Flame-retardant polymer gel electrolyte composition and preparation method thereof

The safety hazards of liquid electrolytes in lithium batteries are solved by using phosphate flame retardant, polyvinylidene fluoride or vinylidene fluoride polymer and ionic conductor active metal salts. The solid-liquid interface impedance problem achieves a solid-state battery with high safety and high performance.

CN118943480APending Publication Date: 2024-11-12HEBEI UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411293654.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The liquid electrolytes in existing lithium batteries have safety hazards of liquid leakage, volatility, combustion and even explosion during use. The poor solid-liquid interface contact of all solid-state batteries leads to a large interface impedance, affecting battery performance.

Method used

The electrolyte is prepared by a spinning liquid preparation and assembly method using a flame retardant polymer gel electrolyte composition including a phosphate flame retardant, polyvinylidene fluoride or vinylidene fluoride polymer and an ionic conductor active metal salt. , used to modify the interface of solid-state batteries.

Benefits of technology

This electrolyte has excellent electrochemical stability and flame retardant properties, which reduces the interface impedance of solid-state batteries, improves safety, and does not require polymerization and curing of external initiators, avoids the negative impact on cycle life. It is suitable for a variety of secondary batteries. system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943480A_ABST
    Figure CN118943480A_ABST
Patent Text Reader

Abstract

The invention discloses a flame-retardant polymer gel electrolyte composition and a preparation method thereof. The composition comprises a phosphate flame retardant, polyvinylidene fluoride and / or a vinylidene fluoride-based polymer and an ionic conductor active metal salt. The flame-retardant gel electrolyte disclosed by the invention is simple in proportioning, has no adverse effect on the cycle life of a solid-state battery, has excellent electrochemical stability and good flame-retardant property, and can be used for interface modification of a solid-state electrolyte and an electrode, so that the interface impedance of the solid-state battery can be reduced, the safety of the solid-state battery can be effectively improved, and the service life of the solid-state battery can be prolonged. And the method has wide applicability, not only can be used as interface modification of a solid electrolyte and an electrode, but also can be independently used as a gel electrolyte, and can be used for manufacturing a high-energy-density and high-safety solid-state battery. And the preparation method is simple and adjustable, can meet the production requirements of the existing process, and has the advantage of easiness in large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a flame retardant polymer gel electrolyte composition and a preparation method thereof. Background Art

[0002] In recent years, with the development of economy and the improvement of living standards, people's demand for energy has been increasing. Lithium batteries have been favored by people because of their advantages such as safety, environmental protection, high specific energy and good electrochemical performance. The lithium batteries currently used use liquid electrolytes, which may leak, volatilize, burn or even explode during use, causing great safety hazards. In order to ensure the safety and stability of the battery during use, the development direction of lithium battery electrolytes has gradually shifted to gel and solid states. All-solid-state batteries can well solve the safety performance of batteries, but compared with conventional solid-liquid interfaces, their interface contact is poor, which will greatly increase the interface impedance between the electrode and the solid electrolyte, and its room temperature ionic conductivity is low, which greatly affects the performance of the battery. In contrast, gel electrolytes reduce free solvents, reduce the risk of electrolyte leakage and the possibility of combustion and explosion, and improve the safety performance of batteries. At present, the flame retardant performance of electrolytes is mainly improved by adding flame retardant additives to the electrolytes. The addition of flame retardant additives changes the organic electrode liquid from flammable to non-flammable or even flame retardant, thereby enhancing the safety performance and stability of the electrolyte and reducing the risk of combustion or explosion of the electrolyte during use. However, the addition of flame retardant additives also reduces the ionic conductivity of the electrolyte, thereby affecting the capacity of the battery and having an adverse effect on the cycle life of the battery. Summary of the invention

[0003] In view of this, the present invention provides a flame retardant polymer gel electrolyte composition and a preparation method thereof.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] A flame retardant polymer gel electrolyte composition comprises a phosphate flame retardant, polyvinylidene fluoride and / or a vinylidene fluoride-based polymer and an ion conductor active metal salt.

[0006] Preferably, the phosphate flame retardant includes at least one of trimethyl phosphate, triethyl phosphate, tributyl phosphate and triphenyl phosphate.

[0007] Preferably, the vinylidene fluoride-based polymer includes at least one of polyvinylidene fluoride-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer and fluorinated ethylene propylene copolymer.

[0008] Preferably, the content of the polyvinylidene fluoride and / or the polyvinylidene fluoride-based polymer is 10-30 wt.%.

[0009] Preferably, the ion conductor active metal salt includes lithium salt, sodium salt or magnesium salt.

[0010] Preferably, the lithium salt comprises lithium hexafluorophosphate.

[0011] Preferably, the concentration of the ion conductor active metal salt is 0.8-1.5M.

[0012] A method for preparing a flame retardant polymer gel electrolyte composition comprises the following steps:

[0013] Step 1: Prepare the core layer spinning solution:

[0014] Dissolve the phosphate ester in a mixed solvent of DMF and acetone to make the spinning solution concentration 10wt%;

[0015] Step 2: Prepare shell spinning solution:

[0016] PAN and PVDF-HFP were dissolved in a mixed solvent of DMF and acetone to make the spinning solution concentration 11wt%;

[0017] Step 3:

[0018] Inject the core layer and shell layer spinning solution into the syringe, the spinning speed is: core layer 0.3ml / h, shell layer 1.2ml / h; spinning voltage is 12-15KV; spinning time is 3.5-4h;

[0019] Step 4:

[0020] Dry, cut into 19 mm discs, and soak in 1M lithium hexafluorophosphate electrolyte; then assemble the battery and test it.

[0021] Preferably, the phosphates are dissolved in a mixed solvent of DMF and acetone in a volume ratio of 7:3; PAN and PVDF-HFP are dissolved in a mixed solvent of DMF and acetone in a mass ratio of 5:5, wherein the volume ratio of the mixed solvent of DMF and acetone is 7:3.

[0022] Preferably, the spinning solution is stirred at 60° C. for 6 hours.

[0023] Preferably, the electrolyte solvent is EC / DEC / DMC=1:1:1vt.

[0024] Compared with the prior art, the present invention has achieved the following technical effects:

[0025] 1. The flame-retardant gel electrolyte of the present invention has a simple ratio, excellent electrochemical stability and good flame retardant properties. The gel electrolyte has the advantages of a wide electrochemical window and a high ion migration number. Using it for interface modification between solid electrolyte and electrode can not only reduce the interface impedance of the solid-state battery, but also effectively improve the safety of the solid-state battery.

[0026] 2. The preparation method of the flame-retardant gel electrolyte of the present invention is simple and adjustable, which can meet the production requirements of the existing process and has the advantage of being easy for large-scale production; at the same time, the flame-retardant gel electrolyte of the present invention does not require an external initiator for polymerization and curing, and will not have an adverse effect on the cycle life of the solid-state battery.

[0027] 3. The flame retardant gel electrolyte of the present invention has a wide range of applicability. By replacing the ion conductor lithium salt, it can meet the use requirements of various secondary battery systems such as solid lithium ion, sodium ion, and magnesium ion batteries. At the same time, the flame retardant gel electrolyte of the present invention can not only be used as a solid electrolyte and an interface modification of an electrode, but can also be used alone as a gel electrolyte, which can realize the manufacture of high energy density and high safety solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a flow chart of a flame retardant polymer gel electrolyte composition and a preparation method thereof. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Embodiment 1:

[0031] The present invention discloses a flame retardant polymer gel electrolyte composition, which comprises a phosphate flame retardant, polyvinylidene fluoride and / or a vinylidene fluoride-based polymer and an ion conductor active metal salt. The phosphate flame retardant has high flame retardancy; the phosphate flame retardant comprises at least one of trimethyl phosphate, triethyl phosphate, tributyl phosphate and triphenyl phosphate.

[0032] Polyvinylidene fluoride and / or vinyl fluoride-based polymers have excellent high-voltage resistance and thermal stability. As a network skeleton or packaging shell of a flame-retardant gel electrolyte, they can provide certain mechanical and electrochemical stability and are precursor substances that cure in situ to form a gel. Vinylidene fluoride-based polymers include at least one of polyvinylidene fluoride-hexafluoropropylene copolymers, ethylene-tetrafluoroethylene copolymers and fluorinated ethylene propylene copolymers.

[0033] The content of polyvinylidene fluoride and / or vinylidene fluoride polymer is 10-30 wt.%.

[0034] The ion conductor active metal salt has the function of transmitting lithium ions; the ion conductor active metal salt includes lithium salt, sodium salt or magnesium salt; the lithium salt includes lithium hexafluorophosphate; the concentration of the ion conductor active metal salt is 0.8-1.5M.

[0035] A method for preparing a flame retardant polymer gel electrolyte composition comprises the following steps:

[0036] Step 1: Prepare the core layer spinning solution:

[0037] Dissolve the phosphate ester in a mixed solvent of DMF and acetone to make the spinning solution concentration 10wt%;

[0038] Step 2: Prepare shell spinning solution:

[0039] PAN and PVDF-HFP were dissolved in a mixed solvent of DMF and acetone to make the spinning solution concentration 11wt%;

[0040] Step 3:

[0041] Inject the core layer and shell layer spinning solution into the syringe, the spinning speed is: core layer 0.3ml / h, shell layer 1.2ml / h; spinning voltage is 12-15KV; spinning time is 3.5-4h;

[0042] Step 4:

[0043] Dry, cut into 19 mm discs, and soak in 1M lithium hexafluorophosphate electrolyte; then assemble the battery and test it.

[0044] The volume ratio of phosphate ester dissolved in DMF and acetone mixed solvent is 7:3; PAN and PVDF-HFP are dissolved in DMF and acetone mixed solvent at a mass ratio of 5:5, wherein the volume ratio of DMF and acetone mixed solvent is 7:3.

[0045] The spinning solutions were stirred at 60 °C for 6 h.

[0046] The electrolyte solvent is EC / DEC / DMC=1:1:1vt.

[0047] Embodiment 2:

[0048] The flame retardant gel electrolyte was prepared according to the following method:

[0049] The electrospinning precursor solution of the polymer shell was prepared by adding 18 wt.% polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) into a mixture of DMAc / acetone (w / w=3:7) as solvent, and then the solution was stirred at room temperature for 6 h and then ultrasonicated for 30 min.

[0050] A precursor solution for the core was prepared by using a mixture of DMAc / acetone (w / w=3:7) as solvent and adding triphenyl phosphate (TPP) (the mass percentage can be as high as 60 wt % or more).

[0051] The prepared solutions were electrospun using a double-nozzle coaxial needle, and the flow rates of the core and shell solutions were 1.08 mL h -1 and 0.54 mL h -1 , the distance from the needle to the collector is about 15 cm, the drum speed is about 150 r / min, and the voltage is 15 kV.

[0052] Comparative Example 1:

[0053] Instead of performing core-shell coaxial double-nozzle electrospinning, the flame retardant is mixed with the polymer in an organic solvent and stirred at room temperature for 6 hours. The spinning conditions are the same as those in Case 1. Compared with the PVDF-HFP membrane without flame retardant, it can achieve an effective flame retardant effect. In this comparative case, most of the flame retardant is attached to the polymer surface and in direct contact with the electrolyte, which will increase the viscosity of the electrolyte, reduce the conductivity, and also have a certain impact on the negative electrode of the battery.

[0054] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, any slight modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A flame retardant polymer gel electrolyte composition, characterized in that: The composition comprises 10 wt % to 20 wt % of a phosphate flame retardant, 80 wt % to 90 wt % of polyvinylidene fluoride and / or a vinylidene fluoride-based polymer and an ion conductor active metal salt.

2. A flame retardant polymer gel electrolyte composition according to claim 1, characterized in that: The phosphate flame retardant includes at least one of trimethyl phosphate, triethyl phosphate, tributyl phosphate and triphenyl phosphate.

3. The flame retardant polymer gel electrolyte composition according to claim 1, characterized in that: The vinylidene fluoride-based polymer includes at least one of a polyvinylidene fluoride-hexafluoropropylene copolymer, an ethylene-tetrafluoroethylene copolymer, and a fluorinated ethylene propylene copolymer.

4. The flame retardant polymer gel electrolyte composition according to claim 1, characterized in that: The ion conductor active metal salt includes a lithium salt, a sodium salt or a magnesium salt.

5. The flame retardant polymer gel electrolyte composition according to claim 4, characterized in that: The lithium salt includes lithium hexafluorophosphate.

6. The flame retardant polymer gel electrolyte composition according to claim 1, characterized in that: The concentration of the ion conductor active metal salt is 0.8-1.5M.

7. A method for preparing a flame retardant polymer gel electrolyte composition, characterized in that: The following steps are involved: Step 1: Prepare the core layer spinning solution: Dissolve the phosphate ester in a mixed solvent of DMF and acetone to make the spinning solution concentration 10wt%; Step 2: Prepare shell spinning solution: PAN and PVDF-HFP were dissolved in a mixed solvent of DMF and acetone to make the spinning solution concentration 11wt%; Step 3: Inject the core layer and shell layer spinning solution into the syringe, the spinning speed is: core layer 0.3ml / h, shell layer 1.2ml / h; spinning voltage is 12-15KV; spinning time is 3.5-4h; Step 4: Dry, cut into 19 mm discs, and soak in 1M lithium hexafluorophosphate electrolyte; then assemble the battery and test it.

8. The method for preparing a flame retardant polymer gel electrolyte composition according to claim 7, characterized in that: The phosphates are dissolved in a DMF and acetone mixed solvent in a volume ratio of 7:3; PAN and PVDF-HFP are dissolved in a DMF and acetone mixed solvent in a mass ratio of 5:5, wherein the volume ratio of the DMF and acetone mixed solvent is 7:

3.

9. The method for preparing a flame retardant polymer gel electrolyte composition according to claim 7, characterized in that: The spinning solutions were stirred at 60° C. for 6 h.

10. The method for preparing a flame retardant polymer gel electrolyte composition according to claim 7, characterized in that: The electrolyte solvent is EC / DEC / DMC=1:1:1vt.

Citation Information

Patent Citations

  • Flame-retardant gel electrolyte as well as preparation method and application thereof

    CN114400373A

  • Fabrication methods of cellulose-based gel polymer electrolyte for a secondary battery

    KR1020130088960A

  • A method and system for registering the owner of music copyright and transacting some or all of the same

    KR1020220161086A