Long-circulation high-nickel ternary positive electrode material and preparation method thereof

The high-nickel ternary cathode material is ground or heated by sulfide or sulfur element, replacing its shallow surface oxygen ions, solving the material stability and life problems and achieving better cycling performance and energy density.

CN118943361AActive Publication Date: 2024-11-12安徽得壹能源科技有限公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411246953.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-12
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Due to the high nickel content, high nickel ternary cathode material has reduced stability, increased surface residual alkali, increased interface side reaction with the electrolyte, enhanced water absorption, and shortened its service life.

Method used

By grinding or heating treatment with sulfide or sulfur element and high-nickel ternary cathode material, the surface of the material is reconstructed by replacing the shallow surface oxygen ions, thereby inhibiting oxygen release and structural collapse and improving cycling performance.

Benefits of technology

It significantly extends the life of high-nickel ternary cathode material, improves its cycling performance, reduces side reactions with the electrolyte, and increases energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005031052340000011
    Figure HDA0005031052340000011
Patent Text Reader

Abstract

The invention discloses a long-circulation high-nickel ternary positive electrode material and a preparation method thereof. The shallow layer oxygen of the high-nickel ternary positive electrode material is substituted by anion sulfur. The high-nickel ternary positive electrode material is long in service life and good in cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium batteries, and in particular to a long-cycle high-nickel ternary positive electrode material and a preparation method thereof. Background Art

[0002] With the rapid growth of electric vehicles in recent years, along with the increasingly prominent problem of battery life anxiety, the demand for lithium batteries for materials with higher energy density is increasing. High-nickel ternary positive electrode materials have a high reversible energy density, which to a certain extent meets people's needs for long battery life and has gradually been widely used in new energy electric vehicles. However, due to the high nickel content, high-nickel ternary positive electrode materials have reduced material stability, significantly increased surface residual alkali, increased interfacial side reactions with the electrolyte, enhanced water absorption, etc., which in turn seriously affects the service life of high-nickel ternary positive electrode materials.

[0003] In order to solve the problem of short cycle life of high-nickel ternary positive electrode materials, the industry usually adopts doping, multi-element doping, water washing and surface modification methods to suppress or improve it. For example: Patent CN113764647A discloses a ternary positive electrode material co-doped with Zr and multiple anions, its preparation method and lithium-ion battery, using various combinations of zirconium and fluorine, chlorine and sulfur, and using a co-precipitation method to prepare the corresponding ternary precursor, and then using a high-temperature solid phase method to prepare the corresponding ternary positive electrode material. Since the atmosphere used in the preparation of the ternary positive electrode material is oxidizing, the S claimed in the patent is 2- As a kind of polyanion source, it has theoretical errors; Patent CN114162881A discloses a fluorine-doped ternary cathode material, which uses a coprecipitation method to precipitate fluorine into the precursor during the precursor preparation process, and then uses the precursor to mix with a lithium source, and finally obtains a fluorine-doped ternary cathode material by a high-temperature solid phase method. Although fluorine doping can inhibit the oxygen precipitation of ternary cathode materials to a certain extent, fluorine has a high corrosion intensity on equipment, and the patent adopts a coprecipitation method, and the distribution of fluorine is relatively uniform. While improving the oxygen precipitation problem of ternary cathode materials, it leads to a serious deterioration in the energy density of the material. Summary of the invention

[0004] In view of the defects of the prior art that medium-lithium ion high-nickel ternary positive electrode materials release oxygen and have serious side reactions with the electrolyte, resulting in poor life and cycle performance of the high-nickel ternary positive electrode materials, the present invention provides a long-cycle high-nickel ternary positive electrode material and a preparation method thereof. The present invention uses sulfide or sulfur to replace part of the oxygen in the shallow surface layer of the high-nickel ternary positive electrode material by grinding or heating, thereby reconstructing the shallow surface layer of the high-nickel ternary positive electrode material to achieve the above-mentioned improvement.

[0005] In the first aspect of the present invention, the present invention proposes a high-nickel ternary positive electrode material. According to an embodiment of the present invention, the shallow surface oxygen of the high-nickel ternary positive electrode material is replaced by anionic sulfur. The high-nickel ternary positive electrode material according to the embodiment of the present invention has a long life and good cycle performance.

[0006] In another aspect of the present invention, the present invention provides a method for preparing a high-nickel ternary positive electrode material. According to an embodiment of the present invention, the method comprises:

[0007] 1) mixing the high-nickel ternary positive electrode material to be treated with a sulfur source to obtain a mixture;

[0008] 2) Grinding or heating the mixture to obtain the high-nickel ternary positive electrode material. The high-nickel ternary positive electrode material obtained by the method of the embodiment of the present invention has a long life and good cycle performance.

[0009] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:

[0010] According to an embodiment of the present invention, the sulfur source is sulfur or sulfide. The present invention uses sulfide or sulfur to replace part of the oxygen in the shallow surface layer of the high-nickel ternary positive electrode material by grinding or heating, thereby reconstructing the shallow surface layer of the high-nickel ternary positive electrode material to achieve the above improvement.

[0011] According to an embodiment of the present invention, the sulfide includes one or more selected from zinc disulfide, carbon disulfide, molybdenum disulfide, lithium sulfide, phosphorus pentasulfide, and ammonium sulfide.

[0012] According to an embodiment of the present invention, the mass ratio of the sulfur source to the high-nickel ternary positive electrode material to be treated is 1000-3000 ppm, wherein the sulfur source is measured in terms of sulfur element.

[0013] According to an embodiment of the present invention, the temperature of the heating treatment is 100-150°C.

[0014] According to an embodiment of the present invention, the heating treatment time is 6 to 10 hours.

[0015] According to an embodiment of the present invention, the heating treatment further includes cooling the heated material to room temperature and crushing and screening the material.

[0016] In another aspect of the present invention, the present invention further provides a high-nickel ternary positive electrode material. According to an embodiment of the present invention, the high-nickel ternary positive electrode material is prepared according to the method described above.

[0017] In another aspect of the present invention, the present invention further provides a battery. According to an embodiment of the present invention, the battery comprises the high-nickel ternary positive electrode material described above or the high-nickel ternary positive electrode material prepared according to the method described above.

[0018] According to an embodiment of the present invention, sulfur ions are Lewis bases and can absorb hydrogen fluoride produced in the electrolyte to a certain extent, thereby inhibiting the corrosion of hydrogen fluoride on the surface of the high-nickel ternary positive electrode material, thereby achieving the effect of improving the cycle life of the ternary positive electrode material; at the same time, sulfur ions replace part of the oxygen ions in the shallow surface layer of the high-nickel ternary positive electrode material particles, so that the shallow surface layer of the ternary positive electrode material is reconstructed, which can effectively inhibit the release of oxygen on the surface of the high-nickel ternary positive electrode material and the structural collapse caused by the oxygen release, thereby improving the gas production problem and cycle life problem of the high-nickel positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0020] Figure 1 is the cycle discharge capacity of the button battery according to the embodiment of the present invention. DETAILED DESCRIPTION

[0021] The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0022] Example 1

[0023] A certain amount of high-nickel ternary positive electrode material (the molar content of nickel is Ni / (Ni+Co+Mn)≥0.8) and ammonium sulfide are weighed respectively, and the mass ratio of sulfur element in ammonium sulfide to high-nickel ternary positive electrode material is 2000ppm. Then the two materials are mixed evenly, and then the mixture is heat-treated at 130°C in an inert atmosphere for 8h. Finally, the heat-treated material is cooled to room temperature, and crushed and screened in a temperature-controlled environment to obtain an anion-modified high-nickel ternary positive electrode material.

[0024] Example 2

[0025] A certain amount of high-nickel ternary positive electrode material (the molar content of nickel is Ni / (Ni+Co+Mn)≥0.8) and ammonium sulfide are weighed respectively, and the mass ratio of sulfur element in ammonium sulfide to high-nickel ternary positive electrode material is 3000ppm. Then the two materials are mixed evenly, and then the mixture is heat-treated at 100°C in an inert atmosphere for 15h. Finally, the heat-treated material is cooled to room temperature, and crushed and screened in a temperature-controlled environment to obtain an anion-modified high-nickel ternary positive electrode material.

[0026] Example 3

[0027] A certain amount of high-nickel ternary positive electrode material (the molar content of nickel is Ni / (Ni+Co+Mn)≥0.8) and ammonium sulfide are weighed separately, and the mass ratio of sulfur element in ammonium sulfide to high-nickel ternary positive electrode material is 1000ppm. Then the two materials are mixed evenly, and then the mixture is heat treated at 150°C in an inert atmosphere for 6h. Finally, the heat-treated material is cooled to room temperature, and crushed and screened in a temperature-controlled environment to obtain an anion-modified high-nickel ternary positive electrode material.

[0028] Comparative Example 1

[0029] A certain amount of high-nickel ternary positive electrode material (nickel molar content ratio is Ni / (Ni+Co+Mn)≥0.8) is weighed and crushed and screened in a temperature-controlled environment.

[0030] Comparative Example 2

[0031] A certain amount of high-nickel ternary positive electrode material (nickel molar content ratio is Ni / (Ni+Co+Mn)≥0.8) was weighed, and then the high-nickel ternary positive electrode material was heat treated at 130°C in an inert atmosphere for 8 hours. Finally, the heat-treated material was cooled to room temperature and crushed and screened in a temperature-controlled environment.

[0032] Preparation of button cells: Preparation of button cells: The positive electrode materials prepared in the above Examples 1 to 2 and Comparative Examples 1 to 2 are respectively assembled as follows: The positive electrode material, the conductive agent (acetylene black) and the binder (PVDF) are weighed in a mass ratio of 90%:5%:5%, and the weighed positive electrode material and acetylene black are mixed and ground in an agate mortar. After grinding evenly, they are added to N-methylpyrrolidone (NMP) that has been fully reacted with PVDF and continuously ground until the slurry becomes a viscous liquid with a certain fluidity. The ground slurry is evenly transferred to aluminum foil, and the sample is evenly coated with a coater with a thickness of 300 μm, followed by pre-baking in air at 60°C for 5 hours, and then vacuuming and drying at 90°C for 12 hours to achieve the purpose of removing water and organic matter in the coated sample, and the electrode sheet is cut out according to size for use to obtain the positive electrode sheet.

[0033] The lithium sheet was used as the negative electrode, the prepared electrode sheet was used as the positive electrode, the electrolyte ratio was EC:DMC=1:1, and button cells were assembled. The charge and discharge test was performed using a BTV charge and discharge tester. At 25°C, the lithium-ion battery assembled with the above positive electrode sheet was charged and discharged at 0.5C / 1C at a working voltage of 3.0-4.3V. The button battery cycle discharge capacity curve is shown in Figure 1 ,from Figure 1It can be seen that the cycle of Example 1 and Example 2 is significantly improved compared with Comparative Example 1, and the dry coating cycle is also significantly improved compared with Comparative Example 2.

[0034] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0035] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A high-nickel ternary positive electrode material, characterized in that: The shallow surface oxygen of the high-nickel ternary positive electrode material is replaced by anionic sulfur.

2. A method for preparing a high-nickel ternary positive electrode material, characterized in that: include: 1) mixing the high-nickel ternary positive electrode material to be treated with a sulfur source to obtain a mixture; 2) Grinding or heating the mixture to obtain the high-nickel ternary positive electrode material.

3. The method according to claim 2, characterized in that The sulfur source is sulfur element or sulfide.

4. The method according to claim 3, characterized in that The sulfide includes one or more selected from zinc disulfide, carbon disulfide, molybdenum disulfide, lithium sulfide, phosphorus pentasulfide, and ammonium sulfide.

5. The method according to claim 2, characterized in that: The mass ratio of the sulfur source to the high-nickel ternary positive electrode material to be treated is 1000-3000 ppm, wherein the sulfur source is measured in terms of sulfur element.

6. The method according to claim 2, characterized in that The temperature of the heating treatment is 100-150°C.

7. The method according to claim 2, characterized in that The heating treatment time is 6 to 10 hours.

8. The method according to claim 2, characterized in that: The heating treatment further includes cooling the heated material to room temperature and crushing and screening the material.

9. A high-nickel ternary positive electrode material, characterized in that: The high-nickel ternary positive electrode material is prepared by the method according to any one of claims 2-8.

10. A battery, characterized in that: The battery comprises the high-nickel ternary positive electrode material according to claim 1 or 9 or the high-nickel ternary positive electrode material prepared by the method according to any one of claims 2-8.

Citation Information

Patent Citations

  • Method for preparing anode material for lithium ion batteries

    CN101986441A

  • Molybdenum disulfide-coated lithium nickel cobalt manganate composite material, and preparation method and application thereof

    CN108832089A

  • A high nickel large-grain ternary material and a preparation method thereof

    CN109216697A

  • Positive electrode material surface modification method and positive electrode material prepared by method

    CN110635131A

  • Positive electrode active material for rechargeable lithium ion battery, preparing method of the same, and rechargeable lithium ion battery comprising the same

    CN112939036A