Porous current collector and preparation process thereof, negative electrode and magnesium metal battery
By using alkali lignin and magnesium-containing activator in magnesium metal batteries to prepare magnesium-doped porous carbon materials and relaxed ferroelectric nanolayers, the problems of uneven metal deposition and irregular dendrites in magnesium metal batteries are solved, and the problem of uneven metal deposition and irregular dendrites in magnesium metal batteries is achieved. The uniform deposition and electrochemical performance of magnesium metal are improved.
Patent Information
- Application Number
- CN202411429682.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-10-14
AI Technical Summary
There are problems of uneven metal deposition and irregular dendrites in magnesium metal batteries.
Porous current collectors are prepared by alkali lignin and magnesium-containing activator, and porous carbon materials doped with magnesium element are obtained through carbonization. Combined with a relaxed ferroelectric nanolayer, it promotes uniform deposition of magnesium metal in the porous structure and plane-oriented deposition.
Doping magnesium elements increases the dielectric properties of the skeleton magnesium magnesium and relaxed ferroelectric nanolayers, achieving uniform deposition and electrochemical performance of magnesium metals, avoiding irregular growth of dendrites, and improving the cycling stability of the battery.
Smart Images

Figure CN118943382A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of magnesium metal batteries, and in particular to a porous current collector and a preparation process thereof, a negative electrode and a magnesium metal battery. Background Art
[0002] The theoretical volume capacity of magnesium metal anode can reach 3833mAh / cm 3 , the potential relative to the standard hydrogen electrode is -2.37V, and it has a high abundance on Earth (1.94%), Mg 2+ The carriers can transport two charges, so they have better transmission efficiency than monovalent alkali metal batteries. However, the metal negative electrode side also faces the problems of uneven deposition of magnesium metal and irregular growth of dendrites. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a porous current collector and its preparation process, a negative electrode and a magnesium metal battery, which can solve the problems of uneven metal deposition and irregular dendrite growth in magnesium metal batteries.
[0004] In order to solve the above technical problems, a technical solution adopted by the present invention is: A porous current collector, comprising a porous current collector made from alkali lignin and a magnesium-containing activator as raw materials; The alkali lignin and the magnesium-containing activator are reacted and then carbonized to obtain a porous carbon material current collector doped with magnesium.
[0005] Furthermore, the mass ratio of the alkali lignin to the magnesium-containing activator is 1:1-6.
[0006] Furthermore, the magnesium-containing activator includes MgCl 2 MgC 2 O 4 Mg(HCO 3 ) 2 MgCO 3 Mg(CH 3 COO 2 Mg(OH) 2 One or more of .
[0007] In order to solve the above technical problems, another technical solution adopted by the present invention is: A preparation process of the above-mentioned porous current collector comprises the following steps: Add alkali lignin and magnesium-containing activator into deionized water in a mass ratio of 1:1-6, stir at 50-70°C for 30-120 minutes, and evaporate the solvent at 100-120°C; The solid precursor is heated to 500-900° C. for carbonization treatment for 1-4 hours, cooled to room temperature and then pickled for 30-90 minutes, washed with deionized water and dried to obtain a porous carbon material current collector.
[0008] In order to solve the above technical problems, another technical solution adopted by the present invention is: A negative electrode comprises the above-mentioned porous current collector.
[0009] Furthermore, the porous current collector is a pre-magnesiumized porous current collector; In addition, a relaxor ferroelectric nanolayer is plated on the surface of the pre-magnesiumized porous current collector.
[0010] Furthermore, the relaxor ferroelectric nanolayer is a relaxor ferroelectric nanolayer having oxygen vacancies.
[0011] Further, the pre-magnesiation comprises: The porous carbon collecting material fluid, glass fiber separator and magnesium metal foil are assembled into a button battery, 0.4MMg (TFSI) 2 Magnesium salt is dissolved in ACN as electrolyte; Use 0.2-0.5 mA / cm 2 The battery is discharged for 4-10 hours to deposit magnesium metal on the porous carbon material current collector.
[0012] Furthermore, the relaxor ferroelectric nanolayer material is PbMg 1 / 3 Nb 2 / 3 O 3 、PbZn 1 / 3 Nb 2 / 3 O 3 、(1-x)PbMg 1 / 3 Nb 2 / 3 O 3 -xPbTiO 3 (0.1≤x≤0.3) and (1-x)PbZn 1 / 3 Nb 2 / 3 O 3 -xPbTiO 3 One of (0.1≤x≤0.3), with a thickness of 10-100nm.
[0013] In order to solve the above technical problems, a technical solution adopted by the present invention is: A magnesium metal battery comprises the above-mentioned negative electrode.
[0014] The beneficial effect of the present invention is that after carbonization treatment of alkali lignin and magnesium-containing activator, a magnesium-doped carbon-based porous current collector is obtained. The carbon material itself has no affinity for magnesium. By doping with magnesium, the affinity of the skeleton can be increased, which helps the magnesium metal to be uniformly deposited in the pore structure, rather than gathered on the surface of the 3D current collector. Therefore, by applying it to magnesium metal batteries, magnesium metal can be uniformly deposited in the pore structure of the porous current collector, and the pore structure provides sufficient buffer space for the volume change of magnesium metal during the charge and discharge process; in addition, the relaxor ferroelectric nanolayer has excellent polarization ability, which can play the role of uniform interface electric field and ion flow, promote the deposition of magnesium metal in the plane direction, and the oxygen vacancies in the relaxor ferroelectric material can also capture active lattice oxygen and protect the metal negative electrode. The design of the present invention can effectively solve the problems of uneven metal deposition and irregular growth of dendrites in magnesium metal batteries through synergistic effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The present invention is a flowchart of the steps of a process for preparing a porous current collector according to an embodiment of the present invention.
[0016] Figure 2 The present invention is a flowchart of a process for preparing a negative electrode according to an embodiment of the present invention. DETAILED DESCRIPTION
[0017] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in combination with the implementation modes and the accompanying drawings.
[0018] The porous current collector and its preparation process, negative electrode and magnesium metal battery described above in the present application can be applied to the preparation of magnesium metal batteries. The porous current collector can be used as a component of the negative electrode in the magnesium metal battery. The following is an explanation through specific implementation methods: In an optional embodiment, a porous current collector is a porous current collector made from alkali lignin and a magnesium-containing activator as raw materials; The alkali lignin and the magnesium-containing activator are carbonized to obtain a porous carbon material current collector doped with magnesium.
[0019] In another optional embodiment, the mass ratio of the alkali lignin to the magnesium-containing activator is 1:1-6.
[0020] In another optional embodiment, the magnesium-containing activator comprises MgCl 2 MgC 2 O 4 Mg(HCO 3 ) 2 MgCO 3 Mg(CH 3 COO 2 Mg(OH)2 One or more of .
[0021] In another optional embodiment, Figure 1 As shown, a process for preparing a porous current collector described in any of the above embodiments comprises the steps of: Add alkali lignin and magnesium-containing activator into deionized water in a mass ratio of 1:1-6, stir at 50-70°C for 30-120 minutes, and evaporate the solvent at 100-120°C; The solid precursor is heated to 500-900°C for carbonization treatment for 1-4 hours, cooled to room temperature and then acid-washed for 30-90 minutes, washed with deionized water and dried to obtain a porous carbon material current collector; Among them, the magnesium-containing activator is MgCl 2 MgC 2 O 4 Mg(HCO 3 ) 2 MgCO 3 Mg(CH 3 COO 2 Mg(OH) 2 One or more of the following, the heating rate is 5-10℃ / min, the experimental acid is 5%-30% HCl, H 2 SO 4 or CH 3 COOH.
[0022] In this embodiment, a porous carbon material is first prepared using alkali lignin as a carbon source. The porous carbon material can be used as a 3D current collector and a host material for Mg deposition. Commonly used alkali lignin activators are NaOH, ZnCl 2 , so in this embodiment, MgCl 2 MgC 2 O 4 Mg(HCO 3 ) 2 MgCO 3 、Mg(CH3COO) 2 Mg(OH) 2 These magnesium-containing active agents will retain the Mg element in the porous carbon material after carbonization to form a Mg-doped porous material. The carbon material itself has no affinity for Mg, but doping with Mg can increase the magnesium affinity of the skeleton, which helps Mg to be evenly deposited in the pore structure instead of gathering on the surface of the 3D current collector, thereby better ensuring the uniform deposition of Mg.
[0023] In another optional embodiment, a negative electrode includes a porous current collector as described in any of the above embodiments.
[0024] In another optional embodiment, the porous current collector is a pre-magnesiumized porous current collector; In addition, a relaxor ferroelectric nanolayer is plated on the surface of the pre-magnesiumized porous current collector.
[0025] Among them, Figure 2 As shown, the pre-magnesiation includes: The porous carbon material current collector, glass fiber separator and Mg metal foil are assembled into a button cell, 0.4 MMg (TFSI) 2 Magnesium salt is dissolved in ACN as electrolyte; Use 0.2-0.5 mA / cm 2 The Mg metal was deposited on the porous current collector after discharging for 4-10 hours.
[0026] Specifically, in a glove box (water and oxygen values <0.1 ppm), the porous current collector, glass fiber separator, and Mg metal foil described in any of the above embodiments are assembled into a button battery, wherein the electrolyte is 0.4 MMg (TFSI) 2 Magnesium salt is dissolved in ACN (acetonitrile). Use 0.2-0.5 mA / cm 2 Discharge for 4-10h to deposit Mg metal on the porous current collector, then disassemble the battery in a glove box, and wash and dry the pre-magnesiumized current collector in ACN; The pre-magnesiumized current collector was transferred to a magnetron sputtering chamber to deposit the relaxor ferroelectric nanolayer. The chamber was evacuated to 2×10 -5 Pa-6×10 -5 Pa, Ar and O were introduced at 10-100 sccm 2 The mixed gas (volume ratio 4:1), the working gas pressure is 1Pa-5Pa, the power is 50-150W, and the RF mode is used to sputter the relaxor ferroelectric nanolayer on the pre-magnesiumized current collector with a thickness of 10-100nm to obtain the negative electrode.
[0027] In this embodiment, the porous current collector is firstly doped with Mg, which not only improves the magnesium affinity of the porous current collector, but also can construct a sufficient number of pore skeleton structures to help Mg to be uniformly deposited in the pores, and the pore structure can also provide sufficient buffer space to adapt to the volume change of Mg metal during the charging and discharging process; then pre-magnesiation is performed, and Mg metal is deposited by electrochemical means, so that Mg metal is uniformly deposited in the pore structure of the Mg-doped porous carbon material; then, a relaxor ferroelectric nanolayer is deposited on its surface by magnetron sputtering, which plays a role in uniform interface electric field and ion flow, regulating magnesium metal electroplating, and improving the electrochemical performance of magnesium metal batteries.
[0028] In another optional embodiment, the relaxor ferroelectric nanolayer material is PbMg 1 / 3Nb 2 / 3 O 3 、PbZn 1 / 3 Nb 2 / 3 O 3 、(1-x)PbMg 1 / 3 Nb 2 / 3 O 3 -xPbTiO 3 (0.1≤x≤0.3) and (1-x)PbZn 1 / 3 Nb 2 / 3 O 3 -xPbTiO 3 One of (0.1≤x≤0.3), with a thickness of 10-100nm.
[0029] The role of the ferroelectric material layer at the negative electrode is to use the polarization characteristics to achieve the uniformity of the interface electric field and ion field. The dielectric constant of the material determines the polarization ability. In this embodiment, a relaxor ferroelectric material is used because the relaxor ferroelectric material has a higher dielectric constant and a stronger polarization ability than the ferroelectric material, and has a better effect of uniformizing the electric field and ion flow at the interface and inducing uniform deposition; and the use of magnetron sputtering to deposit the relaxor ferroelectric nanolayer will not increase the Mg 2+ The impedance of transmission at the interface further promotes its uniform diffusion at the interface.
[0030] In another optional embodiment, the relaxor ferroelectric nanolayer is a relaxor ferroelectric nanolayer having oxygen vacancies.
[0031] In order to construct oxygen vacancies, the relaxor ferroelectric material target is placed in a reducing atmosphere for annealing, thereby forming oxygen vacancies in the material. The reducing atmosphere is H 2 Atmosphere, pressure is 10 5 Pa, annealing temperature is 400-800℃, annealing time is 6-18h. The annealed target is installed in a magnetron sputtering instrument, and then the relaxor ferroelectric material with oxygen vacancies is deposited on the pre-magnesiumized current collector to obtain the negative electrode.
[0032] In this embodiment, by depositing a relaxor ferroelectric nanolayer with oxygen vacancies on the pre-magnesiumized current collector, the lattice oxygen that migrates to the negative electrode can be effectively captured, thereby avoiding harmful side reactions between magnesium metal and lattice oxygen.
[0033] In another optional embodiment, a magnesium metal battery comprises a negative electrode as described in any of the above embodiments.
[0034] Specifically, the magnesium metal battery consists of a positive electrode, a glass fiber separator, a negative electrode, and an electrolyte. The magnesium metal battery is assembled in a glove box (water and oxygen values <0.1ppm). The positive electrode is made by slurrying active materials, conductive carbon black, and PVDF in a mass ratio of 7:2:1 and coating them on aluminum foil. 2 O 5 Granules, Mg(CH3COO) 2 The MgxV was dissolved in deionized water at a molar ratio of 1:2-3, and stirred for 30-60 min after adding 1-10% hydrogen peroxide. The reaction was then carried out at 160-200 °C for 6-36 h. The reaction product was annealed at 350-400 °C for 1-4 h to obtain MgxV 2 O 5 •nH 2 O positive electrode material; wherein the electrolyte is 0.4M Mg(TFSI) 2 The magnesium salt was dissolved in ACN.
[0035] According to the above-mentioned implementation mode, several comparative examples and embodiments are given: Comparative Example 1: Magnesium metal foil was used as the negative electrode.
[0036] In a glove box (water and oxygen values < 0.1ppm), the prepared porous current collector, glass fiber separator, and magnesium metal foil were assembled into button cells. The electrolyte was 0.4MMg (TFSI) 2 The magnesium salt was dissolved in ACN. 0.5 mA / cm 2 After discharging for 4 h, magnesium metal was deposited on the porous current collector. The battery was then disassembled and the pre-magnesiumized current collector was washed and dried in ACN.
[0037] V 2 O 5 Granules, Mg(CH3COO) 2 The mixture was dissolved in deionized water at a molar ratio of 1:2.5, and stirred for 45 min after adding 5% hydrogen peroxide. The mixture was then reacted at 180 °C for 24 h, and the reaction product was annealed at 400 °C for 2 h to obtain the positive electrode active material MgxV 2 O 5 •nH 2 The prepared positive electrode active material, conductive carbon black, and PVDF were homogenized in a mass ratio of 7:2:1, coated on aluminum foil to obtain a positive electrode sheet, and assembled into a button cell with glass fiber and pre-magnesiumized negative electrode, using an electrolyte of 0.4M Mg(TFSI) 2 The magnesium salt was dissolved in ACN.
[0038] The prepared battery was subjected to a cycle test at a current density of 50 mA / g.
[0039] Comparative Example 2: In Comparative Example 1, the porous current collector is configured to be composed of alkali lignin and ZnCl 2 Made from raw materials.
[0040] Comparative Example 3: The porous current collector in Comparative Example 1 is set to be composed of alkali lignin and MgCl 2 Made from raw materials.
[0041] Comparative Example 4: The porous current collector in Comparative Example 1 is set to be composed of alkali lignin and MgCl 2 The negative electrode is coated with a 20nm layer of 0.7PbMg 1 / 3 Nb 2 / 3 O 3 -0.3PbTiO 3 . Embodiment 1:
[0042] Alkali lignin and MgCl 2 The solid precursor was added to deionized water at a mass ratio of 1:4, stirred at 60 °C for 90 min, and the water solvent was evaporated at 110 °C. The solid precursor was then heated to 800 °C at 10 °C / min for 3 h for carbonization. After cooling to room temperature, it was heated with CH 3 The porous carbon material current collector was obtained by washing with COOH for 90 min, washing with deionized water and drying.
[0043] In a glove box (water and oxygen values < 0.1 ppm), the prepared porous current collector, glass fiber separator, and Mg metal foil were assembled into a button cell, and the electrolyte was 0.4 M Mg (TFSI) 2 The magnesium salt was dissolved in ACN. 0.5 mA / cm 2 After 4 h of discharge, Mg metal was deposited on the porous current collector. The battery was then disassembled and the pre-magnesiumized current collector was washed and dried in ACN. The pre-magnesiumized current collector was transferred to a magnetron sputtering chamber to deposit the relaxor ferroelectric 0.7PbMg containing oxygen vacancies. 1 / 3 Nb 2 / 3 O 3 -0.3PbTiO 3 The negative electrode is made of the material layer, and the cavity is evacuated to 4×10 -5 Pa, Ar and O were introduced at 80 sccm 2 Mixed gas (volume ratio 4:1), working pressure is 2Pa, power is 80W, and thickness is 20nm.
[0044] V 2 O 5 Granules, Mg(CH3COO) 2It was dissolved in deionized water at a molar ratio of 1:2.5, and stirred for 45 min after adding 5% hydrogen peroxide, and then reacted at 180 °C for 24 h to obtain MgxV 2 O 5 The positive electrode material was annealed at 400°C for 2h. The active material, conductive carbon black, and PVDF were homogenized in a mass ratio of 7:2:1, coated on aluminum foil to obtain a positive electrode sheet, and assembled into a button cell with glass fiber and negative electrode. The electrolyte used was 0.4 Mmg (TFSI) 2 The magnesium salt was dissolved in ACN.
[0045] The prepared battery was subjected to a cycle test at a current density of 50 mA / g. Embodiment 2:
[0046] The porous current collector in Example 1 is configured to be composed of alkali lignin and MgC 2 O 4 The negative electrode is coated with 20nm oxygen vacancy 0.7PbMg 1 / 3 Nb 2 / 3 O 3 -0.3PbTiO 3 . Embodiment 3:
[0047] The porous current collector in Example 1 is configured to be composed of alkali lignin and Mg(HCO 3 ) 2 The negative electrode is coated with 20nm oxygen vacancy 0.7PbMg 1 / 3 Nb 2 / 3 O 3 -0.3PbTiO 3 . Embodiment 4:
[0048] The porous current collector in Example 1 is configured to be composed of alkali lignin and MgCl 2 The negative electrode is coated with 20nm PbMg containing oxygen vacancies 1 / 3 Nb 2 / 3 O 3 . Embodiment 5:
[0049] The porous current collector in Example 1 is configured to be composed of alkali lignin and MgCl 2 The negative electrode is coated with 20nm PbZn containing oxygen vacancies 1 / 3 Nb 2 / 3 O 3 . Embodiment 6:
[0050] The porous current collector in Example 1 is configured to be composed of alkali lignin and MgCl 2The negative electrode is coated with 0.7PbZn with 20nm oxygen vacancies. 1 / 3 Nb 2 / 3 O 3 -0.3PbTiO 3 .
[0051] The comparison results are shown in Table 1:
[0052] Table 1 summarizes the number of cycles when the battery capacity decays to 80%. Magnesium-doped porous carbon material current collector is an excellent host material for magnesium metal deposition. The rich pore structure and improved magnesium affinity can induce the deposition of magnesium in the three-dimensional current collector; nano-relaxed ferroelectric materials have dielectric properties superior to ferroelectric materials, which can better homogenize the electric field and ion field at the interface, guide the uniform migration of magnesium ion flow at the interface, and promote the uniform growth of magnesium metal on the negative electrode surface; oxygen vacancies in relaxor ferroelectric materials can capture lattice oxygen to avoid harmful side reactions between magnesium metal and lattice oxygen.
[0053] In summary, the present invention provides a porous current collector and its preparation process, a negative electrode and a magnesium metal battery. The inexpensive and readily available alkaline lignin is used as a raw material, an activator containing magnesium is introduced, and a magnesium-doped carbon-based porous current collector is obtained after carbonization treatment. The pore structure becomes a preferential nucleation site for magnesium metal, which alleviates the irregular deposition behavior. The magnesium metal negative electrode is introduced into the porous current collector by electrodeposition, and then a relaxor ferroelectric nanolayer containing oxygen vacancies is deposited on the surface of the negative electrode. The relaxor ferroelectric has a dielectric constant superior to that of traditional ferroelectric materials and has stronger polarization ability. It can more effectively regulate the distribution of the interfacial electric field and the ion field, promote the orderly deposition of magnesium, and thus inhibit the growth behavior of dendrites. The design of oxygen vacancies can also block the violent side reactions between magnesium metal and lattice oxygen, thereby improving the safety and stability of the battery during the cycle. The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A porous current collector, characterized in that: It includes a porous current collector made from alkali lignin and a magnesium-containing activator as raw materials; The alkali lignin and the magnesium-containing activator are carbonized to obtain a porous carbon material current collector doped with magnesium.
2. A porous current collector according to claim 1, characterized in that: The mass ratio of the alkali lignin to the magnesium-containing activator is 1:1-6.
3. A porous current collector according to claim 1, characterized in that: The magnesium-containing activator includes one or more of MgCl2, MgC2O4, Mg(HCO3)2, MgCO3, Mg(CH3COO)2, and Mg(OH)2.
4. A process for preparing a porous current collector as claimed in any one of claims 1 to 3, characterized in that: Includes steps: Add alkali lignin and magnesium-containing activator into deionized water in a mass ratio of 1:1-6, stir at 50-70°C for 30-120 minutes, and evaporate the solvent at 100-120°C; The solid precursor is heated to 500-900° C. for carbonization treatment for 1-4 hours, cooled to room temperature and then pickled for 30-90 minutes, washed with deionized water and dried to obtain a porous carbon material current collector.
5. A negative electrode, characterized in that: The invention comprises a porous current collector as claimed in any one of claims 1 to 3.
6. A negative electrode according to claim 5, characterized in that: The porous current collector is a pre-magnesiumized porous current collector; In addition, a relaxor ferroelectric nanolayer is plated on the surface of the pre-magnesiumized porous current collector.
7. A negative electrode according to claim 6, characterized in that: The relaxor ferroelectric nanolayer is a relaxor ferroelectric nanolayer having oxygen vacancies.
8. A negative electrode according to claim 6 or 7, characterized in that: The pre-magnesiation comprises: The porous carbon material current collector, glass fiber separator and magnesium metal foil are assembled into a button cell, and 0.4M Mg(TFSI)2 magnesium salt is dissolved in ACN as an electrolyte; Use 0.2-0.5 mA / cm 2 The battery is discharged for 4-10 hours to deposit magnesium metal on the porous carbon material current collector.
9. A negative electrode according to claim 6 or 7, characterized in that: The relaxor ferroelectric material is PbMg 1 / 3 Nb 2 / 3O3、PbZn 1 / 3 Nb 2 / 3 O3、(1-x)PbMg 1 / 3 Nb 2 / 3 O3-xPbTiO3 (0.1≤x≤0.3) and (1-x)PbZn 1 / 3 Nb 2 / 3 One of O3-xPbTiO3 (0.1≤x≤0.3), with a thickness of 10-100nm.
10. A magnesium metal battery, characterized in that: The invention comprises a negative electrode as claimed in any one of claims 5 to 9.
Citation Information
Patent Citations
Three-dimensional current collector for metal secondary battery anode and preparation and application thereof
CN106898778A
Multi-gradient flexible metal secondary battery negative electrode current collector and preparation method and application thereof
CN115995564A
Sodium metal negative electrode current collector and preparation method and application thereof
CN117996087A
Nitrogen-doped porous carbon material for aluminum battery as well as preparation method and application of nitrogen-doped porous carbon material
CN118651844A
Conductive porous material and electrode using same, and method for producing conductive porous material
WO2023243231A1