlled at 7.4-8.2 Between, stirring, drying and sintering treatments were performed to obtain a precursor powder with a moisture content of less than 5 wt%, and then sintered under a protective atmosphere to obtain a monocrystalline sodium ion battery positive electrode material.

Benefits of technology

The crystal phase purity and electrochemical performance of the positive electrode material of single crystal sodium ion battery are improved, and the sodium storage capacity and cycle stability are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943336A_ABST
    Figure CN118943336A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a single crystal type sodium ion battery positive electrode material and a preparation method thereof. According to the preparation method, the iron phosphate slurry is pre-ground to the target particle size (D90 is less than or equal to 0.5 mu m) and then is mixed with the supplemented phosphorus source, sodium source, carbon source and deionized water to form the precursor slurry, so that the mixing uniformity of the phosphorus source, the sodium source, the carbon source and the iron phosphate in the precursor slurry is improved; the pH value of the precursor slurry is further controlled to be 7.4-8.2, and the reaction path of the iron-based complex is changed, so that the iron-based complex is easier to dissolve, and the reaction with phosphate radical (-PO4) and pyrophosphate radical (-P2O7) is facilitated; and then the single crystal type NFPP material with relatively high crystal phase purity is prepared through gradient sintering, so that the sodium storage capacity and the electrochemical performance of the NFPP material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and more specifically, to a single crystal sodium ion battery positive electrode material and a preparation method thereof. Background Art

[0002] Compared with lithium-ion positive electrode materials, sodium-ion positive electrode materials are relatively cheap, but they also face the problem of low energy density. On the one hand, it is attributed to the relatively low specific capacity of sodium-ion positive electrode materials, and on the other hand, the compaction density of sodium-ion positive electrode materials is generally smaller than that of lithium-ion positive electrode materials. Therefore, improving energy density can be done from two aspects. On the one hand, the energy density can be improved by increasing the specific capacity, and on the other hand, the energy density of the material can be improved by increasing the compaction density of the material. The capacity is determined by the element ratio and type of a specific material, and there is little room for improvement. The compaction density is closely related to the morphology of the material and the density of its own particles. Therefore, it is feasible and effective to improve the energy density of a specific proportion of materials by increasing the compaction density.

[0003] The patent document with the announcement number CN117228646A discloses a method for preparing a single-crystal sodium ferric pyrophosphate positive electrode material for sodium ion batteries, which improves the compaction density and cycle stability of the obtained single-crystal positive electrode material by treating the sodium ferric pyrophosphate positive electrode material into a single crystal. However, in the mixing stage of the precursor slurry of the patent, the mixing degree of various soluble auxiliary materials and the iron source (ferrous phosphate or ferrous oxalate) is poor, and if the pH value of the precursor slurry is high or low, the crystal phase purity and electrical properties of the finished product show poor results. Summary of the invention

[0004] In order to solve the problem of poor crystal phase purity and electrical performance of sodium ion battery positive electrode materials in the prior art, the purpose of the present invention is to provide a method for preparing a single crystal sodium ion battery positive electrode material, and the sodium ion battery positive electrode material prepared by this preparation method has higher crystal phase purity and electrical performance.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0007] S1: grinding the iron phosphate slurry to a particle size of D90≤0.5 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 15-60 wt%, and controlling the pH of the precursor slurry to be between 7.4-8.2;

[0008] S2: stirring and drying the precursor slurry in sequence to obtain a precursor powder having a water content of less than 5 wt %;

[0009] S3: Grind the precursor powder to a particle size of D90≤5μm, then sinter it under a protective atmosphere, take it out and crush it after natural cooling in the furnace to obtain a single crystal sodium ion battery positive electrode material.

[0010] Preferably, in step S3, nitrogen is introduced into the sintering furnace to make the oxygen content in the sintering furnace no greater than 500 ppm.

[0011] Preferably, in step S3, the precursor powder is first sintered in a sintering furnace at 300±5°C for 6 hours, then sintered at 580±5°C for 10 hours, and then naturally cooled.

[0012] Preferably, the single crystal sodium ion battery positive electrode material prepared in step S3 has a structure of carbon layer coated phosphate, and its structural formula is Na a Fe b (PO4) c (P2O7) d / C, where 2≤a≤4, 1≤b≤3, 0≤c≤2, 1≤d≤2.

[0013] Preferably, the structural formula of the single crystal sodium ion battery positive electrode material is Na4Fe3(PO4)2P2O7 / C.

[0014] Preferably, the carbon layer is 1-8 wt % of the single crystal sodium ion battery positive electrode material.

[0015] Preferably, the supplemental phosphorus source is selected from one or more of phosphoric acid, sodium dihydrogen phosphate, ammonium dihydrogen phosphate, ferric phosphate, sodium pyrophosphate and sodium dihydrogen pyrophosphate.

[0016] Preferably, the sodium source is selected from one or more of sodium carbonate, sodium bicarbonate, sodium oxalate, sodium acetate, sodium dihydrogen phosphate, sodium monohydrogen phosphate, sodium pyrophosphate and sodium dihydrogen pyrophosphate.

[0017] Preferably, the carbon source is selected from one or more of citric acid, oxalic acid, ascorbic acid, glucose, sucrose, fructose, polyethylene glycol, starch, carboxymethyl cellulose polyethylene, polypropylene, polystyrene, polyacrylonitrile, polyethylene glycol, starch, carboxymethyl cellulose, chitosan, maltodextrin, phenolic resin, epoxy resin and urea-formaldehyde resin.

[0018] Another object of the present invention is to provide a single crystal sodium ion battery positive electrode material, which is prepared by the aforementioned preparation method.

[0019] The present application has the following beneficial effects: based on full liquid phase mixing, the ferric phosphate slurry is pre-grinded to a target particle size (D90≤0.5μm), and then mixed with supplementary phosphorus source, sodium source, carbon source and deionized water to form a precursor slurry, thereby improving the mixing uniformity of the phosphorus source, sodium source, carbon source and ferric phosphate in the precursor slurry; the pH of the precursor slurry is further controlled between 7.4-8.2, the reaction path of the iron-based complex is changed, making it easier to dissolve and more conducive to reaction with phosphate (-PO4) and pyrophosphate (-P2O7); and then a single-crystal NFPP material with higher crystal phase purity is obtained by gradient sintering, thereby improving the sodium storage capacity and electrochemical performance of the NFPP material. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the XRD diagram of the finished product prepared in Example 1 of the present invention;

[0021] Figure 2 This is a SEM image of the finished product prepared in Example 1 of the present invention;

[0022] Figure 3 This is a test chart of the charging rate of the finished product prepared in Example 1 of the present invention.

[0023] Figure 4 This is a test diagram of the finished product power-on cycle prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] The present application is further described in detail below with reference to the accompanying drawings and embodiments.

[0025] Example 1

[0026] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, use sodium dihydrogen phosphate as the supplementary phosphorus source, glucose and citric acid mixed in a mass ratio of 1:2 as the carbon source, and sodium carbonate as the sodium source.

[0027] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0028] S1: grinding the particle size D90 of the iron phosphate slurry to 0.06 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 30 wt%, and controlling the pH of the precursor slurry to 7.4;

[0029] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0030] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0031] The single crystal sodium ion battery positive electrode material prepared above was subjected to X-ray diffraction test, and the results are as follows Figure 1 As shown, it indicates that the prepared single crystal sodium ion battery positive electrode material has a higher purity.

[0032] The single crystal sodium ion battery cathode material prepared above was observed by scanning electron microscope, and the results are as follows Figure 2 As shown, it shows that the process parameters of the preparation method are reasonable, the grain boundaries between the finished particles are clear, the finished product has a distinct single crystal morphology, the crystal phase purity is high, there are very few impurities, and the electrical performance test results are excellent.

[0033] The single crystal sodium ion battery positive electrode material prepared above was assembled into a battery and subjected to a 1C charge test at room temperature. The results are as follows Figure 3 As shown, the charge and discharge voltage range is 1.5-4.0V; the first three cycles are 0.2C current charge and discharge, the discharge specific capacity is 109.6mAh / g, and the discharge specific capacity is 106.4mAh / g when the current is 1C. In the form of a button half-cell, after 600 cycles with a current of 0.2C, the discharge specific capacity is 104.0mAh / g, and the capacity retention rate is 94.9%. Figure 4 As shown; it shows that the single crystal Na4Fe3(PO4)2P2O7 / C positive electrode material has very high cycle stability.

[0034] Example 2

[0035] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, use sodium dihydrogen phosphate as the supplementary phosphorus source, glucose and citric acid mixed in a mass ratio of 1:2 as the carbon source, and sodium carbonate as the sodium source.

[0036] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0037] S1: grinding the particle size D90 of the iron phosphate slurry to 0.1 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 40 wt%, and controlling the pH of the precursor slurry to 7.6;

[0038] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0039] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0040] Example 3

[0041] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, use sodium dihydrogen phosphate as the supplementary phosphorus source, glucose and citric acid mixed in a mass ratio of 1:2 as the carbon source, and sodium carbonate as the sodium source.

[0042] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0043] S1: grinding the particle size D90 of the iron phosphate slurry to 0.2 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 45 wt%, and controlling the pH of the precursor slurry to 7.8;

[0044] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0045] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0046] Example 4

[0047] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, use sodium dihydrogen phosphate as the supplementary phosphorus source, glucose and citric acid mixed in a mass ratio of 1:2 as the carbon source, and sodium carbonate as the sodium source.

[0048] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0049] S1: grinding the particle size D90 of the iron phosphate slurry to 0.4 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 50 wt%, and controlling the pH of the precursor slurry to 8.0;

[0050] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0051] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0052] Example 5

[0053] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, use sodium dihydrogen phosphate as the supplementary phosphorus source, glucose and citric acid mixed in a mass ratio of 1:2 as the carbon source, and sodium carbonate as the sodium source.

[0054] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0055] S1: grinding the particle size D90 of the iron phosphate slurry to 0.5 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 55 wt%, and controlling the pH of the precursor slurry to 8.2;

[0056] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0057] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0058] Comparative Example 1

[0059] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, use sodium dihydrogen phosphate as the supplementary phosphorus source, glucose and citric acid mixed in a mass ratio of 1:2 as the carbon source, and sodium carbonate as the sodium source.

[0060] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0061] S1: grinding the particle size D90 of the iron phosphate slurry to 0.64 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 30 wt%, and controlling the pH of the precursor slurry to 7.4;

[0062] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0063] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0064] Comparative Example 2

[0065] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, use sodium dihydrogen phosphate as the supplementary phosphorus source, glucose and citric acid mixed in a mass ratio of 1:2 as the carbon source, and sodium carbonate as the sodium source.

[0066] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0067] S1: grinding the particle size D90 of the iron phosphate slurry to 1.23 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 30 wt%, and controlling the pH of the precursor slurry to 7.6;

[0068] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0069] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0070] Comparative Example 3

[0071] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, use sodium dihydrogen phosphate as the supplementary phosphorus source, glucose and citric acid mixed in a mass ratio of 1:2 as the carbon source, and sodium carbonate as the sodium source.

[0072] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0073] S1: directly preparing an iron phosphate slurry, and then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 30 wt%, and controlling the pH of the precursor slurry to be 7.3;

[0074] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0075] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0076] Comparative Example 4

[0077] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, use sodium dihydrogen phosphate as the supplementary phosphorus source, glucose and graphite mixed in a mass ratio of 1:1 as the carbon source, and sodium carbonate as the sodium source.

[0078] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0079] S1: grinding the particle size D90 of the iron phosphate slurry to 0.06 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 30 wt%, and controlling the pH of the precursor slurry to be 10.8;

[0080] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0081] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0082] Comparative Example 5

[0083] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, using sodium dihydrogen phosphate as the supplementary phosphorus source, citric acid as the carbon source, and sodium carbonate as the sodium source.

[0084] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0085] S1: grinding the particle size D90 of the iron phosphate slurry to 0.06 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 30 wt%, and controlling the pH of the precursor slurry to 4.5;

[0086] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0087] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0088] Comparative Example 6

[0089] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, use sodium dihydrogen phosphate as the supplementary phosphorus source, glucose and citric acid mixed in a mass ratio of 1:2 as the carbon source, and sodium carbonate as the sodium source.

[0090] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0091] S1: directly preparing an iron phosphate slurry, and then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 30 wt%, and controlling the pH of the precursor slurry to be 4.5;

[0092] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0093] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0094] Comparative Example 7

[0095] According to formula (I): Na4Fe3(PO4)2P2O7 / C→4 sodium sources + 2.91FePO4 + 1.09 supplementary phosphorus source + 1 carbon source, prepare the raw materials, using sodium dihydrogen phosphate as the supplementary phosphorus source, graphite as the carbon source, and sodium carbonate as the sodium source.

[0096] A method for preparing a single crystal sodium ion battery positive electrode material comprises the following steps:

[0097] S1: directly preparing an iron phosphate slurry, and then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 30 wt%, and controlling the pH of the precursor slurry to be 11.1;

[0098] S2: using an emulsifying disperser with a speed of 6000-12000 r / min to mix the components in the precursor slurry evenly, using spray drying according to a method well known to those skilled in the art, adjusting the air inlet temperature to 230±5°C and the air outlet temperature to 95±5°C, to obtain a precursor powder with a moisture content of less than 5wt%;

[0099] S3: Use air flow milling to grind the precursor powder to a particle size of D90≤5μm, then put it into a sintering furnace, introduce nitrogen and make the oxygen content in the sintering furnace not more than 500ppm, and then carry out a temperature increase program, first sinter at 300±5℃ for 6h, continue to heat at a rate of 2℃ / min, and then sinter at 580±5℃ for 10h, then cool naturally, take out, and crush to D50=2-4μm to obtain a single crystal sodium ion battery positive electrode material.

[0100] The performance of the single crystal sodium ion battery positive electrode materials prepared in the above Examples 1-5 and Comparative Examples 1-7 was tested, and the following data were obtained:

[0101] Table 1 Test performance table

[0102]

[0103] As can be seen from Table 1, the present application improves the mixing uniformity of the phosphorus source, sodium source, carbon source and iron phosphate in the precursor slurry by pre-grinding the iron phosphate slurry to the target particle size (D90≤0.5μm) and then mixing it with supplementary phosphorus source, sodium source, carbon source and deionized water to form a precursor slurry; further controls the pH of the precursor slurry between 7.4-8.2, changes the reaction path of the iron-based complex, makes it easier to dissolve, and is more conducive to reaction with phosphate (-PO4) and pyrophosphate (-P2O7); and then obtains a single-crystal NFPP material with higher crystal phase purity through gradient sintering, thereby improving the sodium storage capacity and electrochemical properties of the NFPP material.

[0104] The above specific embodiments are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they are protected by the patent law.

Claims

1. A method for preparing a single crystal sodium ion battery positive electrode material, characterized in that: The following steps are involved: S1: grinding the iron phosphate slurry to a particle size of D90≤0.5 μm, then adding a supplementary phosphorus source, a sodium source, a carbon source and deionized water to prepare a precursor slurry with a solid content of 15-60 wt%, and controlling the pH of the precursor slurry to be between 7.4-8.2; S2: stirring and drying the precursor slurry in sequence to obtain a precursor powder having a water content of less than 5 wt %; S3: Grind the precursor powder to a particle size of D90≤5μm, then sinter it under a protective atmosphere, take it out and crush it after natural cooling in the furnace to obtain a single crystal sodium ion battery positive electrode material.

2. The method for preparing a single crystal sodium ion battery positive electrode material according to claim 1, characterized in that: In step S3, nitrogen is introduced into the sintering furnace to make the oxygen content in the sintering furnace no greater than 500 ppm.

3. The method for preparing a single crystal sodium ion battery positive electrode material according to claim 1, characterized in that: In step S3, the precursor powder is first sintered in a sintering furnace at 300±5°C for 6 hours, then sintered at 580±5°C for 10 hours, and then naturally cooled.

4. The method for preparing a single crystal sodium ion battery positive electrode material according to claim 1, characterized in that: The single crystal sodium ion battery positive electrode material prepared in step S3 has a structure of carbon layer coated phosphate, and its structural formula is Na a Fe b (PO4) c (P2O7) d / C, where 2≤a≤4, 1≤b≤3, 0≤c≤2, 1≤d≤2.

5. The method for preparing a single crystal sodium ion battery positive electrode material according to claim 4, characterized in that: The structural formula of the single crystal sodium ion battery positive electrode material is Na4Fe3(PO4)2P2O7 / C.

6. The method for preparing a single crystal sodium ion battery positive electrode material according to claim 4, characterized in that: The carbon layer is 1-8wt% of the single crystal sodium ion battery positive electrode material.

7. The method for preparing a single crystal sodium ion battery positive electrode material according to claim 1, characterized in that: The supplementary phosphorus source is selected from one or more of phosphoric acid, sodium dihydrogen phosphate, ammonium dihydrogen phosphate, ferric phosphate, sodium pyrophosphate and sodium dihydrogen pyrophosphate.

8. The method for preparing a single crystal sodium ion battery positive electrode material according to claim 1, characterized in that: The sodium source is selected from one or more of sodium carbonate, sodium bicarbonate, sodium oxalate, sodium acetate, sodium dihydrogen phosphate, sodium monohydrogen phosphate, sodium pyrophosphate and sodium dihydrogen pyrophosphate.

9. The method for preparing a single crystal sodium ion battery positive electrode material according to claim 1, characterized in that: The carbon source is selected from one or more of citric acid, oxalic acid, ascorbic acid, glucose, sucrose, fructose, polyethylene glycol, starch, carboxymethyl cellulose polyethylene, polypropylene, polystyrene, polyacrylonitrile, polyethylene glycol, starch, carboxymethyl cellulose, chitosan, maltodextrin, phenolic resin, epoxy resin and urea-formaldehyde resin.

10. A single crystal sodium ion battery positive electrode material, characterized in that: The positive electrode material of a single-crystal sodium ion battery is prepared by the method for preparing the positive electrode material of a single-crystal sodium ion battery according to any one of claims 1 to 9.

Citation Information

Cited By

  • Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery

    CN119581540A

  • High-compaction-density ferric sodium pyrophosphate positive electrode material and preparation method thereof

    CN119929768A

  • Pyrophosphate ferric sodium phosphate / C composite material and preparation and application thereof in sodium ion battery

    CN120057883A

  • Spherical monocrystal-like sodium ferric phosphate pyrophosphate material, preparation method and application thereof, and sodium ion battery

    CN122585985A

  • Flaky single-crystal sodium iron phosphate positive electrode material based on external magnetic field induction growth and preparation method and application thereof

    CN123026205A