High-thermal-conductivity energy storage battery material, preparation method thereof and flow battery structure
By using electrolyte composed of high thermal conductivity of vanadium and iron ions in all vanadium flow batteries, and combining the heat dissipation structure, the problem of insufficient battery stability at extreme temperatures is solved, and a wider temperature adaptability and high-efficiency energy conversion are achieved. .
Patent Information
- Application Number
- CN202411369721.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing all-vanadium flow batteries require additional temperature control measures in extremely high or low temperature environments, which increases system complexity and cost, and the electrolyte is insufficient in stability within the temperature range.
Using high thermal conductivity energy storage battery materials, including positive electrode electrolyte and negative electrode electrolyte, consisting of vanadium ions and iron ions, vanadate and iron ions are generated through the electrolysis process, and sulfuric acid-hydrochloric acid solution is added to form high concentration and high stability. The electrolyte is provided in the liquid flow battery structure, and a heat dissipation hole and a motor-driven heat dissipation fan blade are installed to adapt to different temperature environments.
Improve the stability and energy efficiency of the electrolyte over a wider temperature range, reduce the capacitance loss rate, optimize the electrochemical performance and cost-effectiveness, and adapt to applications in extreme climate conditions.
Smart Images

Figure CN118943445A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of liquid flow batteries and relates to a liquid flow battery, in particular to a high thermal conductivity energy storage battery material and a preparation method thereof and a liquid flow battery structure. Background Art
[0002] All-vanadium, Fe-Cr, Na-S, Zn-Br and other metal ion flow batteries are green and environmentally friendly energy storage batteries. They are redox energy storage flow batteries that use different valence ions as positive and negative active substances dissolved in supporting electrolytes in a liquid circulating flow state. Among them, all-vanadium, Fe-Cr and others have been applied to renewable energy storage, grid peak regulation, backup power supply and other fields. All-vanadium flow batteries have the advantages of high energy conversion efficiency, long service life, adjustable capacity according to user requirements, high safety and environmental friendliness, and have become one of the most promising methods for large-scale energy storage such as wind energy, solar energy and electricity peak shaving and valley filling.
[0003] After searching, for example, Chinese patent documents disclose an electrolyte for all-vanadium flow battery and a preparation method thereof, as well as an all-vanadium flow battery including the electrolyte [Application No.: 200910148218.0; Publication No.: CN101572319A]. This electrolyte for all-vanadium flow battery and a preparation method thereof, as well as an all-vanadium flow battery including the electrolyte, prepares a positive electrode electrolyte precursor and a negative electrode electrolyte precursor for all-vanadium flow battery according to the difference in solubility of vanadium compounds of different valence states in sulfuric acid solutions of different concentrations; then, high-concentration, high-stability positive electrode electrolyte and negative electrode electrolyte are obtained respectively by electrolysis.
[0004] Although the electrolyte of the all-vanadium liquid flow battery disclosed in this patent has high stability and performs well within a specific temperature range, the all-vanadium liquid flow battery may require additional temperature control measures to maintain performance in extremely high or low temperature environments, which may increase the complexity and cost of the system. Summary of the invention
[0005] The first purpose of the present invention is to address the above-mentioned problems in the existing technology and to propose a high thermal conductivity energy storage battery material. The technical problem to be solved by the invention is: how to achieve stable adaptation of energy storage battery materials to a wider temperature range.
[0006] The first object of the present invention can be achieved by the following technical solutions: A high thermal conductivity energy storage battery material, comprising a positive electrode electrolyte and a negative electrode electrolyte, wherein the positive electrode electrolyte is composed of a sulfuric acid-hydrochloric acid solution containing vanadium ions and iron ions, wherein the vanadium ions are tetravalent vanadium ions (V 4+ ) and pentavalent vanadium ions (V 5 +), the vanadium ion concentration is 1.2-2.4 mol / L, the iron ion concentration is 0.3-0.6 mol / L, the positive electrode electrolyte contains vanadium ions, 6-10 parts of iron ions and sulfuric acid-hydrochloric acid solution in a ratio of 4:1:5, and the negative electrode electrolyte is composed of a sulfuric acid-hydrochloric acid solution containing vanadium and vanadium ions, and the vanadium ions are divalent vanadium ions (V 2+ ) and trivalent vanadium ions (V 3+ ), the vanadium ion concentration is 2.0-2.8 mol / L, and the ratio of vanadium ions and sulfuric acid-hydrochloric acid solution in the negative electrode electrolyte is 4:5.
[0007] The vanadium ions are generated by electrolysis of vanadate, the purity of vanadate is 99.9%, and the iron ions are generated by electrolysis of iron sheets.
[0008] The sulfuric acid-hydrochloric acid solution contains sulfate and chloride ions, wherein the concentration of sulfate is 2.0-3.2 mol / L and the concentration of chloride ions is 6.2-6.8 mol / L.
[0009] The second purpose of the present invention is to propose a method for preparing a high thermal conductivity energy storage battery material in view of the above-mentioned problems existing in the prior art. The technical problem to be solved by the invention is: how to ensure that the energy efficiency of the electrolyte is improved and the capacity loss rate is reduced during the use of the battery in low-temperature and high-temperature environments.
[0010] The second object of the present invention can be achieved by the following technical solutions: A method for preparing a high thermal conductivity energy storage battery material comprises the following steps: Step 1: placing the vanadate and the iron sheet into an electrolytic cell, the electrolytic cell containing a sulfuric acid solution, turning on the power supply of the electrolytic cell, and during the electrolysis process, the iron sheet undergoes an oxidation reaction at the anode to generate Fe2+ ions, and the vanadate undergoes an oxidation reaction at the anode to generate V5+ ions; The iron sheet and vanadate undergo a hydrogen ion reduction reaction at the cathode, and the reaction is expressed as: 2H++2e−→H2↑. In this reaction, hydrogen ions obtain electrons from the electrolyte and form hydrogen (H2) on the cathode surface and release it; The vanadium ions in the vanadate undergo a reduction reaction at the cathode, and the reaction is as follows: V5++e−→V4+In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V4+), forming a cathode electrolyte precursor; Step 2: placing the vanadate in an electrolytic cell, the electrolytic cell containing a sulfuric acid solution, turning on the power supply of the electrolytic cell, during the electrolysis process, the vanadate undergoes an oxidation reaction at the anode to generate V5+ ions, and the vanadate undergoes a reduction reaction of hydrogen ions at the cathode, and the reaction is shown as: 2H++2e−→H2↑, in which the hydrogen ions obtain electrons from the electrolyte, and hydrogen (H2) is formed and released on the cathode surface, and the vanadium ions in the vanadate undergo a reduction reaction, and the reaction is shown as: V5++e−→V4+, in which the pentavalent vanadium ions obtain an electron from the electrolyte and are reduced to tetravalent vanadium ions (V4+), and V4+ continues to undergo a reduction reaction to generate V2+ and V3+ ions, forming a negative electrode electrolyte precursor; Step 3: Filtration: Add a reducing agent containing chloride ions to the positive electrode electrolyte precursor and the negative electrode electrolyte precursor to generate a positive electrode electrolyte and a negative electrode electrolyte.
[0011] The positive electrode electrolyte contains V5+, V4+, Fe2+ ions, sulfate ions and chloride ions, and the negative electrode electrolyte contains V2+, V3+, sulfate ions and chloride ions.
[0012] The chloride ion concentration is 6.2 mol / L, and the sulfate concentration is 2.5 mol / L.
[0013] A liquid flow battery structure includes a positive electrode storage tank, a negative electrode storage tank, a first circulation pump, a second circulation pump and two end plates, a battery stack is fixed between the two end plates, the positive electrode storage tank is filled with a positive electrode electrolyte, and the negative electrode storage tank is filled with a negative electrode electrolyte. The electrolytes are positive electrode electrolytes and negative electrode electrolytes prepared by the method for preparing high thermal conductivity energy storage battery materials.
[0014] With the above structure, during the charging process, the external power supply provides electrical energy through the positive and negative electrodes of the battery, the V+ ions in the positive electrode electrolyte will lose electrons and be oxidized into V+ ions, and the Fe+ ions in the positive electrode electrolyte will lose electrons and be oxidized into trivalent iron ions (Fe+). During the discharge process, the chemical energy inside the battery is converted into electrical energy and released, and the vanadium-iron ions are stably converted into ions within a wider temperature range.
[0015] A heat dissipation hole is provided on the side of the end plate away from the fuel cell stack, a dustproof net is fixed in the heat dissipation hole, an angle steel is fixed to the front end of the end plate, a first motor is fixed on the angle steel, a rotating plate is fixed to the output end of the first motor, a rotating cover is fixed to the lower end of the rotating plate, the specification of the rotating cover is adapted to the heat dissipation hole, a second motor is fixed to the front end of the rotating cover, a rotating shaft is fixed to the output end of the second motor, and heat dissipation fan blades are fixed on the rotating shaft.
[0016] With the above structure, in a high temperature environment, the first motor is operated to drive the rotating plate to rotate, and the rotating cover rotates with the rotating plate to expose the heat dissipation holes to dissipate the temperature inside the battery stack. The second motor is operated to drive the rotating shaft to rotate, and the heat dissipation fan blades rotate with the rotating shaft to accelerate the air circulation around the heat dissipation holes and enhance heat dissipation.
[0017] A first sealing ring is fixed in the heat dissipation hole, a second sealing ring is fixed at the rear end of the rotating cover, and an outer wall of the second sealing ring contacts an inner wall of the first sealing ring.
[0018] With the above structure, in a low-temperature environment, the first motor is operated to drive the rotating plate to rotate, the rotating cover moves closer to the end plate with the rotating plate, and the second sealing ring contacts the first sealing ring with the rotating cover until it is a tight ring sleeve, thereby reducing air circulation at the battery stack and allowing the temperature generated during its own operation to accumulate to adapt to the low-temperature environment.
[0019] The front end of the end version is integrally formed with a connecting piece, the first motor output end is passed through the connecting piece on the left and right sides, and the connecting piece is rotatably connected to the rotating plate.
[0020] With the above structure, the connecting member is used to support the output shaft of the first motor, thereby improving the stability of the rotating cover driven by the first motor.
[0021] Compared with the prior art, the high thermal conductivity energy storage battery material and its preparation method and flow battery structure have the following advantages: 1. By adding vanadium ions and iron ions to the sulfuric acid-hydrochloric acid solution, the cyclic voltammetry and AC impedance tests of the electrolyte performed well, which means less energy loss and higher efficiency during the charge and discharge process, optimizing its electrochemical performance.
[0022] 2. Adding iron ions when the vanadium concentration meets the standard can reduce its material cost and show high cost-effectiveness in long-term application.
[0023] 3. By adding iron ions to the electrolyte, the environmental adaptability of the flow battery is enhanced, so that the flow battery can work stably in a wider temperature range, and the application of the flow battery outdoors or under extreme climatic conditions is optimized.
[0024] 4. By adding iron ions, the electrolyte system can use sulfuric acid-hydrochloric acid mixed acid, so that the iron-vanadium electrolyte can maintain good stability and high energy conversion efficiency under a variety of environments and operating conditions.
[0025] 5. By opening heat dissipation holes on the end plate of the liquid flow battery, and the opening and closing of the heat dissipation holes can be controlled by a motor, and adding a cooling fan can accelerate air circulation and optimize heat dissipation conditions in a high temperature environment, the liquid flow battery can adapt to a wider range of ambient temperatures from the inside out. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1This is a table of steps for preparing the high thermal conductivity energy storage battery material of the present invention.
[0027] Figure 2 It is a schematic table of the composition of the high thermal conductivity energy storage battery material in the present invention.
[0028] Figure 3 It is a schematic diagram of the structure of the liquid flow battery in the present invention.
[0029] Figure 4 It is a structural schematic diagram of the end cover part of the present invention.
[0030] Figure 5 yes Figure 4 A magnified view of the structure at center.
[0031] Figure 6 It is a structural schematic diagram of the rotary cover of the present invention.
[0032] Figure 7 yes Figure 6 A magnified view of the structure at point B.
[0033] Figure 8 yes Figure 6 Enlarged view of the structure at C in the middle.
[0034] In the figure, 101, negative electrode liquid storage tank; 102, positive electrode liquid storage tank; 201, end plate; 202, fuel cell stack; 301, first circulation pump; 302, second circulation pump; 4, heat dissipation hole; 5, dust screen; 6, rotating plate; 7, rotating cover; 8, connecting piece; 9, second motor; 10, rotating shaft; 11, heat dissipation fan blade; 12, first sealing ring; 13, second sealing ring; 14, angle steel; 15, first motor. DETAILED DESCRIPTION
[0035] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.
[0036] Embodiment 1 like Figure 2 As shown, the high thermal conductivity energy storage battery material includes a positive electrode electrolyte and a negative electrode electrolyte. The positive electrode electrolyte is composed of a sulfuric acid-hydrochloric acid solution containing vanadium ions and iron ions. The vanadium ions are tetravalent vanadium ions (V 4+ ) and pentavalent vanadium ions (V 5+ ), the vanadium ion concentration is 1.2mol / L, the iron ion concentration is 0.3mol / L, the ratio of vanadium ions, iron ions and sulfuric acid-hydrochloric acid solution in the positive electrolyte is 4:1:5, and the negative electrolyte is composed of sulfuric acid-hydrochloric acid solution containing vanadium and vanadium ions, and the vanadium ions are divalent vanadium ions (V 2+ ) and trivalent vanadium ions (V 3+), the vanadium ion concentration is 2.0 mol / L, and the ratio of vanadium ions and sulfuric acid-hydrochloric acid solution in the negative electrode electrolyte is 4:5.
[0037] Vanadium ions are generated by electrolysis of vanadates, the purity of which is 99.9%. Iron ions are generated by electrolysis of iron flakes.
[0038] The sulfuric acid-hydrochloric acid solution contains sulfate and chloride ions, with the sulfate concentration being 2.0 mol / L and the chloride ion concentration being 6.2 mol / L.
[0039] like Figure 1 As shown, a method for preparing a high thermal conductivity energy storage battery material comprises the following steps: Step 1: Put vanadate and iron sheet into an electrolytic cell containing sulfuric acid solution, turn on the power of the electrolytic cell, and during the electrolysis process, the iron sheet undergoes oxidation reaction at the anode to generate Fe 2+ ions, vanadate undergoes oxidation reaction at the anode to generate V 5+ ion; The iron sheet and vanadate undergo a hydrogen ion reduction reaction at the cathode, and the reaction is as follows: 2H + +2e−→H 2 In this reaction, hydrogen ions take electrons from the electrolyte and form hydrogen gas (H 2 ) and released; The vanadium ions in vanadate undergo a reduction reaction at the cathode, and the reaction is as follows: V 5+ +e−→V 4+ In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V 4+ ), forming a cathode electrolyte precursor; Step 2: Put the vanadate into an electrolytic cell containing sulfuric acid solution, turn on the power of the electrolytic cell, and during the electrolysis process, the vanadate undergoes oxidation reaction at the anode to generate V 5+ Ions, vanadate undergoes hydrogen ion reduction reaction at the cathode, and the reaction is as follows: 2H + +2e−→H 2 In this reaction, hydrogen ions take electrons from the electrolyte and form hydrogen gas (H 2 ) and released, the vanadium ions in the vanadate undergo a reduction reaction, the reaction performance is: V 5+ +e−→V 4+ In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V 4+ ), V 4+ The reduction reaction continues to generate V 2+ and V 3+ions, forming a negative electrode electrolyte precursor; Step 3: Filtration: Add the reducing agent containing chloride ions to the positive electrode electrolyte precursor and the negative electrode electrolyte precursor to generate the positive electrode electrolyte and the negative electrode electrolyte.
[0040] The positive electrolyte contains V 5+ 、V 4+ , Fe 2+ ions, sulfate ions and chloride ions, the negative electrode electrolyte contains V 2+ 、V 3+ , sulfate ions and chloride ions.
[0041] The chloride ion concentration is 6.2 mol / L and the sulfate concentration is 2.5 mol / L.
[0042] The prepared electrolyte was sealed in a glass bottle and then placed in a plexiglass rack. The plexiglass rack containing the V(V) electrolyte was placed in a constant temperature water bath at -20°C for 10 days for stability testing.
[0043] The preparation equipment used in this embodiment is all existing equipment on the market.
[0044] Embodiment 2 like Figure 2 As shown, the high thermal conductivity energy storage battery material includes a positive electrode electrolyte and a negative electrode electrolyte. The positive electrode electrolyte is composed of a sulfuric acid-hydrochloric acid solution containing vanadium ions and iron ions. The vanadium ions are tetravalent vanadium ions (V 4+ ) and pentavalent vanadium ions (V 5+ ), the vanadium ion concentration is 1.6mol / L, the iron ion concentration is 0.4mol / L, the ratio of vanadium ions, iron ions and sulfuric acid-hydrochloric acid solution in the positive electrolyte is 4:1:5, and the negative electrolyte is composed of sulfuric acid-hydrochloric acid solution containing vanadium and vanadium ions, and the vanadium ions are divalent vanadium ions (V 2+ ) and trivalent vanadium ions (V 3+ ), the vanadium ion concentration is 2.4 mol / L, and the ratio of vanadium ions and sulfuric acid-hydrochloric acid solution in the negative electrode electrolyte is 4:5.
[0045] Vanadium ions are generated by electrolysis of vanadates, the purity of which is 99.9%. Iron ions are generated by electrolysis of iron flakes.
[0046] The sulfuric acid-hydrochloric acid solution contains sulfate and chloride ions, with the sulfate concentration being 2.4 mol / L and the chloride ion concentration being 6.4 mol / L.
[0047] like Figure 1 As shown, a method for preparing a high thermal conductivity energy storage battery material comprises the following steps: Step 1: Put vanadate and iron sheet into an electrolytic cell containing sulfuric acid solution, turn on the power of the electrolytic cell, and during the electrolysis process, the iron sheet undergoes oxidation reaction at the anode to generate Fe 2+ ions, vanadate undergoes oxidation reaction at the anode to generate V 5+ ion; The iron sheet and vanadate undergo a hydrogen ion reduction reaction at the cathode, and the reaction is as follows: 2H + +2e−→H 2 In this reaction, hydrogen ions take electrons from the electrolyte and form hydrogen gas (H 2 ) and released; The vanadium ions in vanadate undergo a reduction reaction at the cathode, and the reaction is as follows: V 5+ +e−→V 4+ In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V 4+ ), forming a cathode electrolyte precursor; Step 2: Put the vanadate into an electrolytic cell containing sulfuric acid solution, turn on the power of the electrolytic cell, and during the electrolysis process, the vanadate undergoes oxidation reaction at the anode to generate V 5+ Ions, vanadate undergoes hydrogen ion reduction reaction at the cathode, and the reaction is as follows: 2H + +2e−→H 2 In this reaction, hydrogen ions take electrons from the electrolyte and form hydrogen gas (H 2 ) and released, the vanadium ions in the vanadate undergo a reduction reaction, the reaction performance is: V 5+ +e−→V 4+ In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V 4+ ), V 4+ The reduction reaction continues to generate V 2+ and V 3+ ions, forming a negative electrode electrolyte precursor; Step 3: Filtration: Add the reducing agent containing chloride ions to the positive electrode electrolyte precursor and the negative electrode electrolyte precursor to generate the positive electrode electrolyte and the negative electrode electrolyte.
[0048] The positive electrolyte contains V 5+ 、V 4+ , Fe 2+ ions, sulfate ions and chloride ions, the negative electrode electrolyte contains V 2+ 、V 3+ , sulfate ions and chloride ions.
[0049] The chloride ion concentration is 6.2 mol / L and the sulfate concentration is 2.5 mol / L.
[0050] The prepared electrolyte was sealed in a glass bottle and then placed in a plexiglass rack. The plexiglass rack containing the V(V) electrolyte was placed in a constant temperature water bath at 0°C for 10 days for stability testing.
[0051] The preparation equipment used in the preparation method of the high thermal conductivity energy storage battery material in this embodiment is the same as the equipment in the first embodiment, and the difference lies in the different static environment temperature.
[0052] like Figure 3-8 As shown, a liquid flow battery structure includes a positive electrode storage tank 101, a negative electrode storage tank 102, a first circulation pump 301, a second circulation pump 302 and two end plates 201, a battery stack 202 is fixed between the two end plates 201, a positive electrode storage tank 101 is filled with a positive electrode electrolyte, and a negative electrode storage tank 102 is filled with a negative electrode electrolyte. The electrolyte adopts a high thermal conductivity energy storage battery material, or the electrolyte adopts a positive electrode electrolyte and a negative electrode electrolyte prepared by a preparation method of a high thermal conductivity energy storage material in this embodiment. In this embodiment, during the charging process, an external power supply provides electrical energy through the positive and negative electrodes of the battery, and V in the positive electrode electrolyte 4+ The ion loses electrons and is oxidized to V 5+ ions, Fe in the positive electrolyte 2+ The ion loses electrons and is oxidized to ferric iron (Fe 3+ ), during the discharge process, the chemical energy inside the battery is converted into electrical energy and released, and the vanadium-iron ions are stably converted into ions within a wider temperature range.
[0053] A heat dissipation hole 4 is provided on the side of the end plate 201 away from the battery stack 202, and a dustproof net 5 is fixed in the heat dissipation hole 4. An angle steel 14 is fixed to the front end of the end plate 201, and a first motor 15 is fixed on the angle steel 14. A rotating plate 6 is fixed to the output end of the first motor 15, and a rotating cover 7 is fixed to the lower end of the rotating plate 6. The specifications of the rotating cover 7 are adapted to the heat dissipation hole 4. A second motor 9 is fixed to the front end of the rotating cover 7, and a rotating shaft 10 is fixed to the output end of the second motor 9, and a heat dissipation fan blade 11 is fixed on the rotating shaft 10. In this embodiment, the first motor 15 and the second motor 9 are both prior arts and will not be described in detail hereinafter. In a high temperature environment, the first motor 15 is operated, the first motor 15 drives the rotating plate 6 to rotate, and the rotating cover 7 rotates with the rotating plate 6 to expose the heat dissipation hole 4, so as to dissipate the temperature in the battery stack 202. The second motor 9 is operated to drive the rotating shaft 10 to rotate, and the heat dissipation fan blade 11 rotates with the rotating shaft 10, so as to accelerate the air circulation around the heat dissipation hole 4 and enhance the heat dissipation.
[0054] A first sealing ring 12 is fixed in the heat dissipation hole 4, and a second sealing ring 13 is fixed at the rear end of the rotating cover 7. The outer wall of the second sealing ring 13 contacts the inner wall of the first sealing ring 12. In this embodiment, under a low temperature environment, the first motor 15 is operated to drive the rotating plate 6 to rotate, and the rotating cover 7 approaches the end plate 201 along with the rotating plate 7. The second sealing ring 13 contacts the first sealing ring 12 along with the rotating cover 7 until a tight ring sleeve is formed, thereby reducing air circulation at the battery stack 202 and allowing the temperature accumulation generated during its own operation to adapt to the low temperature environment.
[0055] A connecting piece 8 is integrally formed at the front end of the end plate 201, and the output end of the first motor 15 is passed through the connecting piece 8 on the left and right sides. The connecting piece 8 is rotatably connected to the rotating plate 6. In this embodiment, the connecting piece 8 is used to support the output shaft of the first motor 15 to improve the rotation stability of the rotating cover 7.
[0056] Embodiment 3 like Figure 2 As shown, the high thermal conductivity energy storage battery material includes a positive electrode electrolyte and a negative electrode electrolyte. The positive electrode electrolyte is composed of a sulfuric acid-hydrochloric acid solution containing vanadium ions and iron ions. The vanadium ions are tetravalent vanadium ions (V 4+ ) and pentavalent vanadium ions (V 5+ ), the vanadium ion concentration is 2.2mol / L, the iron ion concentration is 0.5mol / L, the ratio of vanadium ions, iron ions and sulfuric acid-hydrochloric acid solution in the positive electrolyte is 4:1:5, and the negative electrolyte is composed of sulfuric acid-hydrochloric acid solution containing vanadium and vanadium ions, and the vanadium ions are divalent vanadium ions (V 2+ ) and trivalent vanadium ions (V 3+ ), the vanadium ion concentration is 2.3 mol / L, and the ratio of vanadium ions and sulfuric acid-hydrochloric acid solution in the negative electrode electrolyte is 4:5.
[0057] Vanadium ions are generated by electrolysis of vanadates, the purity of which is 99.9%. Iron ions are generated by electrolysis of iron flakes.
[0058] The sulfuric acid-hydrochloric acid solution contains sulfate and chloride ions, with the sulfate concentration being 3.0 mol / L and the chloride ion concentration being 6.6 mol / L.
[0059] like Figure 1 As shown, a method for preparing a high thermal conductivity energy storage battery material comprises the following steps: Step 1: Put vanadate and iron sheet into an electrolytic cell containing sulfuric acid solution, turn on the power of the electrolytic cell, and during the electrolysis process, the iron sheet undergoes oxidation reaction at the anode to generate Fe 2+ ions, vanadate undergoes oxidation reaction at the anode to generate V 5+ ion; The iron sheet and vanadate undergo a hydrogen ion reduction reaction at the cathode, and the reaction is as follows: 2H + +2e−→H2 In this reaction, hydrogen ions take electrons from the electrolyte and form hydrogen gas (H 2 ) and released; The vanadium ions in vanadate undergo a reduction reaction at the cathode, and the reaction is as follows: V 5+ +e−→V 4+ In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V 4+ ), forming a cathode electrolyte precursor; Step 2: Put the vanadate into an electrolytic cell containing sulfuric acid solution, turn on the power of the electrolytic cell, and during the electrolysis process, the vanadate undergoes oxidation reaction at the anode to generate V 5+ Ions, vanadate undergoes hydrogen ion reduction reaction at the cathode, and the reaction is as follows: 2H + +2e−→H 2 In this reaction, hydrogen ions take electrons from the electrolyte and form hydrogen gas (H 2 ) and released, the vanadium ions in the vanadate undergo a reduction reaction, the reaction performance is: V 5+ +e−→V 4+ In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V 4+ ), V 4+ The reduction reaction continues to generate V 2+ and V 3+ ions, forming a negative electrode electrolyte precursor; Step 3: Filtration: Add the reducing agent containing chloride ions to the positive electrode electrolyte precursor and the negative electrode electrolyte precursor to generate the positive electrode electrolyte and the negative electrode electrolyte.
[0060] The positive electrolyte contains V 5+ 、V 4+ , Fe 2+ ions, sulfate ions and chloride ions, the negative electrode electrolyte contains V 2+ 、V 3+ , sulfate ions and chloride ions.
[0061] The chloride ion concentration is 6.2 mol / L and the sulfate concentration is 2.5 mol / L.
[0062] The prepared electrolyte was sealed in a glass bottle and then placed in a plexiglass rack. The plexiglass rack containing the V(V) electrolyte was placed in a constant temperature water bath at 20°C for 10 days for stability testing.
[0063] The preparation equipment used in the preparation method of the high thermal conductivity energy storage battery material in this embodiment is the same as the equipment in the first embodiment, and the difference lies in the different static environment temperature.
[0064] Embodiment 4 like Figure 2 As shown, the high thermal conductivity energy storage battery material includes a positive electrode electrolyte and a negative electrode electrolyte. The positive electrode electrolyte is composed of a sulfuric acid-hydrochloric acid solution containing vanadium ions and iron ions. The vanadium ions are tetravalent vanadium ions (V 4+ ) and pentavalent vanadium ions (V 5+ ), the vanadium ion concentration is 2.4mol / L, the iron ion concentration is 0.6mol / L, the ratio of vanadium ions, iron ions and sulfuric acid-hydrochloric acid solution in the positive electrolyte is 4:1:5, and the negative electrolyte is composed of sulfuric acid-hydrochloric acid solution containing vanadium and vanadium ions, and the vanadium ions are divalent vanadium ions (V 2+ ) and trivalent vanadium ions (V 3+ ), the vanadium ion concentration is 2.8 mol / L, and the ratio of vanadium ions and sulfuric acid-hydrochloric acid solution in the negative electrode electrolyte is 4:5.
[0065] Vanadium ions are generated by electrolysis of vanadates, the purity of which is 99.9%. Iron ions are generated by electrolysis of iron flakes.
[0066] The sulfuric acid-hydrochloric acid solution contains sulfate and chloride ions, with the sulfate concentration being 3.2 mol / L and the chloride ion concentration being 6.8 mol / L.
[0067] like Figure 1 As shown, a method for preparing a high thermal conductivity energy storage battery material comprises the following steps: Step 1: Put vanadate and iron sheet into an electrolytic cell containing sulfuric acid solution, turn on the power of the electrolytic cell, and during the electrolysis process, the iron sheet undergoes oxidation reaction at the anode to generate Fe 2+ ions, vanadate undergoes oxidation reaction at the anode to generate V 5+ ion; The iron sheet and vanadate undergo a hydrogen ion reduction reaction at the cathode, and the reaction is as follows: 2H + +2e−→H 2 In this reaction, hydrogen ions take electrons from the electrolyte and form hydrogen gas (H 2 ) and released; The vanadium ions in vanadate undergo a reduction reaction at the cathode, and the reaction is as follows: V 5+ +e−→V 4+ In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V 4+ ), forming a cathode electrolyte precursor; Step 2: Put the vanadate into an electrolytic cell containing sulfuric acid solution, turn on the power of the electrolytic cell, and during the electrolysis process, the vanadate undergoes oxidation reaction at the anode to generate V 5+ Ions, vanadate undergoes hydrogen ion reduction reaction at the cathode, and the reaction is as follows: 2H + +2e−→H 2 In this reaction, hydrogen ions take electrons from the electrolyte and form hydrogen gas (H 2 ) and released, the vanadium ions in the vanadate undergo a reduction reaction, the reaction performance is: V 5+ +e−→V 4+ In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V 4+ ), V 4+ The reduction reaction continues to generate V 2+ and V 3+ ions, forming a negative electrode electrolyte precursor; Step 3: Filtration: Add the reducing agent containing chloride ions to the positive electrode electrolyte precursor and the negative electrode electrolyte precursor to generate the positive electrode electrolyte and the negative electrode electrolyte.
[0068] The positive electrolyte contains V 5+ 、V 4+ , Fe 2+ ions, sulfate ions and chloride ions, the negative electrode electrolyte contains V 2+ 、V 3+ , sulfate ions and chloride ions.
[0069] The chloride ion concentration is 6.2 mol / L and the sulfate concentration is 2.5 mol / L.
[0070] The prepared electrolyte was sealed in a glass bottle and then placed in a plexiglass rack. The plexiglass rack containing the V(V) electrolyte was placed in a constant temperature water bath at 50°C for 10 days for stability testing.
[0071] The preparation equipment used in the preparation method of the high thermal conductivity energy storage battery material in this embodiment is the same as the equipment in the first embodiment, and the difference lies in the different static environment temperature.
[0072] Experimental example The electrolyte prepared in Example 1-4 was taken after standing for ten days, and the electrolyte prepared by the existing battery material preparation method was taken after standing for ten days at different temperatures, and its energy efficiency and capacity loss were tested. The measured results are as follows:
[0073] In summary, the electrolyte prepared by using the iron-vanadium electrolyte of the present invention with a chloride ion concentration of 6.2 mol / L and a sulfate concentration of 2.5 mol / L has better energy efficiency and capacity loss than the all-vanadium electrolyte in the prior art over a wider temperature range.
[0074] Embodiments 1, 2 and 4 are significantly better than the existing examples in terms of energy efficiency and capacitance loss, indicating that the electrolyte of the present invention is applicable to a wider temperature range.
[0075] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. A high thermal conductivity energy storage battery material, comprising a positive electrode electrolyte and a negative electrode electrolyte, It is characterized in that The positive electrode electrolyte is composed of a sulfuric acid-hydrochloric acid solution containing vanadium ions and iron ions, wherein the vanadium ions are tetravalent vanadium ions (V 4+ ) and pentavalent vanadium ions (V 5+ ), the vanadium ion concentration is 1.2-2.4 mol / L, the iron ion concentration is 0.3-0.6 mol / L, the positive electrode electrolyte contains vanadium ions, 6-10 parts of iron ions and sulfuric acid-hydrochloric acid solution in a ratio of 4:1:5, and the negative electrode electrolyte is composed of a sulfuric acid-hydrochloric acid solution containing vanadium and vanadium ions, and the vanadium ions are divalent vanadium ions (V 2+ ) and trivalent vanadium ions (V 3+ ), the vanadium ion concentration is 2.0-2.8 mol / L, and the ratio of vanadium ions and sulfuric acid-hydrochloric acid solution in the negative electrode electrolyte is 4:
5.
2. A high thermal conductivity energy storage battery material according to claim 1, It is characterized in that The vanadium ions are generated by electrolysis of vanadate, the purity of vanadate is 99.9%, and the iron ions are generated by electrolysis of iron sheets.
3. A high thermal conductivity energy storage battery material according to claim 1, It is characterized in that The sulfuric acid-hydrochloric acid solution contains sulfate and chloride ions, wherein the concentration of sulfate is 2.0-3.2 mol / L and the concentration of chloride ions is 6.2-6.8 mol / L.
4. A method for preparing a high thermal conductivity energy storage battery material according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Step 1: Put the vanadate and iron sheet into an electrolytic cell, which contains a sulfuric acid solution, and turn on the power of the electrolytic cell. During the electrolysis process, the iron sheet undergoes an oxidation reaction at the anode to generate Fe 2+ ions, vanadate undergoes oxidation reaction at the anode to generate V 5+ ion; The iron sheet and vanadate undergo a hydrogen ion reduction reaction at the cathode, and the reaction is as follows: 2H + +2e−→H 2 In this reaction, hydrogen ions take electrons from the electrolyte and form hydrogen gas (H 2 ) and released; The vanadium ions in the vanadate undergo a reduction reaction at the cathode, and the reaction is as follows: V 5+ +e−→V 4+ In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V 4+ ), forming a cathode electrolyte precursor; Step 2: placing the vanadate in an electrolytic cell containing a sulfuric acid solution, turning on the power supply of the electrolytic cell, and during the electrolysis process, the vanadate undergoes an oxidation reaction at the anode to generate V 5+ Ions, vanadate undergoes hydrogen ion reduction reaction at the cathode, and the reaction is as follows: 2H + +2e−→H 2 In this reaction, hydrogen ions take electrons from the electrolyte and form hydrogen gas (H 2 ) and released, the vanadium ions in the vanadate undergo a reduction reaction, the reaction performance is: V 5+ +e−→V 4+ In this reaction, the pentavalent vanadium ion obtains an electron from the electrolyte and is reduced to a tetravalent vanadium ion (V 4+ ), V4+ continues to undergo reduction reaction to generate V 2+ and V 3+ ions, forming a negative electrode electrolyte precursor; Step 3: Filtration: Add a reducing agent containing chloride ions to the positive electrode electrolyte precursor and the negative electrode electrolyte precursor to generate a positive electrode electrolyte and a negative electrode electrolyte.
5. A method for preparing a high thermal conductivity energy storage battery material according to claim 4, It is characterized in that The positive electrode electrolyte comprises V 5+ 、V 4+ , Fe 2+ ions, sulfate ions and chloride ions, the negative electrode electrolyte contains V 2+ 、V 3+ , sulfate ions and chloride ions.
6. A method for preparing a high thermal conductivity energy storage battery material according to claim 5, It is characterized in that The chloride ion concentration is 6.2 mol / L, and the sulfate concentration is 2.5 mol / L.
7. A liquid flow battery structure, comprising a positive electrode storage tank (101), a negative electrode storage tank (102), a first circulation pump (301), a second circulation pump (302) and two end plates (201), a battery stack (202) being fixed between the two end plates (201), a positive electrode storage tank (101) containing a positive electrode electrolyte, a negative electrode storage tank (102) containing a negative electrode electrolyte, It is characterized in that The electrolyte is a positive electrode electrolyte and a negative electrode electrolyte prepared by the preparation method according to any one of claims 4 to 6.
8. The liquid flow battery structure according to claim 7, It is characterized in that A heat dissipation hole (4) is provided on a side of the end plate (201) away from the battery stack (202), a dust screen (5) is fixed in the heat dissipation hole (4), an angle steel (14) is fixed at the front end of the end plate (201), a first motor (15) is fixed on the angle steel (14), a rotating plate (6) is fixed at the output end of the first motor (15), a rotating cover (7) is fixed at the lower end of the rotating plate (6), the specification of the rotating cover (7) is compatible with the heat dissipation hole (4), a second motor (9) is fixed at the front end of the rotating cover (7), a rotating shaft (10) is fixed at the output end of the second motor (9), and a heat dissipation fan blade (11) is fixed on the rotating shaft (10).
9. The liquid flow battery structure according to claim 8, It is characterized in that A first sealing ring (12) is fixed inside the heat dissipation hole (4), a second sealing ring (13) is fixed at the rear end of the rotating cover (7), and an outer wall of the second sealing ring (13) contacts an inner wall of the first sealing ring (12).
10. The liquid flow battery structure according to claim 8, It is characterized in that A connecting piece (8) is integrally formed at the front end of the end plate (201), and the output ends of the first motor (15) are passed through the connecting piece (8) on the left and right sides, and the connecting piece (8) is rotatably connected to the rotating plate (6).
Citation Information
Patent Citations
Electrolyte for all-vanadium redox flow battery and preparation method thereof, and all-vanadium redox flow battery including the electrolyte
CN101572319A