Proton exchange membrane and preparation method and application thereof

Through electrostatic self-assembly of single-atom vacancies titanium oxide nanosheets and positive polymers, a high-density negative-voltage single-atom vacancies titanium oxide nanosheets proton exchange membrane was prepared, solving the stability and conductivity of traditional proton exchange membranes at high temperatures. Problem, high proton selectivity and thermal stability at high temperatures are achieved, and are suitable for high temperature applications.

CN118943435APending Publication Date: 2024-11-12UNIV OF MACAU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411075107.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional proton exchange membranes lose moisture, expand or have their performance affected under high temperature conditions, making it difficult to maintain stability and high proton conductivity in an environment above 100°C.

Method used

Single-atom vacancies titanium oxide nanosheets are used as raw materials, and prepared by ion exchange and mechanical oscillation peeling to form high-density negative single atom vacancies. Combined with positive-electric polymers, electrostatic self-assembly is prepared to prepare an ultra-thin proton exchange membrane with high protons. Selectivity and thermal stability.

Benefits of technology

It achieves the maintenance of structural stability and high proton conductivity at high temperatures. Proton conduction does not depend on wettization conditions and is suitable for high-temperature applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943435A_ABST
    Figure CN118943435A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nano materials, and discloses a proton exchange membrane as well as a preparation method and application thereof. The proton exchange membrane comprises monatomic vacancy titanium oxide nanosheets which are stacked and stacked, the molecular formula of the single-atom vacancy titanium oxide nanosheet is selected from at least one of the following components: # imgabs0 #. The proton exchange membrane provided by the invention is ultrathin and adjustable in thickness, controllable in area, high in proton selectivity, high in proton conductivity and good in thermal stability; the preparation method of the proton exchange membrane is simple in steps and suitable for industrial application; the proton exchange membrane can meet the application requirements of high-temperature occasions in the fields of energy conversion and storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials, and in particular to a proton exchange membrane and a preparation method and application thereof. Background Art

[0002] Proton Exchange Membrane (PEM) is an important functional material, widely used in energy conversion and storage, such as fuel cells and water electrolysis to produce hydrogen. Commonly used proton exchange membrane materials include polytetrafluoroethylene-modified fluorinated polyurethane membrane (Nafion), sulfonated polyether ether ketone membrane (SPEEK) and phosphoric acid polymer membrane. These traditional proton exchange membrane materials can play a good role in environments below 60°C, but for some applications that need to be used under high temperature conditions above 100°C, such as high temperature oxidation, high temperature electrolysis, high temperature acid-base catalysis, etc., traditional proton exchange membranes are often not competent. For example, Nafion is highly dependent on moisture and needs to strictly control moisture content. It is easy to lose moisture and degrade under high temperature conditions above 80°C, which seriously affects its structural stability in high temperature applications; SPEEK is prone to large expansion at high temperatures, resulting in mismatch with other components and affecting the performance and life of the overall structure; phosphoric acid polymer membranes are sensitive to humidification conditions and require sufficient moisture to maintain effective proton conduction. Excessive drying caused by high temperature will significantly affect the performance of the membrane. Therefore, it is of great significance to develop new proton exchange membrane materials to ensure the high proton conductivity of the proton exchange membrane while improving its stability at high temperatures. Summary of the invention

[0003] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, one of the purposes of the present invention is to provide a proton exchange membrane; the second purpose of the present invention is to provide a method for preparing the proton exchange membrane; the third purpose of the present invention is to provide an application of the proton exchange membrane.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is:

[0005] The basic principle of the present invention is described as follows:

[0006] 1) The present invention uses single-atom vacancy titanium oxide nanosheets as raw materials to prepare proton exchange membranes. The single-atom vacancy titanium oxide nanosheets are prepared by ion exchange and mechanical vibration exfoliation of layered titanium oxide. During this process, due to the loss of some titanium atoms, high-density and negatively charged single-atom vacancies are spontaneously introduced into the titanium oxide nanosheets. Single-atom vacancies at the nanoscale can impose strong restrictions on other ions or molecules while allowing only protons to pass through, resulting in high proton selectivity.

[0007] 2) Compared with the macromolecular polymer materials of traditional proton exchange membranes, the thickness of single-atom vacancy titanium oxide nanosheets is only about 1.1 nanometers. These ultra-thin channels with nanometer thickness are conducive to the rapid passage of protons, thereby maximizing proton conductivity.

[0008] 3) Single-atom vacancy titanium oxide nanosheets have excellent thermal stability and can maintain structural stability at high temperatures. Therefore, using single-atom vacancy titanium oxide as raw material can prepare ultra-thin proton exchange membranes with high proton selectivity, high proton conductivity and good thermal stability.

[0009] A first aspect of the present invention provides a proton exchange membrane comprising stacked single-atom vacancy titanium oxide nanosheets;

[0010] The molecular formula of the single-atom vacancy titanium oxide nanosheet is selected from at least one of the following:

[0011] Preferably, the single-atom vacancy density of the single-atom vacancy titanium oxide nanosheet is 9% to 15%.

[0012] Preferably, the size of a single vacancy in the single-atom vacancy titanium oxide nanosheet is (0.28-0.32) nm×(0.35-0.40) nm; further preferably, the size of a single vacancy in the single-atom vacancy titanium oxide nanosheet is (0.29-0.31) nm×(0.37-0.39) nm.

[0013] Preferably, the thickness of the single-atom vacancy titanium oxide nanosheet is 0.8-1.5 nm; further preferably, the thickness of the single-atom vacancy titanium oxide nanosheet is 0.9-1.2 nm.

[0014] Preferably, the proton exchange membrane has a thickness of 10 to 1000 nm.

[0015] Preferably, the membrane area of ​​the proton exchange membrane is 1 to 100 cm 2 .

[0016] The second aspect of the present invention provides a method for preparing the proton exchange membrane according to the first aspect of the present invention, comprising the following steps:

[0017] The single-atom vacancy titanium oxide nanosheets are self-assembled layer by layer on the substrate surface through the electrostatic force between the nanosheets and the positively charged polymer to obtain the proton exchange membrane.

[0018] Specifically, the single-atom vacancy titanium oxide nanosheets have high-density and negatively charged single-atom vacancies, and the positively charged polymer has a positive charge. When the single-atom vacancy titanium oxide nanosheets come into contact with the positively charged polymer, electrostatic force is generated, allowing the single-atom vacancy titanium oxide nanosheets to be stacked layer by layer.

[0019] Preferably, the positively charged polymer is prepared in the form of an aqueous solution.

[0020] Preferably, the volume mass fraction of the positively charged polymer aqueous solution is 20 to 30 g / L.

[0021] Preferably, the pH value of the positively charged polymer aqueous solution is 9-11; more preferably, the pH value of the positively charged polymer aqueous solution is 9-10.

[0022] Preferably, the positively charged polymer comprises polydiallyldimethylammonium chloride (PDDA).

[0023] Preferably, the single-atom vacancy titanium oxide nanosheets are prepared in the form of a suspension.

[0024] Preferably, the volume mass fraction of the single-atom vacancy titanium oxide nanosheet suspension is 0.02 to 0.16 g / L; further preferably, the volume mass fraction of the single-atom vacancy titanium oxide nanosheet suspension is 0.04 to 0.16 g / L.

[0025] Preferably, the pH value of the single-atom vacancy titanium oxide nanosheet suspension is 9-11; further preferably, the pH value of the single-atom vacancy titanium oxide nanosheet suspension is 9-10.

[0026] Preferably, the pH values ​​of the positively charged polymer aqueous solution and the single-atom vacancy titanium oxide nanosheet suspension are adjusted by hydrochloric acid (HCl) and tetra-n-butylammonium hydroxide (TBAOH).

[0027] Specifically, the present invention utilizes the electrostatic force between negatively charged single-atom vacancy titanium oxide nanosheets and positively charged positively charged polymers for layer-by-layer adsorption. Titanium oxide will partially adsorb positively charged hydrogen ions in an acidic environment, hindering the full adsorption of the positively charged polymer, thereby affecting the uniformity and integrity of the positively charged polymer adsorption layer, resulting in uneven thickness of the titanium oxide film finally formed. Therefore, it is necessary to control the pH value of the positively charged polymer aqueous solution and the single-atom vacancy titanium oxide nanosheet suspension to be alkaline, and the adsorption effect is better when the pH value is 9 to 10.

[0028] Preferably, the substrate is selected from any one of quartz, glass and silicon wafer.

[0029] Preferably, the substrate area is 1 to 100 cm 2 .

[0030] Preferably, the shape of the substrate can be selected from any shape such as circular, rectangular, etc.

[0031] Specifically, the shape and membrane area of ​​the proton exchange membrane can be accurately controlled by changing the shape and area of ​​the substrate.

[0032] Preferably, the method specifically comprises the following steps:

[0033] S1, immersing the substrate in a suspension of single-atom vacancy titanium oxide nanosheets to form a single-atom vacancy titanium oxide film on the surface;

[0034] S2, immersing the substrate carrying the single-atom vacancy titanium oxide film into a positively charged polymer aqueous solution to form a single-atom vacancy titanium oxide film adsorbing positively charged polymer molecules on the surface;

[0035] S3, repeating steps S1 and S2, annealing to remove the positively charged polymer, and obtaining the proton exchange membrane.

[0036] Preferably, in step S1, the soaking time is 5 to 90 minutes; more preferably, the soaking time is 5 to 20 minutes.

[0037] Preferably, in the step S1, a pure water washing step is also included after the soaking is completed.

[0038] Preferably, in step S2, the soaking time is 20 to 30 minutes; more preferably, the soaking time is 5 to 20 minutes.

[0039] Preferably, in the step S2, a pure water washing step is also included after the soaking is completed.

[0040] Preferably, in the step S3, before annealing, the step also includes drying the single-atom vacancy titanium oxide film that adsorbs the positively charged polymer molecules.

[0041] Preferably, in step S3, the annealing temperature is 300-800°C; more preferably, the annealing temperature is 300-500°C.

[0042] Preferably, in step S3, annealing is performed under a protective atmosphere; the protective atmosphere is selected from nitrogen or argon.

[0043] Preferably, in step S3, the number of times of repeating steps S1 and S2 is regulated according to the thickness of the proton exchange membrane to be obtained.

[0044] The method for preparing a proton exchange membrane provided by the present invention can form proton exchange membranes on the upper and lower surfaces of a substrate respectively after one preparation. After the preparation is completed, two groups of thin films are removed from the surface of the substrate respectively by dry or wet transfer to obtain two groups of identical proton exchange membranes.

[0045] The third aspect of the present invention provides the application of the proton exchange membrane described in the first aspect of the present invention in the field of energy conversion and storage.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] 1) The proton exchange membrane provided by the present invention has a thin thickness, controllable thickness, area and shape, high proton selectivity, high proton conductivity and good thermal stability.

[0048] 2) The method for preparing the proton exchange membrane provided by the present invention regulates the shape and membrane area of ​​the proton exchange membrane by the shape and size of the substrate, and controls the thickness of the proton exchange membrane by the adsorption times of the single-atom vacancy titanium oxide nanosheets and the positively charged polymer. The steps are simple and suitable for industrial use.

[0049] 3) The proton conduction of the proton exchange membrane provided by the present invention does not rely on humidification conditions, and there is no need to consider the weakening of the proton conductivity caused by drying and dehydration caused by high temperature, and can meet the application requirements of high-temperature occasions in the field of energy conversion and storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 Schematic diagram of the single-atom vacancy titanium oxide / PDDA composite film in Example 1, wherein 1-substrate, 2-single-atom vacancy titanium oxide nanosheet, 3-PDDA;

[0051] Figure 2 is the proton conductivity of the single-atom vacancy titanium oxide nanosheet at different temperatures in Example 1;

[0052] Figure 3 The XPS graphs of the single-atom vacancy titanium oxide nanosheets before and after high-temperature heating in Example 1;

[0053] Figure 4 This is an atomic force microscope image of the single-atom vacancy titanium oxide nanosheet in Example 1 after being heated at 300° C. for 1 hour;

[0054] Figure 5 is the current-voltage curve of the single-atom vacancy titanium oxide nanosheet in hydrochloric acid solution in Example 1;

[0055] Figure 6 is the electrical conductivity of the single-atom vacancy titanium oxide nanosheet in Example 1 in different electrolytes. DETAILED DESCRIPTION

[0056] The present invention is further described in detail below by specific examples. The raw materials, reagents or devices used in the examples can be obtained from conventional commercial sources or by prior art methods unless otherwise specified. Unless otherwise specified, the experiments or test methods are conventional methods in the art.

[0057] The thickness of the single-atom vacancy titanium oxide nanosheets in Examples 1-3 is about 1.1 nm. The nanosheets have high-density negatively charged single-atom vacancies, each of which has a size of about 0.30 nm×0.38 nm. The single-atom vacancy densities are 13%, 9%, and 11.11%, respectively.

[0058] Example 1

[0059] This embodiment provides a proton exchange membrane, which is prepared by the following steps:

[0060] S1. Cut the clean silicon wafer into 1cm×1cm size and immerse it in single atomic vacancy titanium oxide nanosheets. In the suspension, the suspension volume mass fraction is 0.04 g / L, the suspension pH is adjusted to 9 by adding HCl and TBAOH, soaked for 20 min, taken out and rinsed with water, and a single atomic vacancy titanium oxide film is obtained;

[0061] S2, immersing the substrate with the single-atom vacancy titanium oxide film attached into a PDDA aqueous solution, wherein the volume mass fraction of PDDA is 20 g / L, adding HCl and TBAOH to adjust the pH of the suspension to 9, soaking for 20 minutes, taking out and rinsing with water to obtain a single-atom vacancy titanium oxide film adsorbed with PDDA molecules;

[0062] S3, repeat the operations in steps S1 and S2 50 times to obtain 50 layers of single-atom vacancy titanium oxide / PDDA composite films; dry the 50 layers of single-atom vacancy titanium oxide / PDDA composite films with nitrogen, and place them in nitrogen at 300°C to fully anneal to remove PDDA, thereby obtaining two sets of proton exchange membranes, each with an area of ​​1 cm 2 , each with a thickness of approximately 90nm.

[0063] Example 2

[0064] This embodiment provides a proton exchange membrane, which is prepared by the following steps:

[0065] S1. Cut the clean silicon wafer into a 2 cm diameter circle and immerse it in the single atomic vacancy titanium oxide nanosheet. In the suspension, the suspension volume mass fraction is 0.08 g / L, the suspension pH is adjusted to 9 by adding HCl and TBAOH, soaked for 10 min, taken out and rinsed with water, and a single atomic vacancy titanium oxide film is obtained;

[0066] S2, immersing the substrate with the single-atom vacancy titanium oxide film attached into a PDDA aqueous solution, wherein the volume mass fraction of PDDA is 25 g / L, adding HCl and TBAOH to adjust the pH of the suspension to 9, soaking for 10 minutes, taking out and rinsing with water to obtain a single-atom vacancy titanium oxide film adsorbed with PDDA molecules;

[0067] S3, repeat the operations in steps S1 and S2 10 times to obtain 10 layers of single-atom vacancy titanium oxide / PDDA composite films; dry the 10 layers of single-atom vacancy titanium oxide / PDDA composite films with nitrogen, and place them in nitrogen at 300°C to fully anneal and remove PDDA, thereby obtaining two sets of proton exchange membranes, each with an area of ​​3.14 cm 2 , each with a thickness of approximately 20 nm.

[0068] Example 3

[0069] This embodiment provides a proton exchange membrane, which is prepared by the following steps:

[0070] S1. Cut the clean silicon wafer into 10cm×10cm size and immerse it in single atomic vacancy titanium oxide nanosheets. In the suspension, the suspension volume mass fraction is 0.016 g / L, the suspension pH is adjusted to 9 by adding HCl and TBAOH, soaked for 5 min, taken out and rinsed with water, and a single atomic vacancy titanium oxide film is obtained;

[0071] S2, immersing the substrate with the single-atom vacancy titanium oxide film attached into a PDDA aqueous solution, wherein the volume mass fraction of PDDA is 30 g / L, adding HCl and TBAOH to adjust the pH of the suspension to 9, soaking for 5 minutes, taking out and rinsing with water to obtain a single-atom vacancy titanium oxide film adsorbed with PDDA molecules;

[0072] S3, repeat the operations in steps S1 and S2 for 5 times to obtain 5 layers of single-atom vacancy titanium oxide / PDDA composite film; blow dry the 10 layers of single-atom vacancy titanium oxide / PDDA composite film with nitrogen, and place it in nitrogen at 300°C to fully anneal to remove PDDA, so as to obtain two sets of proton exchange membranes, each with an area of ​​100 cm 2 , each with a thickness of approximately 10 nm.

[0073] Figure 1 Schematic diagram of the single-atom vacancy titanium oxide / PDDA composite film in Example 1. Figure 1 It can be seen that single-atom vacancy titanium oxide nanosheets and PDDA are adsorbed on the substrate surface in sequence to form a single-atom vacancy titanium oxide / PDDA composite film. In the subsequent steps, PDDA is removed by annealing treatment to obtain a proton exchange membrane formed by stacking single-atom vacancy titanium oxide nanosheets layer by layer.

[0074] Performance Testing and Characterization

[0075] 1. Testing the single-atom vacancy titanium oxide nanosheets in Example 1 Proton conductivity at different temperatures:

[0076] Figure 2 is the proton conductivity of the single-atom vacancy titanium oxide nanosheet at different temperatures in Example 1, Figure 2 It can be seen that the proton conductivity of the single-atom vacancy titanium oxide nanosheets used in Example 1 increases with increasing temperature, and the proton conductivity at a high temperature of 260°C is as high as 200 S / cm -2 Using this as raw material to prepare proton exchange membrane is beneficial to improving the thermal stability of the proton exchange membrane, so that the proton exchange membrane has both high proton conductivity and high temperature stability.

[0077] 2. Testing the single-layer titanium oxide nanosheet in Example 1 X-ray photoelectron spectra before and after high temperature heating:

[0078] The single atomic vacancy titanium oxide nanosheets were annealed in air at 200℃ and 300℃ for 3h. Figure 3 This is the XPS graph of the single-atom vacancy titanium oxide nanosheet in Example 1 before and after high-temperature heating, where: Figure 3 (a) Ti 2p structure of single atomic vacancy titanium oxide nanosheets before and after annealing. 1 / 2 and Ti 2p 3 / 2 Energy spectrum, Figure 3 (b) is the Ti-O bond energy spectrum of single-atom vacancy titanium oxide nanosheets before and after annealing. Figure 3 It can be seen that after the single-atom vacancy titanium oxide nanosheets used in Example 1 were annealed in air at 200°C and 300°C for 3h, the Ti 2p 1 / 2 、Ti 2p 3 / 2 As well as the characteristic peak shape and intensity of the Ti-O bond, there is no difference compared with before annealing, indicating that the chemical structure of the raw material has not changed at a high temperature of 300°C.

[0079] 3. Testing the single-atom vacancy titanium oxide nanosheets in Example 1 Atomic force microscopy image after heating at 300℃ for 1h:

[0080] Figure 4 This is an atomic force microscope image of the single-atom vacancy titanium oxide nanosheet in Example 1 after being heated at 300°C for 1 hour. Figure 4 It can be seen that the single-atom vacancy titanium oxide nanosheets still retain their two-dimensional structure after being heated at 300°C, without any gaps or cracks, and the crystal structure is stable.

[0081] 4. Testing the single-atom vacancy titanium oxide nanosheets in Example 1 Current-voltage curve in hydrochloric acid solution:

[0082] The test method is as follows: the concentrations of hydrochloric acid on both sides of the nanosheet are 0.1 mol / L and 1 mol / L respectively, silver / silver chloride electrodes are inserted into the hydrochloric acid on both sides, and voltage is applied to test the transmission current of ions penetrating the single-atom vacancy titanium oxide nanosheet. Figure 5 is the current-voltage curve of the single-atom vacancy titanium oxide nanosheet in hydrochloric acid solution in Example 1, Figure 5 It can be seen that the zero current voltage is -59mV, and the proton (H + ) migration number is 1, indicating that all the current is provided by protons. Only protons can pass through the single-atom vacancy titanium oxide nanosheets while chloride ions cannot pass through. That is, the raw material single-atom vacancy titanium oxide nanosheets has proton selectivity.

[0083] 5. Testing the single-atom vacancy titanium oxide nanosheets in Example 1 Conductivity in different electrolytes:

[0084] Figure 6 is the conductivity of the single-atom vacancy titanium oxide nanosheet in Example 1 in different electrolytes, Figure 6 It can be seen that the electrical conductivity of single-atom vacancy titanium oxide nanosheets in hydrochloric acid is two orders of magnitude higher than that in other electrolytes, indicating that except protons, other cations (including the smallest cation lithium ions) cannot pass through single-atom vacancy titanium oxide nanosheets, that is, the raw material single-atom vacancy titanium oxide nanosheets have proton selectivity.

[0085] The proton exchange membrane provided by the present invention is formed by stacking and piling up single-atom vacancy titanium oxide nanosheets. The single-atom vacancy titanium oxide nanosheets have high-density and negatively charged single-atom vacancies, which only allow protons to pass through and have high selectivity; the single-atom vacancy titanium oxide nanosheets have good thermal stability and high-temperature proton conductivity, and can maintain structural stability in air above 300°C. The proton exchange membrane obtained by stacking and piling up single-atom vacancy titanium oxide nanosheets also has high proton selectivity and thermal stability, and its proton conduction does not rely on humidification conditions. Compared with traditional proton exchange membranes, there is no need to consider the weakening of proton conductivity caused by drying and dehydration caused by high temperature, and it can meet the application requirements of high-temperature occasions.

Claims

1. A proton exchange membrane, characterized in that: Includes layer-by-layer stacked single-atom vacancy titanium oxide nanosheets; The molecular formula of the single-atom vacancy titanium oxide nanosheet is selected from at least one of the following:

2. The proton exchange membrane according to claim 1, characterized in that The single-atom vacancy density of the single-atom vacancy titanium oxide nanosheet is 9% to 15%; And / or, the single vacancy size of the single atomic vacancy titanium oxide nanosheet is (0.28-0.32) nm×(0.35-0.40) nm; And / or, the thickness of the single-atom vacancy titanium oxide nanosheet is 0.8-1.5 nm.

3. The proton exchange membrane according to claim 1, characterized in that The thickness of the proton exchange membrane is 10 to 1000 nm; And / or, the membrane area of ​​the proton exchange membrane is 1 to 100 cm 2 .

4. The method for preparing a proton exchange membrane according to any one of claims 1 to 3, characterized in that: The following steps are involved: The single-atom vacancy titanium oxide nanosheets are self-assembled layer by layer on the substrate surface through the electrostatic force between the nanosheets and the positively charged polymer to obtain the proton exchange membrane.

5. The preparation method according to claim 4, characterized in that: The positively charged polymer is prepared in the form of an aqueous solution; Preferably, the volume mass fraction of the positively charged polymer aqueous solution is 20 to 30 g / L; Preferably, the pH value of the positively charged polymer aqueous solution is 9 to 11; Preferably, the positively charged polymer comprises polydiallyldimethylammonium chloride.

6. The preparation method according to claim 4, characterized in that: The single-atom vacancy titanium oxide nanosheets are prepared in the form of a suspension; Preferably, the volume mass fraction of the single-atom vacancy titanium oxide nanosheet suspension is 0.02 to 0.16 g / L; Preferably, the pH value of the single-atom vacancy titanium oxide nanosheet suspension is 9-11.

7. The preparation method according to claim 4, characterized in that: The substrate is selected from any one of quartz, glass and silicon wafer.

8. The preparation method according to claim 7, characterized in that: The method specifically comprises the following steps: S1, immersing the substrate in a suspension of single-atom vacancy titanium oxide nanosheets to form a single-atom vacancy titanium oxide film on the surface; S2, immersing the substrate carrying the single-atom vacancy titanium oxide film into a positively charged polymer aqueous solution to form a single-atom vacancy titanium oxide film adsorbing positively charged polymer molecules on the surface; S3, repeating steps S1 and S2, annealing to remove the positively charged polymer, and obtaining the proton exchange membrane.

9. The preparation method according to claim 8, characterized in that: In step S1, the soaking time is 5 to 90 minutes; And / or, in step S2, the soaking time is 20 to 30 minutes; And / or, in step S3, the annealing temperature is 300-800°C.

10. Use of the proton exchange membrane according to any one of claims 1 to 3 in the field of energy conversion and storage.