Battery cell and electronic device

By using polymer matrix layer and conductive layer in the battery cell to form a composite fluid, and combining Z-shaped folding and laminated structures, the problems of low energy density of the battery cell and pole fracture are solved, and higher energy density and Structural stability.

CN118943373APending Publication Date: 2024-11-12XIAMEN AMPACE TECH LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411215031.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing battery cells, the current collector thickness of the negative electrode sheet is relatively large, resulting in low energy density and the electrode sheet is prone to fracture, especially during expansion.

Method used

The polymer matrix layer and two conductive layers are used to form a composite liquid collector. The negative electrode sheet adopts a Z-shaped continuous folding structure. The positive electrode sheet adopts a stacked structure. Combined with the composite liquid collector to replace the traditional metal current collector, improve mechanical strength and ductility, and reduce Risk of fracture.

Benefits of technology

On the premise of ensuring mechanical strength, thin the current collector thickness, improve the energy density and structural stability of the battery cell, and reduce the risk of pole fracture and capacity loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943373A_ABST
    Figure CN118943373A_ABST
Patent Text Reader

Abstract

The invention discloses a battery cell and an electronic device. The battery cell comprises a negative plate, a positive plate and an isolating membrane, the negative plate comprises a first current collector and a first active material layer. The first current collector comprises a polymer matrix layer and two conductive layers, and the two conductive layers are arranged on the surfaces of the two sides of the polymer matrix layer respectively in the thickness direction of the polymer matrix layer. The first active material layer is arranged on the surface, away from the polymer matrix layer, of the conductive layer. Wherein the negative plate is continuously folded in a Z shape along the thickness direction of the battery cell, the negative plate comprises a plurality of first straight sections and a plurality of first bent sections, the plurality of first straight sections are sequentially stacked along the thickness direction of the battery cell, and each first bent section is respectively connected between two adjacent first straight sections. And a positive plate is arranged between every two adjacent first straight sections. The isolating membrane is positioned between the negative plate and the positive plate. The battery cell is favorable for improving the energy density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage technology, and in particular to a battery cell and an electronic device. Background Art

[0002] In existing battery cells, the current collector of the negative electrode is usually made of copper foil. Since copper foil needs to maintain a certain mechanical strength, its thickness is relatively large, which is not conducive to improving the energy density of the battery cell. In addition, the positive and negative electrode sheets usually use traditional current collectors (i.e., aluminum foil and copper foil). At this time, the electrode sheet is more likely to break, especially when the electrode sheet expands to a large extent. Summary of the invention

[0003] In view of the above situation, the present application provides a battery cell that is beneficial to improving energy density.

[0004] An embodiment of the present application provides a battery cell, which includes a negative electrode sheet, a positive electrode sheet and a separator. The negative electrode sheet includes a first current collector and a first active material layer. The first current collector includes a polymer matrix layer and two conductive layers, and the two conductive layers are respectively arranged on the surfaces of both sides of the polymer matrix layer along the thickness direction of the polymer matrix layer. The first active material layer is arranged on the surface of the conductive layer away from the polymer matrix layer. Among them, along the thickness direction of the battery cell, the negative electrode sheet is continuously folded in a Z shape, and the negative electrode sheet includes a plurality of first straight sections and a plurality of first bent sections. The plurality of first straight sections are stacked in sequence along the thickness direction of the battery cell, and each first bent section is respectively connected between two adjacent first straight sections. A positive electrode sheet is arranged between each two adjacent first straight sections. The separator is located between the negative electrode sheet and the positive electrode sheet.

[0005] In the above-mentioned battery cell, the first current collector forms a composite current collector through the polymer matrix layer and the two conductive layers. Compared with the traditional metal current collector, it is beneficial to reduce the thickness of the first current collector while ensuring the mechanical strength, and thus it is beneficial to improve the energy density of the battery cell. The above-mentioned battery cell adopts a combination of a negative electrode sheet with a winding structure and a positive electrode sheet with a laminated structure. The negative electrode sheet adopts a composite current collector to replace the traditional metal current collector. Since the ductility of the composite current collector is better, the risk of the negative electrode sheet breaking can be improved. Compared with the battery cell in which both the positive and negative electrode sheets adopt a laminated structure, there will be a problem of unstable connection between the composite current collector used in the negative electrode sheet and the pole lug. Setting the negative electrode sheet into a continuous winding structure is beneficial to reduce the capacity loss of the battery cell after the pole lug connected to the negative electrode sheet breaks. Compared with battery cells in which both the positive and negative electrodes adopt a winding structure, there is a problem that the negative electrode sheet is easy to expand and generate stress on the adjacent positive electrode sheet, causing it to break. The positive electrode sheet is arranged into a stacked structure. Since the composite current collector has better ductility and the opening structure of the two first straight sections away from the first bent section can provide a release space for the stress generated by the expansion of the negative electrode sheet, it is beneficial to reduce the stress on the positive electrode sheet when the negative electrode sheet expands, thereby reducing the risk of the positive electrode sheet breaking.

[0006] In some embodiments of the present application, the elongation of the first current collector is 5% to 20%, so as to reduce the risk of the first current collector being broken and the risk of the battery cell being deformed.

[0007] In some embodiments of the present application, the material of the first active material layer includes a silicon-based material, and the weight percentage of the silicon-based material in the first active material layer is greater than or equal to 5%, so as to improve the specific capacity of the battery cell.

[0008] In some embodiments of the present application, the thickness of the polymer matrix layer is H1, 5 μm≤H1≤10 μm, which is beneficial to reducing the thickness of the first current collector while ensuring mechanical strength, thereby facilitating improving the energy density of the battery cell.

[0009] In some embodiments of the present application, 5 μm≤H 1≤8 μm, so as to further reduce the thickness of the first current collector, thereby further facilitating improving the energy density of the battery cell.

[0010] In some embodiments of the present application, the conductive layer includes a metal material, and the metal material includes copper.

[0011] In some embodiments of the present application, along the thickness direction of the polymer matrix layer, the thickness of the conductive layer is H2, 0.5μm≤H2≤3μm, which is beneficial to thinning the thickness of the first current collector while ensuring the current flow capacity, thereby facilitating improving the energy density of the battery cell.

[0012] In some embodiments of the present application, 0.5 μm≤H2≤1 μm, so as to further reduce the thickness of the first current collector, thereby facilitating improving the energy density of the battery cell 100 .

[0013] In some embodiments of the present application, the battery cell includes two first insulating members, which respectively cover the two ends of the negative electrode sheet along the length direction after the negative electrode sheet is unfolded, so as to reduce the risk of short circuit caused by the end of the negative electrode sheet contacting the adjacent positive electrode sheet when the negative electrode sheet expands.

[0014] In some embodiments of the present application, the spacing between the positive electrode sheet and the corresponding first bending section is W, 2mm≤W≤7mm, so as to reduce the risk of short circuit caused by contact between the positive electrode sheet and the corresponding first bending section when the negative electrode sheet expands, reduce capacity loss, and improve the energy density of the battery cell.

[0015] In some embodiments of the present application, the battery cell includes a second insulating member, which covers the end of the positive electrode sheet facing the corresponding first bending section; or is arranged on a side surface of the first bending section facing the corresponding positive electrode sheet, so as to reduce the risk of short circuit caused by contact between the positive electrode sheet and the corresponding first bending section when the negative electrode sheet expands.

[0016] In some embodiments of the present application, isolation films are respectively bonded to the surfaces on both sides of the negative electrode sheet along the thickness direction of the negative electrode sheet, and isolation films are respectively bonded to the surfaces on both sides of the positive electrode sheet along the thickness direction of the positive electrode sheet to improve the structural stability of the battery cell.

[0017] In some embodiments of the present application, the battery cell includes a first pole tab and a plurality of second pole tabs, the first pole tab is connected to the negative electrode sheet, and each positive electrode sheet is connected to at least one second pole tab.

[0018] An embodiment of the present application further provides an electronic device, which includes any one of the battery cells in the above embodiments.

[0019] In the above-mentioned battery cell and electronic device, the first current collector is formed into a composite current collector through the polymer matrix layer and the two conductive layers. Compared with the traditional metal current collector, it is beneficial to reduce the thickness of the first current collector while ensuring the mechanical strength, and thus it is beneficial to improve the energy density of the battery cell. The above-mentioned battery cell adopts a combination of a negative electrode sheet with a winding structure and a positive electrode sheet with a laminated structure. The negative electrode sheet adopts a composite current collector to replace the traditional metal current collector. Since the ductility of the composite current collector is better, the risk of the negative electrode sheet breaking can be improved. Compared with the battery cell in which both the positive and negative electrode sheets adopt a laminated structure, there will be a problem of unstable connection between the composite current collector used in the negative electrode sheet and the pole ear. Setting the negative electrode sheet into a continuous winding structure is beneficial to reduce the capacity loss of the battery cell after the pole ear connected to the negative electrode sheet breaks. Compared with battery cells in which both the positive and negative electrodes adopt a winding structure, there is a problem that the negative electrode sheet is easy to expand and generate stress on the adjacent positive electrode sheet, causing it to break. The positive electrode sheet is arranged into a stacked structure. Since the composite current collector has better ductility and the opening structure of the two first straight sections away from the first bent section can provide a release space for the stress generated by the expansion of the negative electrode sheet, it is beneficial to reduce the stress on the positive electrode sheet when the negative electrode sheet expands, thereby reducing the risk of the positive electrode sheet breaking. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic structural diagram of a battery cell observed along the length direction of the battery cell in one embodiment of the present application.

[0021] Figure 2 It is a schematic diagram of the structure of the negative electrode sheet of a battery cell in one embodiment of the present application.

[0022] Figure 3 It is a schematic structural diagram of a second insulating member of a battery cell in an embodiment of the present application.

[0023] Figure 4 It is a schematic structural diagram of a second insulating member of a battery cell in another embodiment of the present application.

[0024] Figure 5 It is a schematic diagram of the partial structure of a battery cell observed along the width direction of the battery cell in an embodiment of the present application.

[0025] Figure 6 It is a schematic diagram of the structure of an electronic device in one embodiment of the present application.

[0026] Main component symbols

[0027] Battery Cell 100

[0028] Electronic device 200

[0029] Negative electrode 10

[0030] The first current collector 11

[0031] Polymer matrix layer 111

[0032] Conductive layer 112

[0033] First active material layer 12

[0034] The first straight section 10A

[0035] The first bending section 10B

[0036] Positive electrode 20

[0037] Isolation film 30

[0038] The first insulating member 40

[0039] Part 41

[0040] Part 242

[0041] The second insulating member 50

[0042] Part 351

[0043] Part 452

[0044] First tab 61

[0045] Second pole ear 62

[0046] Thickness direction O

[0047] The following specific implementation methods will further illustrate the present application in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0048] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.

[0049] It should be noted that when an element is considered to be "connected" to another element, it may be directly connected to the other element or there may be a centrally disposed element at the same time. When an element is considered to be "disposed" on another element, it may be directly disposed on the other element or there may be a centrally disposed element at the same time.

[0050] When a value is considered to be "equal" to another value, it means that the two are equal within a set deviation, and the set deviation range is within 5%. In other words, when at least one of the two values ​​fluctuates within the set deviation range, even if their values ​​are not equal, they are still judged to be approximately equal. When a value is considered to be in a ratio of "1:1" to another value, it means that the two are equal within a set deviation, and the set deviation range is within 5%. In other words, when at least one of the two values ​​fluctuates within the set deviation range, even if their values ​​are not equal, they are still judged to be equal in ratio.

[0051] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more related listed items. The term "overlap" used herein refers to the overlap of the projections of two parts or the overlap of the projections of two parts.

[0052] An embodiment of the present application provides a battery cell, which includes a negative electrode sheet, a positive electrode sheet and a separator. The negative electrode sheet includes a first current collector and a first active material layer. The first current collector includes a polymer matrix layer and two conductive layers, and the two conductive layers are respectively arranged on the surfaces of both sides of the polymer matrix layer along the thickness direction of the polymer matrix layer. The first active material layer is arranged on the surface of the conductive layer away from the polymer matrix layer. Among them, along the thickness direction of the battery cell, the negative electrode sheet is continuously folded in a Z shape, and the negative electrode sheet includes a plurality of first straight sections and a plurality of first bent sections. The plurality of first straight sections are stacked in sequence along the thickness direction of the battery cell, and each first bent section is respectively connected between two adjacent first straight sections. A positive electrode sheet is arranged between each two adjacent first straight sections. The separator is located between the negative electrode sheet and the positive electrode sheet.

[0053] In the above-mentioned battery cell, the first current collector forms a composite current collector through the polymer matrix layer and the two conductive layers. Compared with the traditional metal current collector, it is beneficial to reduce the thickness of the first current collector while ensuring the mechanical strength, and thus it is beneficial to improve the energy density of the battery cell. The above-mentioned battery cell adopts a combination of a negative electrode sheet with a winding structure and a positive electrode sheet with a laminated structure. The negative electrode sheet adopts a composite current collector to replace the traditional metal current collector. Since the ductility of the composite current collector is better, the risk of the negative electrode sheet breaking can be improved. Compared with the battery cell in which both the positive and negative electrode sheets adopt a laminated structure, there will be a problem of unstable connection between the composite current collector used in the negative electrode sheet and the pole lug. Setting the negative electrode sheet into a continuous winding structure is beneficial to reduce the capacity loss of the battery cell after the pole lug connected to the negative electrode sheet breaks. Compared with battery cells in which both the positive and negative electrodes adopt a winding structure, there is a problem that the negative electrode sheet is easy to expand and generate stress on the adjacent positive electrode sheet, causing it to break. The positive electrode sheet is arranged into a stacked structure. Since the composite current collector has better ductility and the opening structure of the two first straight sections away from the first bent section can provide a release space for the stress generated by the expansion of the negative electrode sheet, it is beneficial to reduce the stress on the positive electrode sheet when the negative electrode sheet expands, thereby reducing the risk of the positive electrode sheet breaking.

[0054] The embodiments of the present application are further described below in conjunction with the accompanying drawings.

[0055] Please also read Figure 1 and Figure 2 One embodiment of the present application provides a battery cell 100, which is used in a secondary battery. A secondary battery is a battery that can be used continuously by activating active materials by charging after the battery is discharged. The battery cell 100 includes a negative electrode sheet 10, a positive electrode sheet 20, and a separator 30.

[0056] The negative electrode sheet 10 includes a first current collector 11 and a first active material layer 12. The first current collector 11 includes a polymer matrix layer 111 and two conductive layers 112. Along the thickness direction of the polymer matrix layer 111, the two conductive layers 112 are respectively arranged on the surfaces of both sides of the polymer matrix layer 111, and the first active material layer 12 is arranged on the surface of the conductive layer 112 away from the polymer matrix layer 111.

[0057] The polymer matrix layer 111 is made of a polymer insulating material, and has the advantages of low density, light weight, high temperature resistance, and not easily corroded by the electrolyte, and can reduce the thickness of the first current collector 11 and reduce the weight of the first current collector 11. Optionally, the polymer insulating material includes one or more of polyethylene terephthalate (PET), polypropylene (PP), polyethylene (PE), polyimide (PI), polyetherketone (PEK), polyphenylene sulfide (PPS), o-phenylphenol (OPP), and chlorinated polypropylene resin (CPP).

[0058] The conductive layer 112 includes a metal material. Compared with a conventional metal current collector, the thickness of the conductive layer 112 disposed on both sides of the polymer matrix layer 111 is reduced, which is beneficial to reduce the generation of metal burrs when the first current collector 11 is mechanically damaged by an external impact, thereby reducing the risk of short circuit. Optionally, the metal material includes one or more of aluminum, copper, nickel, silver, gold, and iron.

[0059] The first current collector 11 forms a composite current collector through the polymer matrix layer 111 and the two conductive layers 112 . Compared with the traditional metal current collector, it is beneficial to reduce the thickness of the first current collector 11 while ensuring the mechanical strength, thereby improving the energy density of the battery cell 100 .

[0060] Optionally, the current collector of the positive electrode sheet 20 is one of aluminum foil, carbon film or aluminum composite current collector.

[0061] Please continue reading Figure 1 and Figure 2 , along the thickness direction O of the battery cell 100, the negative electrode sheet 10 is continuously folded in a Z shape. The negative electrode sheet 10 includes a plurality of first straight sections 10A and a plurality of first bent sections 10B, and the plurality of first straight sections 10A are sequentially stacked along the thickness direction O of the battery cell 100, and each first bent section 10B is respectively connected between two adjacent first straight sections 10A. The first current collector 11 is formed into a composite current collector by the polymer matrix layer 111 and the two conductive layers 112, which is also conducive to improving the ductility and softness of the negative electrode sheet 10, so as to reduce the risk of the negative electrode sheet 10 being broken by continuous Z-shaped folding.

[0062] A positive electrode sheet 20 is provided between each two adjacent first straight sections 10A, and the first bent section 10B is used to limit the positive electrode sheet 20 between the two adjacent first straight sections 10A, so as to reduce the risk of lithium deposition caused by the displacement of the positive electrode sheet 20 relative to the first straight section 10A. Specifically, along the thickness direction O of the battery cell 100, the projection of the positive electrode sheet 20 is located within the projection of the first straight section 10A, so as to improve the structural stability of the battery cell 100 and reduce the risk of lithium deposition. The isolation film 30 is located between the negative electrode sheet 10 and the positive electrode sheet 20B.

[0063] During the preparation of the battery cell 100, the negative electrode sheet 10 and the isolation film 30 are first stacked so that a layer of isolation film 30 is provided on both side surfaces of the negative electrode sheet 10 in the thickness direction, and then the negative electrode sheet 10 and the isolation film 30 are continuously folded in a Z shape, and then the cut multiple positive electrode sheets 20B are inserted one by one from both sides between each adjacent two first straight sections 10A.

[0064] The existing battery cell structures are mainly divided into winding type and stacking type. Among them, when the tab of the battery cell with stacking structure breaks, it will cause the loss of capacity of the entire tab; and when the active material on the tab of the battery cell with winding structure expands, it will generate stress on the adjacent tab and cause it to break. The above-mentioned battery cell 100 adopts a combination of a negative electrode sheet 10 with a winding structure and a positive electrode sheet 20 with a stacking structure. The negative electrode sheet 10 adopts a composite current collector to replace the traditional metal current collector. Since the ductility of the composite current collector is better, the risk of the negative electrode sheet 10 breaking can be improved. Compared with the battery cell in which both the positive and negative electrodes adopt stacking structure, there will be a problem of unstable connection between the composite current collector used in the negative electrode sheet and the tab. Setting the negative electrode sheet 10 into a continuous winding structure is conducive to reducing the capacity loss of the battery cell 100 after the tab connected to the negative electrode sheet 10 breaks. Compared with the battery cells with both the positive and negative electrodes adopting the winding structure, there is the problem that the negative electrode sheet is easy to expand and generate stress on the adjacent positive electrode sheet, causing it to break. The positive electrode sheet 20 is arranged as a stacked structure. Since the ductility of the composite current collector is relatively good, and the opening structure of the two first straight sections 10A away from the first bent section 10B can provide a release space for the stress generated by the expansion of the negative electrode sheet 10, it is beneficial to reduce the stress on the positive electrode sheet 20 when the negative electrode sheet 10 expands, thereby reducing the risk of the positive electrode sheet 20 breaking.

[0065] In some embodiments, the elongation of the first current collector 11 is 5% to 20%. When the elongation of the first current collector 11 is too small (less than 5%), stress is easily generated on the first current collector 11 when the negative electrode sheet 10 expands, causing it to break. When the elongation of the first current collector 11 is too large (greater than 20%), the position of the first current collector 11 at the head and / or tail of the battery cell 100 is deformed, thereby deforming the battery cell 100. By limiting the elongation of the first current collector 11 to 5% to 20%, the risk of the first current collector 11 breaking is reduced, and the risk of deformation of the battery cell 100 is reduced.

[0066] Optionally, the elongation of the first current collector 11 is 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% and any other value in the range of 5% to 20%.

[0067] It should be noted that the elongation of the first current collector 11 is measured in the following manner: a first sample group is obtained in the longitudinal direction of the first current collector 11, and a second sample group is obtained in the transverse direction of the first current collector 11. The first sample group is cut into 5 samples with a size of 10 mm×100 mm, and the second sample group is cut into 5 samples with a size of 10 mm×100 mm. Tension is applied to 10 samples respectively at a stretching rate of 50 mm / min until the sample breaks. The initial length of the sample is recorded as the B value, and the length stretched before breaking is the C value. Calculate the strength and elongation of each sample, where the elongation is: (CB) / B*100%. The elongation of the first current collector 11 is the average of the elongations of the 10 samples.

[0068] In some embodiments, the material of the first active material layer 12 includes a silicon-based material, and the weight percentage of the silicon-based material in the first active material layer 12 is greater than or equal to 5%, so as to improve the specific capacity of the battery cell 100. In addition, in order to solve the problem of excessive expansion rate of silicon-based negative electrode materials, by setting the positive electrode sheet 20 into a stacked structure, the opening structure of the two first straight sections 10A away from the first bent section 10B can provide a release space for the stress generated by the expansion of the negative electrode sheet 10, which is conducive to reducing the stress on the positive electrode sheet 20 when the negative electrode sheet 10 expands, thereby reducing the risk of the positive electrode sheet 20 breaking.

[0069] Please refer again Figure 2In some embodiments, the thickness of the polymer matrix layer 111 is H1, 5μm≤H1≤10μm. When H1 is too small (less than 5μm), it is easy to cause weak mechanical strength; when H1 is too large (greater than 10μm), it is not conducive to thinning the thickness of the first current collector 11. By limiting 5μm≤H1≤10μm, it is conducive to thinning the thickness of the first current collector 11 while ensuring mechanical strength, thereby facilitating improving the energy density of the battery cell 100.

[0070] Optionally, H1 is one of 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm and any other value in the range of 5 μm≤H1≤10 μm.

[0071] Furthermore, 5 μm≤H 1≤8 μm, so as to further reduce the thickness of the first current collector 11 , thereby further facilitating the improvement of the energy density of the battery cell 100 .

[0072] Please continue reading Figure 2 In some embodiments, along the thickness direction of the polymer matrix layer 111, the thickness of the conductive layer 112 is H2, 0.5μm≤H2≤3μm, when H2 is too small (less than 0.5μm), it is easy to cause weak current flow capacity; when H2 is too large (greater than 3μm), it is not conducive to thinning the thickness of the first current collector 11. By limiting 0.5μm≤H2≤3μm, it is conducive to thinning the thickness of the first current collector 11 while ensuring the current flow capacity, and thus it is conducive to improving the energy density of the battery cell 100.

[0073] Optionally, H2 is 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2 μm,

[0074] 2.1μm, 2.2μm, 2.3μm, 2.4μm, 2.5μm, 2.6μm, 2.7μm, 2.8μm, 2.9μm,

[0075] 3μm and any other value in the range of 0.5μm≤H2≤3μm.

[0076] Furthermore, 0.5 μm≤H2≤1 μm, so as to further reduce the thickness of the first current collector 11 , thereby facilitating improving the energy density of the battery cell 100 .

[0077] Please refer again Figure 1In some embodiments, the battery cell 100 includes two first insulating members 40. Along the length direction of the unfolded negative electrode sheet 10, the two first insulating members 40 respectively cover the two ends of the negative electrode sheet 10 to reduce the risk of short circuit caused by the end of the negative electrode sheet 10 contacting the adjacent positive electrode sheet 20 when the negative electrode sheet 10 expands.

[0078] Optionally, the first insulating member 40 is formed by curing an insulating adhesive coated on the end of the negative electrode sheet 10. The insulating adhesive includes a ceramic layer.

[0079] In some embodiments, the first insulating member 40 includes a first portion 41 and two second portions 42 , wherein the first portion 41 covers the end surface of the negative electrode sheet 10 , and the two second portions 42 are respectively connected to both ends of the first portion 41 and overlap with the negative electrode sheet 10 in the thickness direction of the negative electrode sheet 10 .

[0080] Along the length direction of the unfolded negative electrode sheet 10, the length of the second portion 42 is L1, 2mm≤L1≤10mm. When L1 is too small (less than 2mm), it is easy to cause poor insulation stability at the end of the first insulating member 40; when L1 is too large (greater than 10mm), it is easy to cause the area of ​​the negative electrode sheet 10 wetted by the electrolyte to be reduced, resulting in capacity loss. By limiting 2mm≤L1≤10mm, the insulation stability of the end of the first insulating member 40 is improved, the capacity loss is reduced, and the energy density of the battery cell 100 is improved.

[0081] Optionally, L1 is 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm and any other value in the range of 2 mm ≤ L1 ≤ 10 mm.

[0082] Please continue reading Figure 1 In some embodiments, the spacing between the positive electrode sheet 20 and the corresponding first bending section 10B is W, 2mm≤W≤7mm. When W is too small (less than 2mm), the positive electrode sheet 20 is likely to contact with the corresponding first bending section 10B when the negative electrode sheet 10 expands, resulting in a short circuit; when W is too large (less than 2mm), it will cause capacity loss. By limiting 2mm≤W≤7mm, the risk of short circuit caused by contact between the positive electrode sheet 20 and the corresponding first bending section 10B when the negative electrode sheet 10 expands is reduced, and the capacity loss is reduced, thereby improving the energy density of the battery cell 100.

[0083] Optionally, W is one of 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm and any other value in the range of 2 mm ≤ L 1 ≤ 7 mm.

[0084] See also Figure 3In some embodiments, the battery cell 100 includes a second insulating member 50, which covers the end of the positive electrode sheet 20 facing the corresponding first bending section 10B to reduce the risk of short circuit caused by contact between the positive electrode sheet 20 and the corresponding first bending section 10B when the negative electrode sheet 10 expands.

[0085] In some embodiments, the second insulating member 50 covers the end of the positive electrode sheet 20 toward the corresponding first bending section 10B, and the second insulating member 50 includes a third part 51 and two fourth parts 52, the third part 51 covers the end surface of the positive electrode sheet 20, and the two fourth parts 52 are respectively connected to the two ends of the third part 51 and overlap with the positive electrode sheet 20 in the thickness direction of the positive electrode sheet 20.

[0086] Along the length direction of the positive electrode sheet 20, the length of the fourth portion 52 is L2, 2mm≤L2≤5mm. When L2 is too small (less than 2mm), it is easy to cause poor insulation stability at the end of the positive electrode sheet 20; when L2 is too large (greater than 5mm), it is easy to cause the area of ​​the positive electrode sheet 20 that is infiltrated by the electrolyte to be reduced, which will cause capacity loss. By limiting 2mm≤L2≤5mm, the insulation stability of the end of the positive electrode sheet 20 is improved, the capacity loss is reduced, and the energy density of the battery cell 100 is improved.

[0087] See also Figure 4 In some embodiments, the second insulating member 50 is disposed on a side surface of the first bending section 10B facing the corresponding positive electrode sheet 20 to reduce the risk of short circuit caused by contact between the positive electrode sheet 20 and the corresponding first bending section 10B when the negative electrode sheet 10 expands.

[0088] Please continue reading Figure 1 In some embodiments, the length of the separator 30 beyond the end of the negative electrode sheet 10 is 3 mm to 8 mm, so as to reduce the risk of the end of the negative electrode sheet 10 contacting the adjacent positive electrode sheet 20 and causing a short circuit when the negative electrode sheet 10 expands.

[0089] Optionally, the length of the separator 30 extending beyond the end of the negative electrode sheet 10 is 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, or any other value within the range of 3 mm to 8 mm.

[0090] In some embodiments, the isolation film 30 is sticky, and along the thickness direction of the negative electrode sheet 10, the surfaces on both sides of the negative electrode sheet 10 are respectively bonded with the isolation film 30, and along the thickness direction of the positive electrode sheet 20, the surfaces on both sides of the positive electrode sheet 20 are respectively bonded with the isolation film 30, so as to improve the structural stability of the battery cell 100.

[0091] Optionally, the isolation film 30 is made sticky by providing an adhesive on the surface of the isolation film 30. The adhesive is selected from one or a combination of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene. By selecting different material types and / or mass ratios to adjust the bonding strength of the adhesive, the peeling strength between the isolation film 30 and the negative electrode sheet 10 and the peeling strength between the isolation film 30 and the positive electrode sheet 20 are adjusted.

[0092] See also Figure 5 In some embodiments, the battery cell 100 includes a first pole tab 61 and a plurality of second pole tabs 62. The first pole tab 61 is connected to the negative electrode sheet 10, and each positive electrode sheet 20 is connected to at least one second pole tab 62. The first pole tab 61 and the plurality of second pole tabs 62 are electrically connected to an external circuit through pole tab leads.

[0093] In some embodiments, there are multiple first pole ears 61. When some of the first pole ears 61 are broken from the negative electrode sheet 10, since the negative electrode sheet 10 is arranged in a continuous winding structure, the negative electrode sheet 10 can still be electrically connected to the external circuit through other first pole ears 61, thereby reducing the capacity loss of the battery cell 100.

[0094] During the preparation of the battery cell 100 , the copper foil is firstly roll-welded to the conductive layer 112 on both sides of the first current collector 11 , and then the copper foil is die-cut to obtain a plurality of first pole tabs 61 , and then the first pole tabs 61 are welded to the pole tab leads.

[0095] See also Figure 6 One embodiment of the present application further provides an electronic device 200, which includes the battery cell 100 in any of the above embodiments. Optionally, the electronic device 200 may be a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy, an electric tool, etc.

[0096] In the above-mentioned battery cell 100 and electronic device 200, the first current collector 11 is formed into a composite current collector by means of the polymer matrix layer 111 and the two conductive layers 112. Compared with the traditional metal current collector, it is advantageous to reduce the thickness of the first current collector 11 while ensuring the mechanical strength, thereby facilitating the improvement of the energy density of the battery cell 100. The above-mentioned battery cell 100 adopts a combination of a negative electrode sheet 10 with a winding structure and a positive electrode sheet 20 with a laminated structure. The negative electrode sheet 10 adopts a composite current collector to replace the traditional metal current collector. Since the composite current collector has a relatively good ductility, the risk of the negative electrode sheet 10 breaking can be reduced. Compared with the battery cell in which both the positive electrode sheet and the negative electrode sheet adopt a laminated structure, there is a problem of unstable connection between the composite current collector used in the negative electrode sheet and the tab. The negative electrode sheet 10 is set to a continuous winding structure, which is advantageous to reduce the capacity loss of the battery cell 100 after the tab connected to the negative electrode sheet 10 breaks. Compared with the battery cells with both the positive and negative electrodes adopting the winding structure, there is the problem that the negative electrode sheet is easy to expand and generate stress on the adjacent positive electrode sheet, causing it to break. The positive electrode sheet 20 is arranged as a stacked structure. Since the ductility of the composite current collector is relatively good, and the opening structure of the two first straight sections 10A away from the first bent section 10B can provide a release space for the stress generated by the expansion of the negative electrode sheet 10, it is beneficial to reduce the stress on the positive electrode sheet 20 when the negative electrode sheet 10 expands, thereby reducing the risk of the positive electrode sheet 20 breaking.

[0097] The specific implementation of the battery cell 100 in the embodiment and the comparative example is described below.

[0098] 1. Battery full charge test:

[0099] The battery cell was charged at 25°C with a constant current of 0.2C to 4.25V, and then charged at a constant voltage of 4.25V to 0.05C cutoff. After standing for 15 minutes, the battery cell was disassembled to observe the fracture of the current collector and the deformation of the electrode.

[0100] 2. Battery cycle test:

[0101] The battery cell was charged to 4.25V at 1.0C constant current at 25℃, charged to 0.05C cut-off at 4.25V constant voltage, left to stand for 10min, discharged to 2.0V at 4.0C constant current, left to stand for 15min. The above is one cycle. The battery cell was cycled 500 times in the above manner and the capacity retention rate was calculated.

[0102] 3. Battery impedance test:

[0103] Use an internal resistance tester to apply a 1kHz AC signal to the battery cell, and obtain the internal resistance of the battery cell by testing its AC voltage drop. Calculate the internal resistance using the following formula: Internal resistance R = ΔU / I, where ΔU is the voltage change across the battery cell when an AC signal is applied, and I is the AC current passing through the battery at the same time. Measure the impedance of the battery cell at the first full charge cycle and the impedance of the battery cell at the full charge after 500 cycles, and calculate the impedance change rate of the battery cell.

[0104] Embodiment 1:

[0105] A battery cell with a rated capacity of 5000mAh, the assembly process is as follows:

[0106] (1) Preparation of negative electrode sheet: Mix the negative electrode active material graphite, silicon-based material, adhesive and conductive carbon in a weight ratio of 74:20:5:1, add deionized water as a solvent, prepare a slurry with a weight percentage of 50wt%, and stir evenly. Pre-apply foam glue to part of the surface of the conductive layer (the conductive layer is made of copper foil) of the composite current collector of the negative electrode sheet, and then evenly coat the slurry on one surface of the copper foil. Heat to make the foam glue fall off so that part of the surface of the copper foil is exposed, and then dry at 110°C to obtain a negative electrode sheet with a negative electrode active material layer coated on one side. The coating weight of the negative electrode active material layer is 8kg / cm 2 , compacted density is 1.6g / cm 3 When preparing a double-sided coated negative electrode sheet, the above steps are repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet coated with a negative electrode active material layer on both sides. The copper foil is then roll-welded with the conductive layer of the composite current collector, and the copper foil is die-cut to obtain a plurality of first tabs.

[0107] (2) Preparation of positive electrode sheet: Mix the positive electrode active materials lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and polyvinylidene fluoride (PVDF) in a weight ratio of 97.5:1.0:1.5, add N-methylpyrrolidone (NMP) as a solvent, prepare a slurry with a solid content of 75wt%, and stir evenly. The slurry is evenly coated on one surface of the aluminum foil, and then dried at 90°C to obtain a positive electrode sheet coated with a positive electrode active material layer on one side. The coating weight of the positive electrode active material layer is 13kg / cm 2 , compacted density is 3.5g / cm 3 When preparing a double-sided coated positive electrode sheet, repeat the above coating steps on the other surface of the aluminum foil. Then, die-cut the second tab in the blank area at the edge of the aluminum foil.

[0108] (3) Preparation of electrolyte: In a dry argon atmosphere, ethylene carbonate (EC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) are first mixed in a mass ratio of EC:EMC:DEC:EMC=20:30:40:10 to form a basic organic solvent, and then lithium salt lithium hexafluorophosphate (LiPF6) is added to the basic organic solvent to dissolve and mix evenly to obtain an electrolyte.

[0109] (4) Preparation of isolation membrane: A 7 μm thick polyethylene porous polymer film was used as the isolation membrane.

[0110] (5) Preparation of electrode assembly: The negative electrode sheet and the separator are stacked so that a layer of separator is provided on each side surface of the negative electrode sheet in the thickness direction, and then the negative electrode sheet and the separator are folded continuously in a Z shape, and then the cut positive electrode sheets are inserted one by one from both sides between each two adjacent first straight sections of the negative electrode sheet.

[0111] (6) Electrode assembly assembly: Place the aluminum-plastic film with holes punched and formed in an assembly fixture, with the holes facing upward, place the electrode assembly in the holes, and apply external force to press it. Then, cover the electrode assembly with another aluminum-plastic film with holes punched and formed, with the holes facing downward, and heat-seal the four sides of the two aluminum-plastic films by hot pressing to obtain an assembled electrode assembly.

[0112] (7) Liquid injection packaging: The assembled electrode assembly is injected with electrolyte, with an injection volume of 9g. After vacuum packaging, static standing, hot pressing, shaping and other processes, the battery cell is obtained.

[0113] Comparative Example 1: The positive electrode sheet adopts a winding structure, and the negative electrode sheet adopts a winding structure. It should be noted that, except for the different structure of the tabs, other parameters of Comparative Example 1 are the same as those of Example 1.

[0114] Comparative Example 2: The positive electrode sheet adopts a laminated structure, and the negative electrode sheet adopts a laminated structure. It should be noted that, except for the different structure of the tabs, other parameters of Comparative Example 2 are the same as those of Example 1.

[0115] Table 1

[0116]

[0117] It can be seen from Comparative Examples 1-2 and Example 1 that setting the negative electrode sheet 10 into a continuous winding structure and setting the positive electrode sheet 20 into a stacked structure is beneficial to reducing the risk of electrode sheet breakage, reducing capacity loss and reducing the impedance increase rate.

[0118] The above description is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions within the technical scope disclosed in the present application should be included in the disclosure scope of the present application.

Claims

1. A battery cell, characterized in that: The battery cell comprises: A negative electrode sheet, comprising a first current collector and a first active material layer, wherein the first current collector comprises a polymer matrix layer and two conductive layers, wherein along the thickness direction of the polymer matrix layer, the two conductive layers are respectively arranged on the surfaces of both sides of the polymer matrix layer, and the first active material layer is arranged on the surface of the conductive layer away from the polymer matrix layer; wherein along the thickness direction of the battery cell, the negative electrode sheet is continuously folded in a Z shape, and the negative electrode sheet comprises a plurality of first straight sections and a plurality of first bent sections, wherein the plurality of first straight sections are sequentially stacked along the thickness direction of the battery cell, and each of the first bent sections is respectively connected between two adjacent first straight sections; A positive electrode sheet, one of which is provided between every two adjacent first straight sections; and The separator is located between the negative electrode sheet and the positive electrode sheet.

2. The battery cell according to claim 1, characterized in that: The elongation of the first current collector is 5% to 20%.

3. The battery cell according to claim 1, characterized in that: The material of the first active material layer includes a silicon-based material, and the weight percentage of the silicon-based material in the first active material layer is greater than or equal to 5%.

4. The battery cell according to claim 1, characterized in that: The thickness of the polymer matrix layer is H1, 5 μm≤H1≤10 μm.

5. The battery cell according to claim 4, characterized in that: 5μm≤H 1≤8μm.

6. The battery cell according to claim 1, characterized in that: The conductive layer includes a metal material, and the metal material includes copper.

7. The battery cell according to claim 1, characterized in that: Along the thickness direction of the polymer matrix layer, the thickness of the conductive layer is H2, 0.5 μm≤H2≤3 μm.

8. The battery cell according to claim 7, characterized in that: 0.5μm≤H2≤1μm.

9. The battery cell according to claim 1, characterized in that: The battery core includes two first insulating members, and along the length direction of the unfolded negative electrode sheet, the two first insulating members respectively cover two ends of the negative electrode sheet.

10. The battery cell according to claim 1, characterized in that: The distance between the positive electrode sheet and the corresponding first bending section is W, 2mm≤W≤7mm.

11. The battery cell according to claim 10, characterized in that: The battery core includes a second insulating member, which covers the end of the positive electrode sheet facing the corresponding first bending section; or is arranged on a side surface of the first bending section facing the corresponding positive electrode sheet.

12. The battery cell according to claim 1, characterized in that: The isolation film is sticky. Along the thickness direction of the negative electrode sheet, the surfaces on both sides of the negative electrode sheet are respectively bonded to the isolation film. Along the thickness direction of the positive electrode sheet, the surfaces on both sides of the positive electrode sheet are respectively bonded to the isolation film.

13. The battery cell according to claim 1, characterized in that: The battery cell includes a first pole tab and a plurality of second pole tabs, wherein the first pole tab is connected to the negative electrode sheet, and each of the positive electrode sheets is connected to at least one of the second pole tabs.

14. An electronic device, characterized in that: The electronic device comprises the battery cell as claimed in any one of claims 1 to 13.

Citation Information

Cited By

  • Rechargeable battery and electronic device

    WO2026113667A1

  • Battery cell and electric device

    WO2026143395A1