Negative electrode active material, negative electrode active slurry, negative electrode plate and preparation method

By using specific design carbon-based materials in lithium-ion batteries, including primary and secondary particle carbon-based materials, controlling their aspect ratio and mass fraction, combining graphitization degree and cladding, the energy density of the negative electrode material and The problem of unknown temperature coefficient relationship has achieved a balance between high energy density and good temperature coefficient, and improved the low-temperature discharge capability and interface transmission efficiency.

CN118943363APending Publication Date: 2024-11-12ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411093825.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The relationship between the energy density and temperature coefficient of the negative electrode materials of existing lithium-ion batteries is unknown, and the effect of use at room temperature cannot be guaranteed.

Method used

Using negative electrode active materials including primary particle carbon-based materials and secondary particle carbon-based materials, control their aspect ratio and mass fraction, and combine the graphitization degree and cladding design to ensure high energy density and temperature coefficient are not due to energy density. Increase and greatly decay.

Benefits of technology

High energy density and good temperature coefficient are achieved, overvoltage is avoided, low-temperature discharge capacity and interface transmission impedance are improved, and cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004987295690000091
    Figure BDA0004987295690000091
  • Figure BDA0004987295690000092
    Figure BDA0004987295690000092
  • Figure BDA0004987295690000101
    Figure BDA0004987295690000101
Patent Text Reader

Abstract

The invention discloses a negative active material, negative active slurry, a negative pole piece and a preparation method. The negative electrode active material comprises a carbon-based material, the carbon-based material comprises a primary particle carbon-based material and a secondary particle carbon-based material, the length-diameter ratio a of the primary particle carbon-based material is 1-2, the length-diameter ratio b of the secondary particle carbon-based material is 3-4, and the mass fraction M1 of the primary particle carbon-based material in the carbon-based material is greater than or equal to 0% and less than or equal to 30%. The mass fraction M2 of the secondary particle carbon-based material in the carbon-based material satisfies 70% < = M2 < = 100%. Compared with the prior art, the prepared negative electrode active material is high in energy density, and the temperature coefficient of the negative electrode active material is not greatly attenuated due to the increase of the energy density of the negative electrode active material. Furthermore, the negative electrode active material can be coated with a soft and hard carbon structure layer, and the coating layer can enable the negative electrode active material to be good in low-temperature discharge capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium ion batteries, and in particular relates to a negative electrode active material, a negative electrode active slurry, a negative electrode plate and a preparation method thereof. Background Art

[0002] Nowadays, lithium-ion batteries have become energy storage devices for mainstream electronic products. While people have higher requirements for the energy density and normal use of lithium-ion batteries at room temperature, they also require that the temperature coefficient of the battery be guaranteed. Energy density refers to the amount of electrical energy that can be stored per unit volume or mass of a battery. For lithium-ion batteries, first of all, it is necessary to increase their energy density as much as possible and ensure that their temperature coefficient reaches a certain value so that their use at room temperature can be guaranteed.

[0003] Chinese patent CN 114464774 A discloses a negative electrode plate and its application. The negative electrode plate includes a current collector and a negative electrode material layer arranged on the surface of the current collector. The negative electrode material layer includes a carbon-based material. The carbon-based material includes a primary particle carbon material, a secondary particle carbon material and a carbon coating layer coated on the surface of the secondary particle carbon material. The performance factor i of the negative electrode plate is 0.2 to 10. The expression of the performance factor i is: [(SSA*(D v 90-D v 50) / (D v 50-D v 10))+P*D v 50]*I D / I G , formula (I); wherein SSA is the specific surface area value of the carbon-based material, and the unit corresponding to the specific surface area value is m 2 / g;D v 10. D v 50, Dv90 are the particle size values ​​corresponding to the volume percentage of carbon-based materials reaching 10%, 50%, and 90%, respectively, and the unit corresponding to the particle size value is μm; P is the porosity value of the negative electrode material layer; I D / I G It is the ratio of the peak heights of the D peak and the G peak of the Raman spectrum of the carbon-based material. However, the relationship between the energy density and the temperature coefficient of the negative electrode material in the prior art is unknown, and its use at room temperature cannot be guaranteed.

[0004] In view of this, it is indeed necessary to provide a technical solution to the above problems. Summary of the invention

[0005] One of the purposes of the present invention is to provide a negative electrode active material to address the deficiencies of the prior art, wherein the negative electrode active material has a high energy density and the temperature coefficient does not significantly decay due to the increase of its energy density.

[0006] In order to achieve the above-mentioned purpose, the present invention provides a negative electrode active material, which includes a carbon-based material, and the carbon-based material includes a primary particle carbon-based material and a secondary particle carbon-based material. The aspect ratio a of the primary particle carbon-based material is between 1 and 2, and the aspect ratio b of the secondary particle carbon-based material is between 3 and 4. The mass fraction M1 of the primary particle carbon-based material in the carbon-based material satisfies the range of 0%≤M1≤30%, and the mass fraction M2 of the secondary particle carbon-based material in the carbon-based material satisfies the range of 70%≤M2≤100%; the proportion k of the part with R≤0.15 in the carbon-based material satisfies the range of k≥10%; and R refers to the ratio of the peak intensity of the D peak to the peak intensity of the G peak of the Raman spectrum of the carbon-based material.

[0007] Among them, the above parameters can be adjusted according to actual needs. For example, a can be 1, 1.2, 1.4, 1.6, 1.8 or 2; b can be 3, 3.2, 3.4, 3.6, 3.8 or 4; M1 can be 0%, 5%, 10%, 15%, 20%, 25% or 30%; M2 can be 70%, 75%, 80%, 85%, 90%, 95% or 100%; k can be 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%.

[0008] The negative electrode active material prepared by the present invention has a high energy density, and its temperature coefficient does not significantly decay due to the increase of its energy density. This is because the aspect ratio of the primary particle carbon-based material and the secondary particle carbon-based material in the present invention is controlled within the range disclosed in the technical solution of the present invention. The inventors have found that when the aspect ratio of the secondary particle carbon-based material is in the range of 3 to 4, the secondary particle carbon-based material is in the form of flakes, has better extension and sliding properties during rolling, and has a higher compaction density; when the aspect ratio of the primary particle carbon-based material is in the range of 1 to 2, the primary particle carbon-based material is rounder in shape, has higher isotropy, can achieve a higher operating voltage, and has a better temperature coefficient; the combination of two particles with different aspect ratios has a higher energy density, because the primary particle carbon-based material with a mass fraction of 0% to 30% can improve the temperature coefficient and avoid the existence of overvoltage, while the secondary particle carbon-based material with a mass fraction of 70% to 100% can provide high energy density. When the primary particle carbon-based material and the secondary particle carbon-based material disclosed in the present invention are within the mass fraction range disclosed in the present invention, the negative electrode active material can have a high energy density and the temperature coefficient does not significantly attenuate due to the increase in its energy density.

[0009] It should be noted that the R value is measured by a laser Raman spectrometer, and the measured R value is in the form of a distribution graph. k is obtained by counting the R values ​​within a certain range. The method for measuring the R value and the k value is a method in the prior art. The specific method for measuring the R value is: using a laser microscopic confocal Raman spectrometer to test the surface defect degree of the negative electrode active material, using the sample at 1350cm -1 The peak intensity of D at I D With 1580cm -1 The peak intensity of G at I G The ratio I D / I G The value represents the surface defect degree of the sample.

[0010] Furthermore, the graphitization degree G1 of the primary particle carbon-based material satisfies the range of 93%≤G1≤97%, and the graphitization degree G2 of the secondary particle carbon-based material satisfies the range of 90%≤G2≤93%. The specific values ​​of G1 and G2 can be adjusted according to actual needs, for example: G1 can be 93%, 94%, 95%, 96% or 97%; G2 can be 90%, 91%, 92% or 93%.

[0011] The mass fraction of the degree of graphitization of the carbon-based material used in the present invention is limited because the higher the degree of graphitization of the carbon-based material, the closer the gram capacity is to the theoretical value, and the higher the energy density is, but the smaller the interlayer spacing is, the greater the resistance encountered during the insertion and extraction of lithium ions, resulting in a decrease in the temperature coefficient of the carbon substrate. The lower the degree of graphitization of the carbon-based material, the lower the energy density. The inventors have found that when the range of the degree of graphitization G1 of the primary particle carbon-based material satisfies 93%≤G1≤97%, and the range of the degree of graphitization G2 of the secondary particle carbon-based material satisfies 90%≤G2≤93%, the negative electrode active material can have a high energy density and the temperature coefficient does not significantly attenuate due to the increase in its energy density.

[0012] Furthermore, the particle size D50, tap density T, graphitization degree G2, mass fraction M2 and average Raman value r of the carbon-based material satisfy the relationship (I):

[0013] T*D50 / 3+G2 / (2*r*M2)<11

[0014] (I);

[0015] The unit corresponding to the particle size D50 value is μm; the average Raman value r is the average value of the ratio of the peak intensity of the D peak to the peak intensity of the G peak of the Raman spectrum of the carbon-based material; the unit corresponding to the tap density T value is g / cm 3 .

[0016] Furthermore, the particle size D50, the tap density T, the degree of graphitization G2, the mass fraction M2 and the average Raman value r satisfy the relation (I), thereby effectively improving the temperature coefficient of the battery cell while ensuring high energy density.

[0017] Furthermore, the particle size D50, tap density T, graphitization degree G2, mass fraction M2 and average Raman value r of the carbon-based material satisfy the relationship (I):

[0018] 6<T*D50 / 3+G2 / (2*r*M2)<11

[0019] (I);

[0020] The unit corresponding to the particle size D50 value is μm; the average Raman value r is the average value of the ratio of the peak intensity of the D peak to the peak intensity of the G peak of the Raman spectrum of the carbon-based material; the unit corresponding to the tap density T value is g / cm 3 .

[0021] The particle size D50, the tap density T, the graphitization degree G2, the mass fraction M2 and the average Raman value r satisfy the relation (I). The temperature coefficient of the battery cell can be effectively improved on the basis of further ensuring high energy density.

[0022] Furthermore, the carbon-based material further includes a coating layer, the coating layer includes a hard carbon structure located at the outermost part, and a soft carbon structure located between the carbon-based material and the hard carbon structure; the range of the average Raman value r satisfies 0.12≤r≤0.2, and the range of the tap density T satisfies 0.85≤T≤1.1. The above parameters can be adjusted according to actual needs, for example: r can be 0.12, 0.14, 0.16, 0.18 or 0.2; T can be 0.85, 0.90, 0.95, 1.0, 1.05 or 1.1.

[0023] The second object of the present invention is to provide a negative electrode active material, which has the characteristics of high energy density and a temperature coefficient that does not significantly attenuate due to the increase of its energy density, and has good low-temperature discharge capability. The negative electrode active material includes the carbon-based material and the coating layer coated thereon. The particle size Dv50 of the carbon-based material satisfies the range of 7.0≤D50≤17.0, the average Raman value r satisfies the range of 0.12≤r≤0.2, and the tap density T satisfies the range of 0.85≤T≤1.1.

[0024] The soft carbon structure is coated on the particles of the primary particle carbon-based material and the secondary particle carbon-based material, and has good contact with the above-mentioned carbon-based materials. The hard carbon structure has good fast charging performance. The coordinated use of the soft carbon structure and the hard carbon structure can effectively reduce the interface transmission impedance and improve the temperature coefficient.

[0025] The present invention also discloses a method for preparing the negative electrode active material, comprising the following steps: preparing the carbon-based material by mixing the primary particle carbon-based material and the secondary particle carbon-based material, so that the mass fraction ratio of the primary particle carbon-based material: the secondary particle carbon-based material in the carbon-based material is 0-30%: 70%-100%.

[0026] The third object of the present invention is to provide a method for preparing a negative electrode active material, which has a simple process and low cost.

[0027] Furthermore, the method for preparing the coating layer includes the following steps: after mixing the primary particle carbon-based material and the secondary particle carbon-based material, adding asphalt, reacting t1 in an oxygen flow at a temperature Q1, and then carbonizing at a temperature Q2 in a protective atmosphere.

[0028] The negative electrode active material provided by the present invention, in some disclosed schemes, also includes a coating layer. The above is a method for preparing the coating layer, which is simple and low-cost. The prepared carbon-based material has low interface transmission impedance and high low-temperature discharge capability.

[0029] Furthermore, 150°C≤Q1≤400°C, 16h≤t1≤40h, 1000°C≤Q2≤1300°C, and the protective atmosphere includes at least one of a nitrogen atmosphere, a helium atmosphere, and an argon atmosphere. Among them, Q1 can be 150°C, 200°C, 250°C, 300°C, 350°C, or 400°C; t1 can be 16h, 20h, 24h, 28h, 32h, 34h, 38h, or 40h; Q2 can be 1000°C, 1100°C, 1200°C, or 1300°C.

[0030] The method for preparing the coating layer provided by the present invention first reacts t1 under T1 and oxygen flow to pre-oxidize the asphalt and the carbon-based material to generate the soft carbon structure and the primary hard carbon structure, and then transforms the primary hard carbon structure into a hard carbon structure under a protective atmosphere and T2, wherein the protective atmosphere is for deoxygenation.

[0031] Furthermore, T1 is 250° C., t1 is 32 h, T2 is 1150° C., and the protective atmosphere includes a nitrogen atmosphere. The above parameters selected in the present invention are preferred parameters.

[0032] The present invention also discloses a negative electrode active slurry prepared by using the negative electrode active material. In the negative electrode active slurry, the mass ratio of the negative electrode active material, the binder and the dispersant is (97-99): (0.5-1.5): (0.5-1.5). Preferably, the above mass ratio can be 98:1:1. The mass ratio is the mass ratio in the prior art. Those skilled in the art can select the mass ratio within the range or the disclosed preferred mass ratio according to actual needs. The binder is a binder in the prior art, such as styrene-butadiene rubber. Those skilled in the art can select a binder in the prior art according to actual needs. The dispersant is a dispersant in the prior art, such as sodium carboxymethyl cellulose. Those skilled in the art can select a dispersant in the prior art according to actual needs.

[0033] The present invention also discloses a method for preparing the negative electrode active slurry, which specifically comprises the steps of fully stirring and mixing the negative electrode active material, the binder and the dispersant in the mass ratio disclosed in the technical solution of the present invention to obtain the negative electrode active slurry, wherein the binder comprises styrene-butadiene rubber and the dispersant comprises sodium carboxymethyl cellulose. The method is simple in process, saves raw materials and has high cost performance.

[0034] The present invention also discloses a negative electrode plate, comprising a current collector and the negative electrode active slurry layer of the above technical solution coated on at least one surface thereof, wherein the current collector comprises copper foil or aluminum foil, and the surface density of the negative electrode active slurry is 4.5 mg / cm 2 ~14.5mg / cm 2 , compacted density is 1.70g / cm 3 ~1.85g / cm 3 Among them, the surface density can be 4.5mg / cm 2 , 5.5mg / cm 2 、6.5mg / cm 2 、7.5mg / cm 2 、8.5mg / cm 2 、9.5mg / cm 2 、10.5mg / cm 2 、11.5mg / cm 2 、12.5mg / cm 2 、13.5mg / cm 2 or 14.5 mg / cm 2 ; The compacted density can be 1.70g / cm 3 , 1.75g / cm 3 , 1.80g / cm 3 or 1.85g / cm 3 .

[0035] The present invention also discloses a method for preparing a negative electrode sheet, which specifically includes coating the negative electrode active slurry on a current collector, drying it at room temperature, transferring it to an oven and continuing to dry it at 30°C to 100°C, and then cold pressing and cutting it to obtain a negative electrode sheet. The method for preparing a negative electrode sheet disclosed in the present invention has a simple process and low cost.

[0036] Compared with the prior art, the present invention has at least the following beneficial effects:

[0037] The negative electrode active material prepared by the present invention has a high energy density, and its temperature coefficient does not significantly decay due to the increase of its energy density. This is because the aspect ratio of the primary particle carbon-based material and the secondary particle carbon-based material in the present invention is controlled within the range disclosed in the technical solution of the present invention. The inventors have found that when the aspect ratio of the secondary particle carbon-based material is in the range of 3 to 4, the secondary particle carbon-based material is in the form of flakes, has better extension and sliding properties during rolling, and has a higher compaction density; when the aspect ratio of the primary particle carbon-based material is in the range of 1 to 2, the primary particle carbon-based material is rounder in shape, has higher isotropy, and can achieve a higher operating voltage; the combination of two particles with different aspect ratios has a higher energy density, because the primary particle carbon-based material with a mass fraction of 0% to 30% can improve the temperature coefficient and avoid the existence of overvoltage, while the secondary particle carbon-based material with a mass fraction of 70% to 100% can provide high energy density. When the primary particle carbon-based material and the secondary particle carbon-based material disclosed in the present invention are within the mass fraction range disclosed in the present invention, the negative electrode active material can have a high energy density and the temperature coefficient does not significantly attenuate due to the increase in its energy density. DETAILED DESCRIPTION

[0038] The present invention will be described in further detail below in conjunction with specific implementation modes, but the implementation modes of the present invention are not limited thereto.

[0039] Example 1

[0040] Preparation of negative electrode active material: The negative electrode active material comprises a primary particle carbon-based material and a secondary particle carbon-based material, the aspect ratio a of the primary particle carbon-based material is 1, the mass fraction is 10%, the aspect ratio b of the secondary particle carbon-based material is 3, the mass fraction is 90%; the degree of graphitization of the primary particle carbon-based material is 93%, and the degree of graphitization of the secondary particle carbon-based material is 90%, after mixing the primary particle carbon-based material and the secondary particle carbon-based material, adding 5% by weight of asphalt of the total mass of the carbon-based material, reacting at 250°C for 32h under oxygen flow, after pre-oxidation and cross-linking reaction, and then carbonizing at 1150°C in a N2 environment to form the coating layer, the outermost layer of the coating layer is a hard carbon structure, the inner layer of the hard carbon structure is a soft carbon structure, and the inner layer of the soft carbon structure is a particle structure, the particle structure is the particle structure of the primary particle carbon-based material and the secondary particle carbon-based material, to obtain the negative electrode active material.

[0041] Preparation of negative electrode active slurry: The negative electrode active material, styrene-butadiene rubber and sodium carboxymethyl cellulose are dissolved in deionized water at a weight ratio of 98:1:1, and the different negative electrode slurries are obtained after being fully stirred and mixed. It should be noted that deionized water can be selected according to actual needs as long as it does not affect the homogenization effect and does not cause the subsequent drying process to take too much time due to excessive dilution of the negative electrode active slurry, affecting the efficiency.

[0042] The measured average Raman value r of the carbon-based material is 0.10, the proportion of active substances with R value ≤ 0.15 is 65%, the tap density T is 1.5, and the particle size is 17.0.

[0043] The above values ​​are obtained by the following method: R value measurement method: using laser microscopic confocal Raman spectrometer to test the surface defects of negative electrode active materials, using laser microscopic confocal Raman spectrometer to test the surface defects of negative electrode active materials, using samples at 1350cm -1 The peak intensity of D at I D With 1580cm -1 The peak intensity of G at I G The ratio ID / IG value represents the surface defect degree of the sample.

[0044] r value calculation method: The R value obtained by R value test and its corresponding k value distribution diagram are statistically calculated.

[0045] Particle size test method: tested by sieving method.

[0046] Tap density test method: Adopt the national standard GB / T 5162-2006 "Determination of tap density of metal powders" test method, use the GeoPyc1365 equipment of McMeretics, weigh 50±0.2g of powder sample, vibrate at a frequency of 250 times / min, and test its tap density.

[0047] Preparation of negative electrode sheet: The negative electrode active slurry is evenly applied on the copper foil, dried at room temperature and then transferred to an oven for further drying, and then cold pressed and cut to obtain the negative electrode sheet.

[0048] The surface density of the negative electrode active slurry is 10 mg / cm 2 , compacted density is 1.75g / cm 3 .

[0049] Preparation of positive electrode:

[0050] The positive electrode active material NCM523, the conductive agent acetylene black, and the binder PVDF are mixed in a mass ratio of 97:2:1, and the solvent NMP is added, and stirred under the action of a vacuum mixer until the system is uniform to obtain a positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, dried at room temperature, and then transferred to an oven for further drying, and then cold pressed and cut to obtain a positive electrode sheet.

[0051] Preparation of electrolyte:

[0052] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0053] Preparation of isolation membrane:

[0054] A polyethylene film is selected as the separating film.

[0055] Preparation of lithium-ion batteries:

[0056] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and then wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.

[0057] Tables 1 to 2 are data of Examples 1 to 20 and Comparative Examples 1 to 3, and the rest are the same as Example 1 and will not be repeated here.

[0058] Table 1

[0059] Table 2

[0060]

[0061]

[0062] The following performance tests were performed on the above embodiments and comparative examples, respectively. The parameters and test results of the embodiments and comparative examples are shown in Table 3.

[0063] 1. Temperature coefficient test: At 25℃, charge to 4.50V at 0.5C constant current and constant voltage, cut off at 0.02C, and then discharge to 3.0V at 0.2C constant current, and record the discharge capacity C1; place the battery cell in a 45℃ environment, charge to 4.50V at 0.5C constant current and constant voltage, cut off at 0.02C, and then discharge to 3.0V at 0.2C constant current, and record the discharge capacity C2, temperature coefficient = (C2-C1) / C2.

[0064] 2. Energy density test: At 25°C, fully charge the lithium-ion battery at a 1C rate and fully discharge it at a 1C rate, and record the actual discharge energy at this time; at 25°C, use an electronic balance to weigh the lithium-ion battery; the ratio of the actual discharge energy of the lithium-ion battery at 1C to the weight of the lithium-ion battery is the actual energy density of the lithium-ion battery; that is, energy density (Wh / kg) = discharge capacity (Wh) / mass of lithium-ion secondary battery (kg).

[0065] Table 3

[0066]

[0067]

[0068] It can be seen from the test results in Table 1 above that the test data of energy density and temperature coefficient of Examples 1 to 20 and Comparative Examples 1 to 3 show that when the various values ​​and relationship expressions of the carbon-based material are within the scope disclosed in the technical solution of the present invention, the negative electrode active material has a high energy density and the temperature coefficient does not significantly decay due to the increase in its energy density, but if the various values ​​and relationship expressions of the carbon-based material are not within the scope disclosed in the technical solution of the present invention, the negative electrode active material either has a low energy density or has only a low temperature coefficient at a high energy density.

[0069] By comparing Example 1 with Examples 5 to 7, it can be seen that the temperature coefficient data of Examples 5 to 7 are better than that of Example 1. The main reason is that the oxygen permeation time of Examples 5 to 7 is longer, and oxygen can promote the cross-linking reaction; the temperature coefficient of Examples 5 to 7 increases with the increase of the oxygen permeation time, indicating that the longer the oxygen permeation time, the greater the degree of cross-linking of the outer layer, the higher the degree of disorder, and the more conducive to the rapid transmission of lithium ions, reducing polarization and improving the temperature coefficient.

[0070] By comparing Example 5 with Examples 10 and 11, it can be seen that the energy density data of Examples 10 to 11 are better than those of Example 1. The reason is that the graphite particles with a large aspect ratio are more flaky, and are better at extending and sliding during rolling, and have a higher compaction density; while the particles with a smaller aspect ratio are more round, have higher isotropy and better dynamic properties.

[0071] From the comparison between Example 5 and Examples 12 and 13, it can be seen that the initial efficiency of the secondary particle capacity is relatively low, and reducing the proportion will increase the energy density, but the secondary particles have good isotropy, which can ensure the insertion and extraction of lithium ions and ensure the temperature coefficient.

[0072] By comparing Examples 1 to 16 with Comparative Example 1, it can be seen that the temperature coefficient data of Comparative Example 1 are worse than those of Examples 1 to 16. The direct reason is that the particle size D50, tap density T, degree of graphitization G2, mass fraction M2 and average Raman value r of the carbon-based material of Comparative Example 1 do not satisfy the relationship (I); it means that the active material has a high density and a large particle size, and the secondary particles have a high degree of graphitization, resulting in a small interlayer spacing and a large number of layers. The diffusion resistance of lithium ions between graphite layers is large, and the proportion of secondary particles is small, which significantly reduces the temperature coefficient.

[0073] By comparing Examples 1 to 16 and Comparative Example 2, it can be seen that the temperature coefficient data of Comparative Example 2 are worse than those of Examples 1 to 16, indicating that when the aspect ratio is increased, the single-particle flake structure will obviously increase its orientation degree, and the slip effect after rolling will increase the compaction density of the pole piece and the stacking density of the particles, thereby improving the energy density. However, when the temperature rises, the polarization phenomenon intensifies, including concentrated polarization and increased interface resistance, which has a greater limiting effect on the transmission and diffusion of lithium ions, resulting in a decrease in the temperature coefficient.

[0074] By comparing Examples 1 to 16 and Comparative Example 3, it can be seen that the energy density of Comparative Example 3 is lower than those of Examples 1 to 16, indicating that when the average Raman value r increases, the temperature coefficient increases but the compaction density decreases, thereby resulting in a decrease in energy density; the average Raman r reflects the disorder of the coating layer. The higher the disorder, the more hard carbon components and the fewer soft carbon components on the surface, which is more conducive to kinetic improvement, that is, it is more conducive to improving the temperature coefficient. However, the higher the average Raman value r, the higher the proportion of hard carbon, the lower the compaction level, and the lower the energy density. Therefore, the present invention needs to limit the value range to balance the r value.

[0075] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. A negative electrode active material, characterized in that: The negative electrode active material includes a carbon-based material, and the carbon-based material includes a primary particle carbon-based material and a secondary particle carbon-based material. The aspect ratio a of the primary particle carbon-based material is between 1 and 2, and the aspect ratio b of the secondary particle carbon-based material is between 3 and 4. The mass fraction M1 of the primary particle carbon-based material in the carbon-based material satisfies 0%≤M1≤30%, and the mass fraction M2 of the secondary particle carbon-based material in the carbon-based material satisfies 70%≤M2≤100%; the proportion k of the part with R≤0.15 in the carbon-based material satisfies k≥10%; and R refers to the ratio of the peak intensity of the D peak to the peak intensity of the G peak of the Raman spectrum of the carbon-based material.

2. The negative electrode active material according to claim 1, characterized in that The graphitization degree G1 of the primary particle carbon-based material satisfies the range of 93%≤G1≤97%, and the graphitization degree G2 of the secondary particle carbon-based material satisfies the range of 90%≤G2≤93%.

3. The negative electrode active material according to claim 2, characterized in that: The particle size D50, tap density T, graphitization degree G2, mass fraction M2 and average Raman value r of the carbon-based material satisfy the relationship (I): T*D50 / 3+G2 / (2*r*M2)<11 (I); The unit corresponding to the particle size D50 value is μm; The average Raman value r is the average value of the ratio of the peak intensity of the D peak to the peak intensity of the G peak of the Raman spectrum of the carbon-based material; The unit corresponding to the tap density T value is g / cm 3 .

4. The negative electrode active material according to claim 3, characterized in that The carbon-based material further includes a coating layer, wherein the coating layer includes a hard carbon structure located at the outermost portion and a soft carbon structure located between the carbon-based material and the hard carbon structure; The range of the particle size D50 satisfies 7.0≤D50≤17.0; the range of the average Raman value r satisfies 0.12≤r≤0.2, and the range of the tap density T satisfies 0.85≤T≤1.

1.

5. A method for preparing a negative electrode active material according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: preparing the carbon-based material by mixing the primary particle carbon-based material and the secondary particle carbon-based material, so that the mass fraction ratio of the primary particle carbon-based material: the secondary particle carbon-based material in the carbon-based material is 0-30%: 70%-100%.

6. The method for preparing the negative electrode active material according to claim 5, characterized in that: The preparation method of the coating layer includes the following steps: after mixing the primary particle carbon-based material and the secondary particle carbon-based material, adding asphalt, reacting at temperature Q1 for t1 under oxygen flow, and then carbonizing at temperature Q2 in a protective atmosphere; wherein, 150℃≤Q1≤400℃, 16h≤t1≤40h, 1000℃≤Q2≤1300℃.

7. The method for preparing the negative electrode active material according to claim 6, characterized in that: The protective atmosphere includes at least one of a nitrogen atmosphere, a helium atmosphere and an argon atmosphere.

8. A negative electrode active slurry, characterized in that: It comprises the negative electrode active material, a binder and a dispersant as described in any one of claims 1 to 4; the mass ratio of the negative electrode active material, the binder and the dispersant is (97 to 99):(0.5 to 1.5):(0.5 to 1.5).

9. A negative electrode plate, characterized in that: A current collector and the negative electrode active slurry according to claim 8 coated on at least one surface of the current collector, wherein the surface density of the negative electrode active slurry is 4.5 mg / cm 2 ~14.5mg / cm 2 , compacted density is 1.70g / cm 3 ~1.85g / cm 3 .

10. A method for preparing a negative electrode sheet according to claim 9, characterized in that: The negative electrode active slurry is coated on the current collector, dried at room temperature, and then transferred to an oven to continue drying at 30° C. to 100° C., and then cold pressed and cut to obtain negative electrode sheets.

Citation Information

Cited By

  • Hard carbon material, secondary battery and electronic device

    CN119725524A

  • Hard carbon material, secondary battery, and electronic device

    CN119725524B

  • Hard carbon secondary particle and preparation method thereof, negative electrode plate and sodium battery