Method for recovering layered positive electrode material through hydrothermal calcination and regenerated layered positive electrode material
Through the combination of hydrothermal calcination and flotation, the problems of high energy consumption and toxic solvent use in the cathode material recycling process of lithium-ion batteries are solved, and efficient and environmentally friendly cathode material regeneration is achieved, which simplifies the operation steps and improves the material Performance and environmental friendliness.
Patent Information
- Application Number
- CN202410995441.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing lithium-ion battery recycling technology has high energy consumption, the use of toxic solvents and complex steps, making it difficult to effectively recycle and regenerate efficient cathode materials, and poses a threat to the environment and health.
The hydrothermal calcination method is used to separate the positive electrode material through specific solution treatment and flotation method, and the regeneration of the positive electrode material is achieved by combining hydrothermal reaction, maintaining the structure and optimizing the lithium supplementation reaction, simplifying the operation steps, reducing energy consumption and chemical use.
It realizes green and environmentally friendly positive electrode material recycling, maintains the structure and performance of the material, reduces costs and secondary waste generation, and improves the economic benefits and environmental friendliness of the process.
Smart Images

Figure CN118943548A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode material recycling, and more specifically, to a method for recycling layered positive electrode materials by hydrothermal calcination and the regenerated layered positive electrode materials obtained by the method. Background Art
[0002] With the increasing demand for batteries in electric vehicles and energy storage devices, commercial lithium-ion batteries have developed rapidly. After several years of explosive growth, they are widely used in various electronic product fields. Since the expected life of lithium-ion batteries is 3-10 years, a large number of lithium-ion batteries are retired, generating a large amount of lithium-ion battery waste. The internal reasons for the performance degradation of lithium-ion batteries mainly include: Li migration leads to vacancies in the structure, causing cations to migrate in the structure and produce irreversible phase changes; the formation of SEI film leads to low initial coulomb efficiency; long-term use of binder expansion causes the positive electrode material to fall off; electrolyte degradation and decomposition, etc. The high and low temperatures of the external environment, external stress extrusion, and shell damage can also make lithium-ion batteries scrapped. These lithium-ion batteries are usually piled up in warehouses, but if they are not handled properly, the heavy metal elements contained in the positive electrode materials will cause great harm to the soil, and the toxic gases produced by the volatilization of the electrolyte will cause great harm to human health. With the continuous rise in the price of raw materials for lithium-ion batteries, the recycling of waste lithium-ion batteries has become the focus of many researchers. Therefore, green and environmentally friendly recycling of waste lithium-ion battery positive electrode materials is of great significance to environmental protection and resource recycling. It is urgent to develop a green, efficient, simple and easy recycling method.
[0003] At present, the commonly used battery recycling methods mainly include: pyrometallurgical recycling, wet recycling and a combination of wet and pyrometallurgical recycling, but wet recycling will use a large amount of acid and alkali solutions, or toxic organic solvents. Pyrometallurgical recycling consumes a lot of energy, and the thermal decomposition of organic matter such as polyvinylidene fluoride (PVDF) during the calcination process will also produce fluorine-containing toxic gases. Moreover, both methods have complicated steps, and the structure of the positive electrode particles must be completely destroyed and then reconstructed again. The direct regeneration method has simple and easy operation steps, which can regenerate waste electrode materials while avoiding high-intensity energy consumption and excessive use of chemicals, which significantly reduces costs and the generation of secondary waste.
[0004] Generally, in the process of direct regeneration, the separation of positive electrode materials mainly involves dissolving or inactivating PVDF. For example, Chinese patent application CN202010005820.5 discloses a hydrothermal lithium replenishment-spray remodeling regeneration method for waste ternary positive electrode materials, which separates the positive electrode material and the current collector by alkaline solution; after separation, it is necessary to calcine at high temperature to obtain activated positive electrode materials before subsequent lithium replenishment and other treatments to achieve the regeneration of positive electrode materials. Its recovery process requires multiple calcinations and multiple solvents, and the processing process is complicated. Summary of the invention
[0005] Based on the above technical problems existing in the prior art, the present invention aims to provide a method for recovering layered positive electrode materials by hydrothermal calcination, wherein the positive electrode materials are stripped by a mixed solution, and in this process, the positive electrode materials can be quickly separated by flotation, and then the positive electrode materials are regenerated by a second treatment with a mixed solution and a hydrothermal reaction. The present invention uses a suitable solution for treatment, and can achieve multiple effects such as stripping of positive electrode materials, maintaining the structure of positive electrode materials, optimizing the lithium replenishment reaction interface, and efficient lithium replenishment through the same mixed solution, which greatly simplifies the operation steps to achieve the purpose of directly regenerating positive electrode materials.
[0006] In order to achieve the above object, the technical solution of the present invention is as follows:
[0007] A method for recovering layered positive electrode materials by hydrothermal calcination comprises the following steps:
[0008] S1. Soak and clean the surface of the positive electrode of the waste battery with an organic solvent;
[0009] S2, placing the cleaned positive electrode sheet into the first solution, ultrasonically treating it, and then placing it in a flotation device, adding a frother, and flotation; after the flotation is completed, filtering and drying to separate the waste positive electrode material;
[0010] S3, adding the waste positive electrode material to the second solution to carry out a hydrothermal reaction; after the reaction is completed, the solid-liquid separation and drying are performed to obtain a precursor material;
[0011] S4, calcining the precursor material to obtain a regenerated positive electrode material;
[0012] The first solution in step S2 and the second solution in step S3 respectively include a lithium-containing compound and an alkali.
[0013] In some embodiments, in the first solution, Li + The molar ratio of Li and OH- is 1:1-3. + The molar concentration of OH- is ≥0.5M, preferably 1-3M; the molar concentration of OH- is ≥2M, preferably 2.5-9M.
[0014] In some embodiments, the second solution contains Li + The molar ratio of Li and OH- is 1-3:1. + The molar concentration of OH- is ≥2M, preferably 2.5-15M; the molar concentration of OH- is ≥1M, preferably 2.5-5M.
[0015] In some embodiments, the OH- concentration of the first solution is greater than the OH- concentration of the second solution, and the Li + Less than the second solution Li + concentration.
[0016] In some embodiments, the lithium-containing compound is at least one of an inorganic lithium salt, an organic lithium salt, and lithium hydroxide; the inorganic lithium salt includes but is not limited to at least one of LiNO3, LiCl, and Li2SO4; the organic lithium salt includes but is not limited to at least one of lithium formate, lithium acetate, lithium propionate, lithium oxalate, lithium salicylate, lithium lactate, and lithium citrate.
[0017] In some embodiments, in step S1, the organic solvent is at least one of dimethyl carbonate and diethyl carbonate.
[0018] In some embodiments, in step S2, in step S2, the solid-to-liquid ratio of the positive electrode plate and the first solution is 1 g: 4 to 15 mL.
[0019] In some embodiments, in step S2, the ultrasonic treatment temperature is 20-45°C.
[0020] In some embodiments, in step S2, the ultrasonic treatment time is 0.5-2 h.
[0021] In some embodiments, in step S2, the ultrasonic power is 50-1000W.
[0022] In some embodiments, in step S2, during the flotation process, the dosage of the frother is 0.5-5 mg / g; the rotation speed is 800-1400 r / min; the slurry pH is maintained between 4.5-11; the slurry mass concentration is 0-10%, and the mass concentration is >0; preferably, the slurry mass concentration is 1-10%.
[0023] In some embodiments, in step S3, the hydrothermal temperature is 120-220°C.
[0024] In some embodiments, in step S3, the hydrothermal time is 2-8 hours.
[0025] In some embodiments, in step S3, the solid-liquid ratio of the waste positive electrode material to the second solution is 1 g: 3 to 12 mL.
[0026] In some embodiments, in step S4, the calcination temperature is 700-850°C.
[0027] In some embodiments, in step S4, the calcination time is 1-5 hours.
[0028] In some embodiments, the positive electrode material is at least one of a nickel-cobalt-manganese ternary positive electrode (NCM), a nickel-cobalt-aluminum ternary positive electrode (NCA), and a lithium-rich manganese-based positive electrode (LMO), preferably NCM, and the molecular formula of the positive electrode material is LiNi x Co y Mn 1-x-yO2, wherein 0<x<1, 0<y<1; more preferably, it is at least one of NCM811, NCM523, NCM622, LiCoO2, and LiNiO2.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The recycling method of the present invention comprises the following steps: after disassembling and separating the waste battery to obtain the positive electrode sheet, firstly, the electrolyte and impurities on the surface of the positive electrode sheet are cleaned with an organic solvent; and then, the electrolyte and impurities on the surface of the positive electrode sheet are added to a first solution composed of a lithium-containing compound and an alkali solution at a specific concentration, wherein the alkali solution attacks the C—F bond in the binder PVDF through hydroxide to generate an unsaturated double bond, so that the PVDF loses the halogen element atomic functional group, reduces its bonding ability, loses its mechanical activity, and is extremely easy to break and degrade; and the addition of the lithium-containing compound can effectively inhibit the Li in the waste positive electrode material from being degraded. + leaching, maintaining the original structure of the waste positive electrode material; after being treated with the first solution, flotation can be carried out to effectively separate the waste positive electrode material, and aluminum hydroxide byproducts can be obtained by optimizing the treatment conditions of the first solution, thereby improving the economic benefits of the process without increasing the process flow and reagent costs; the waste positive electrode material obtained after separation is then added to a mixed solution composed of a lithium-containing compound and an alkali solution, and a hydrothermal reaction is carried out to achieve lithium replenishment of the positive electrode material particle structure, wherein the purpose of adding the alkali solution is to further treat the PVDF remaining on the surface of the positive electrode material particles to effectively replenish the positive electrode material particle structure, and finally calcination is performed to remove the collapsed positive electrode particles, impurities, etc., to achieve in-situ regeneration of the positive electrode material particle structure. In addition, by controlling the relationship between the concentrations of lithium ions and hydroxide ions in the first solution and the second solution, not only can the lithium and hydroxide ions in each solution be fully utilized to focus on realizing the main functions of step one and step three, but also the overall performance and stability of the regenerated material can be further optimized.
[0031] The method of the present invention realizes uniform replenishment of lithium sources in an aqueous medium, and can realize lithium replenishment and regeneration of the particle structure of the positive electrode material at a relatively low temperature through a hydrothermal reaction. In addition to using lithium-containing compounds and alkaline solution, no other organic chemicals are added during the treatment process, and the alkaline solution can be recycled, so the treatment process is green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The XRD diagram of the regenerated NCM811 ternary material obtained in Example 1-2 and Comparative Example 1;
[0033] Figure 2 The first cycle charge and discharge diagram of the regenerated NCM811 ternary material half-cell obtained in Example 1 and Comparative Example 1;
[0034] Figure 3The rate curve of the regenerated NCM811 ternary material half-cell obtained by the method provided in Example 1 and Comparative Example 1;
[0035] Figure 4 This is a long cycle curve of the regenerated NCM811 / / graphite full battery obtained according to the method provided in Example 1 and Comparative Example 1.
[0036] Figure 5 This is the XRD diagram of the aluminum hydroxide separated in Example 1. DETAILED DESCRIPTION
[0037] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0039] Example 1
[0040] A method for recovering layered positive electrode materials by hydrothermal calcination comprises the following steps:
[0041] S1. After the used NCM811 batteries were discharged to below 2V at a current density of 0.1C, they were disassembled and sorted in a fume hood to obtain positive electrode sheets, negative electrode sheets, shells, diaphragms, and tabs;
[0042] S2, soaking the positive electrode sheet in a dimethyl carbonate solution for 2 hours, then washing it with deionized water three times, and drying it in a vacuum drying oven at 80° C. for 6 hours to obtain a pretreated positive electrode sheet;
[0043] S3, the pretreated positive electrode sheet was mixed with a LiOH aqueous solution with a concentration of 3 mol / L, the solid-liquid ratio of the positive electrode sheet to the LiOH solution was 1 g: 6 mL, and ultrasonic treatment was performed at 25°C, the ultrasonic power was 100 W, and the ultrasonic time was 1 h; after ultrasonic treatment, it was poured into a flotation machine, methyl isobutyl methanol was added at an amount of 2 mg / g, the slurry pH was adjusted to 8.5, the slurry mass concentration was 8%, and it was stirred at a speed of 1000 r / min, and flotation was performed for 30 minutes. After the flotation was completed, the solid-liquid separation was performed, and the waste positive electrode material and aluminum hydroxide were separated;
[0044] S4, adding the waste positive electrode material to a mixed solution containing LiNO3 and NaOH (in the mixed solution, the concentration of LiNO3 is 5 mol / L, and the concentration of NaOH is 2 mol / L), the solid-liquid ratio of the waste positive electrode material to the mixed solution is 1 g: 10 mL, and after a hydrothermal reaction at 120°C for 8 hours, the solid-liquid is separated and dried to obtain a precursor material;
[0045] S5. Place the precursor material obtained in step S4 in a tube furnace, heat it to 750° C. at a rate of 3° C. / min, and then keep it warm for 5 hours to obtain a regenerated NCM811 positive electrode material.
[0046] The obtained regenerated NCM811 positive electrode material was subjected to XRD detection, and the detection results were as follows Figure 1 shown.
[0047] The electrochemical performance of the regenerated NCM811 positive electrode material prepared in this example was tested as follows:
[0048] The regenerated NCM811 positive electrode material, conductive carbon and PVDF were ground and mixed evenly in a mass ratio of 8:1:1, stirred into a slurry in an N-methylpyrrolidone (NMP) medium, coated on an aluminum foil, and cut into pieces after drying to assemble a lithium-ion battery.
[0049] The preparation method of the negative electrode material is to mix sodium carboxymethyl cellulose (CMC): conductive carbon agent: graphite in a ratio of 1.5:1.5:7. Specifically, CMC is dissolved in deionized water, and then the mixed powder of graphite and carbon conductive agent is slowly added multiple times, stirred on a magnetic stirrer until evenly dispersed, and then coated on a copper foil, dried at 80°C for 12 hours, and then cut to obtain a negative electrode sheet.
[0050] After testing, such as Figure 2-4 As shown, the regenerated positive electrode material recovered by direct hydrothermal calcination according to the method of the present invention maintains excellent cycle and rate performance, such as Figure 3 , the discharge capacity can reach 120mAh / g at a rate of 10C, showing excellent electrochemical performance; Figure 4 After being assembled into a full battery, the test showed that the capacity retention rate could reach 96.95% after 100 cycles at a rate of 1C (1C = 180 mAh / g) in the voltage range of 2.7-4.2 V.
[0051] Example 2
[0052] A method for recovering layered positive electrode materials by hydrothermal calcination comprises the following steps:
[0053] S1. After the used NCM811 batteries were discharged to below 2V at a current density of 0.1C, they were disassembled and sorted in a fume hood to obtain positive electrode sheets, negative electrode sheets, shells, diaphragms, and tabs;
[0054] S2, soaking the positive electrode sheet in a dimethyl carbonate solution for 2 hours, then washing it three times with deionized water, and drying it in a vacuum drying oven at 80° C. for 6 hours to obtain a pretreated positive electrode sheet;
[0055] S3, adding the pretreated positive electrode sheet to a mixed solution containing LiNO3 and NaOH (in the mixed solution, the concentration of LiNO3 is 1 mol / L, and the concentration of NaOH is 3 mol / L), the solid-liquid ratio of the positive electrode sheet to the mixed solution is 1g:5mL, ultrasonic treatment is performed at 30°C, the ultrasonic power is 100W, and the ultrasonic time is 0.75h; after ultrasonic treatment, pour it into a flotation machine, add methyl isobutyl methanol in an amount of 2mg / g, adjust the slurry pH to 8.5, the slurry mass concentration is 8%, stir at a speed of 1000r / min, and flotation is performed for 30min. After the flotation is completed, the solid-liquid separation is performed, and the waste positive electrode material and aluminum hydroxide are separated;
[0056] S4, adding the waste positive electrode material to a mixed solution containing LiNO3 and NaOH (in the mixed solution, the concentration of LiNO3 is 2 mol / L, and the concentration of NaOH is 2 mol / L), the solid-liquid ratio of the waste positive electrode material to the mixed solution is 1 g: 10 mL, and after a hydrothermal reaction at 120° C. for 8 h, the solid-liquid separation is performed, and the precursor material is obtained;
[0057] S5. Place the precursor material obtained in step S4 in a tube furnace, heat it to 750° C. at a rate of 3° C. / min, and then keep it warm for 5 hours to obtain a regenerated NCM811 positive electrode material.
[0058] The obtained regenerated NCM811 positive electrode material was subjected to XRD detection, and the detection results were as follows Figure 1 shown.
[0059] The electrochemical performance of the regenerated NCM811 positive electrode material prepared in this example was tested as follows:
[0060] The regenerated NCM811 positive electrode material, conductive carbon and PVDF were ground and mixed evenly in a mass ratio of 8:1:1, stirred into a slurry in an NMP medium, coated on an aluminum foil, and cut into pieces after drying to assemble a lithium-ion battery.
[0061] The preparation method of the negative electrode material is to mix CMC: conductive carbon agent: graphite in a ratio of 1.5:1.5:7. Specifically, CMC is dissolved in deionized water, and then the mixed powder of graphite and carbon conductive agent is slowly added multiple times. After stirring on a magnetic stirrer until uniform dispersion, it is coated on a copper foil, dried at 80°C for 12 hours, and then cut to obtain a negative electrode sheet.
[0062] After testing, the regenerated positive electrode material recovered by direct hydrothermal calcination in the embodiment maintains excellent cycle and rate performance. The discharge capacity at a rate of 10C in the half-cell system can reach 125mAh / g, showing excellent electrochemical performance. In the full-cell system, in the voltage range of 2.7-4.2V, after 100 cycles at a rate of 1C, the capacity retention rate can reach 91.01%;
[0063] Example 3
[0064] A method for recovering layered positive electrode materials by hydrothermal calcination comprises the following steps:
[0065] S1. After the waste lithium cobalt oxide battery is discharged to below 2V at a current density of 0.1C, it is disassembled and sorted in a fume hood to obtain positive electrode sheets, negative electrode sheets, shells, diaphragms, and tabs;
[0066] S2, soaking the positive electrode sheet in a dimethyl carbonate solution for 2 hours, then washing it with deionized water three times, and drying it in a vacuum drying oven at 80° C. for 6 hours to obtain a pretreated positive electrode sheet;
[0067] S3, the pretreated positive electrode sheet was mixed with 2 mol / L lithium formate and 5 mol / L NaOH solution, the solid-liquid ratio of the positive electrode sheet to the mixed solution was 1g:10mL, and ultrasonic treatment was performed at 20°C, the ultrasonic power was 800W, and the ultrasonic time was 0.5h; after ultrasonic treatment, it was poured into a flotation machine, methyl isobutyl methanol was added at a dosage of 4mg / g, the slurry pH was adjusted to 11, the slurry mass concentration was 5%, and it was stirred at a speed of 800r / min, and flotation was performed for 30min. After the flotation was completed, the solid-liquid separation was performed, and the waste positive electrode material was separated by drying;
[0068] S4, adding the waste positive electrode material to a mixed solution containing lithium nitrate and NaOH (in the mixed solution, the concentration of lithium nitrate is 4 mol / L, and the concentration of NaOH is 2 mol / L), the solid-liquid ratio of the waste positive electrode material to the mixed solution is 1 g: 8 mL, and after a hydrothermal reaction at 170° C. for 5 h, the solid-liquid separation is performed, and the precursor material is obtained by drying;
[0069] S5. Place the precursor material obtained in step S4 in a tube furnace, heat it to 850° C. at a rate of 5° C. / min, and then keep it warm for 3 hours to obtain a regenerated lithium cobalt oxide positive electrode material.
[0070] The electrochemical performance of the regenerated lithium cobalt oxide positive electrode material prepared in this example was tested as follows:
[0071] The regenerated lithium cobalt oxide positive electrode material, conductive carbon and PVDF were ground and mixed evenly in a mass ratio of 8:1:1, stirred into a slurry in an NMP medium, coated on an aluminum foil, and cut into pieces after drying to assemble a lithium-ion battery.
[0072] The preparation method of the negative electrode material is to mix CMC: conductive carbon agent: graphite in a ratio of 1.5:1.5:7. Specifically, CMC is dissolved in deionized water, and then the mixed powder of graphite and carbon conductive agent is slowly added multiple times. After stirring on a magnetic stirrer until uniform dispersion, it is coated on a copper foil, dried at 80°C for 12 hours, and then cut to obtain a negative electrode sheet.
[0073] After testing, the regenerated positive electrode material recovered by direct hydrothermal calcination in the embodiment maintains excellent cycle and rate performance. The discharge capacity at a rate of 5C in a half-cell system can reach 131mAh / g. In a full-cell system, in the voltage range of 2.7-4.2V, after 100 cycles at a rate of 1C, the capacity retention rate can reach 86.53%;
[0074] Example 4
[0075] A method for recovering layered positive electrode materials by hydrothermal calcination comprises the following steps:
[0076] S1. After the used NCM523 batteries were discharged to below 2V at a current density of 0.1C, they were disassembled and sorted in a fume hood to obtain positive electrode sheets, negative electrode sheets, shells, diaphragms, and tabs;
[0077] S2, soaking the positive electrode sheet in a dimethyl carbonate solution for 2 hours, then washing it three times with deionized water, and drying it in a vacuum drying oven at 80° C. for 6 hours to obtain a pretreated positive electrode sheet;
[0078] S3, the pretreated positive electrode sheet was mixed with 0.5 mol / L lithium sulfate and 2.5 mol / L NaOH solution, the solid-liquid ratio of the positive electrode sheet to the mixed solution was 1g:4mL, and ultrasonic treatment was performed at 45°C, the ultrasonic power was 1000W, and the ultrasonic time was 1.5h; after ultrasonic treatment, it was poured into a flotation machine, methyl isobutyl methanol was added in an amount of 5mg / g, the slurry pH was adjusted to 8.0, the slurry mass concentration was 6%, and it was stirred at a speed of 900r / min, and flotation was performed for 45min. After the flotation was completed, the solid-liquid separation was performed, and the waste positive electrode material and aluminum hydroxide were separated;
[0079] S4, adding the waste positive electrode material to a mixed solution containing Li2SO4 and NaOH (in the mixed solution, the concentration of Li2SO4 is 3 mol / L, and the concentration of NaOH is 2 mol / L), the solid-liquid ratio of the waste positive electrode material to the mixed solution is 1 g: 6 mL, and after a hydrothermal reaction at 150° C. for 3.5 h, the solid-liquid is separated and dried to obtain a precursor material;
[0080] S5. Place the precursor material obtained in step S4 in a tube furnace, heat it to 750° C. at a rate of 3° C. / min, and then keep it warm for 5 hours to obtain a regenerated NCM523 positive electrode material.
[0081] The electrochemical performance test of the regenerated NCM523 positive electrode material prepared in this example is as follows:
[0082] The recycled NCM523 positive electrode material, conductive carbon and PVDF were ground and mixed evenly in a mass ratio of 8:1:1, stirred into a slurry in an NMP medium, coated on an aluminum foil, and cut into pieces after drying to assemble a lithium-ion battery.
[0083] The preparation method of the negative electrode material is to mix CMC: conductive carbon agent: graphite in a ratio of 1.5:1.5:7. Specifically, CMC is dissolved in deionized water, and then the mixed powder of graphite and carbon conductive agent is slowly added multiple times. After stirring on a magnetic stirrer until uniform dispersion, it is coated on a copper foil, dried at 80°C for 12 hours, and then cut to obtain a negative electrode sheet.
[0084] After testing, the regenerated positive electrode material recovered by direct hydrothermal calcination in the embodiment maintains excellent cycle and rate performance. The discharge capacity at a rate of 10C in a half-cell system can reach 105mAh / g. In a full-cell system, in the voltage range of 2.7-4.2V, after 100 cycles at a rate of 1C, the capacity retention rate can reach 82.95%;
[0085] Comparative Example 1
[0086] A method for recovering layered positive electrode materials by hydrothermal calcination comprises the following steps:
[0087] S1. After the used NCM811 batteries were discharged to below 2V at a current density of 0.1C, they were disassembled and sorted in a fume hood to obtain positive electrode sheets, negative electrode sheets, shells, diaphragms, and tabs;
[0088] S2, soaking the positive electrode sheet in a dimethyl carbonate solution for 2 hours, then washing it with deionized water three times, and drying it in a vacuum drying oven at 80° C. for 6 hours to obtain a pretreated positive electrode sheet;
[0089] S3, the pretreated positive electrode sheet was mixed with a NaOH solution with a concentration of 3 mol / L, the solid-liquid ratio was 1 g: 6 mL, and ultrasonic treatment was performed at 25°C, the ultrasonic power was 100 W, and the ultrasonic time was 1 h; after ultrasonic treatment, it was poured into a flotation machine, methyl isobutyl methanol was added at a dosage of 2 mg / g, the slurry pH was adjusted to 8.5, the slurry mass concentration was 8%, and it was stirred at a speed of 1000 r / min, and flotation was performed for 30 min. After the flotation was completed, the solid-liquid separation was performed, and the waste positive electrode material and aluminum hydroxide were separated;
[0090] S4, adding the waste positive electrode material to a mixed solution containing LiNO3 and NaOH (in the mixed solution, the concentration of LiNO3 is 5 mol / L, and the concentration of NaOH is 2 mol / L), the volume ratio of the waste positive electrode material to the mixed solution is 1 g: 10 mL, and after a hydrothermal reaction at 120° C. for 8 h, the solid-liquid separation is performed, and the precursor material is obtained by drying;
[0091] S5. Place the precursor material obtained in step S4 in a tube furnace, heat it to 750° C. at a rate of 3° C. / min, and then keep it warm for 5 hours to obtain a regenerated NCM811 positive electrode material.
[0092] The obtained regenerated NCM811 positive electrode material was subjected to XRD detection, and the detection results were as follows Figure 1 shown.
[0093] The electrochemical performance of the regenerated NCM811 positive electrode material obtained by the method of this comparative example was tested as follows:
[0094] The preparation method of the positive electrode sheet is as follows: grind and mix the regenerated NCM811 positive electrode material, conductive carbon and PVDF in a mass ratio of 8:1:1, stir them into slurry in NMP medium, apply them on aluminum foil, dry them and cut them into pieces to obtain the positive electrode sheet;
[0095] The preparation method of the negative electrode sheet is as follows: CMC: conductive carbon agent: graphite is mixed in a ratio of 1.5:1.5:7, specifically, CMC is dissolved in deionized water, and then the mixed powder of graphite and carbon conductive agent is slowly added multiple times, stirred on a magnetic stirrer until uniformly dispersed, and then coated on a copper foil, dried at 80°C for 12 hours, and then cut to obtain the negative electrode sheet;
[0096] The positive electrode sheet, negative electrode sheet, separator and electrolyte are assembled into a lithium-ion battery according to the conventional method in the art, and then the electrochemical performance test is carried out. The test results are as follows: Figure 2-Figure 4 shown.
[0097] like Figure 2-4 In the voltage range of 2.7-4.2V, after 100 cycles at a rate of 1C, the capacity retention rate can reach 80.97%, and the discharge specific capacity is 54mAh / g at a rate of 10C.
[0098] Depend on Figure 2-4 It can be seen that the electrochemical performance of the regenerated NCM811 positive electrode material obtained in this comparative example is significantly lower than the electrochemical performance of the regenerated NCM811 positive electrode material obtained in Example 1.
[0099] Comparative Example 2
[0100] A method for recovering layered positive electrode materials by hydrothermal calcination comprises the following steps:
[0101] S1. After the used NCM811 batteries were discharged to below 2V at a current density of 0.1C, they were disassembled and sorted in a fume hood to obtain positive electrode sheets, negative electrode sheets, shells, diaphragms, and tabs;
[0102] S2, soaking the positive electrode sheet in a dimethyl carbonate solution for 2 hours, then washing it with deionized water three times, and drying it in a vacuum drying oven at 80° C. for 6 hours to obtain a pretreated positive electrode sheet;
[0103] S3, the pretreated positive electrode sheet was mixed with a LiOH solution with a concentration of 3 mol / L at a solid-liquid ratio of 1 g: 6 mL, and ultrasonic treatment was performed at 25°C, with an ultrasonic power of 100 W and an ultrasonic time of 1 h; after ultrasonic treatment, it was poured into a flotation machine, methyl isobutyl methanol was added at a dosage of 2 mg / g, the slurry pH was adjusted to 8.5, the slurry mass concentration was 8%, and it was stirred at a speed of 1000 r / min, and flotation was performed for 30 min. After flotation, the solid-liquid separation was performed, and the waste positive electrode material and aluminum hydroxide were separated and dried;
[0104] S4, adding the waste positive electrode material to a NaOH solution with a concentration of 2 mol / L, the solid-liquid ratio of the waste positive electrode material to the NaOH solution is 1 g:10 mL, and performing a hydrothermal reaction at 120° C. for 8 h, followed by solid-liquid separation and drying to obtain a precursor material;
[0105] S5. Place the precursor material obtained in step S4 in a tube furnace, heat it to 750° C. at a rate of 3° C. / min, and then keep it warm for 5 hours to obtain a regenerated NCM811 positive electrode material.
[0106] The electrochemical performance of the regenerated NCM811 positive electrode material prepared in this comparative example was tested as follows:
[0107] Preparation of positive electrode sheet: Grind and mix the regenerated NCM811 positive electrode material, conductive carbon and PVDF in a mass ratio of 8:1:1, stir them into slurry in NMP medium, apply them on aluminum foil, dry and cut them into pieces to obtain positive electrode sheet;
[0108] Preparation of negative electrode sheet: CMC was dissolved in deionized water according to the mass ratio of CMC: conductive carbon agent: graphite = 1.5:1.5:7, and then the mixed powder of graphite and carbon conductive agent was slowly added several times, stirred on a magnetic stirrer until uniformly dispersed, and then coated on copper foil, dried at 80°C for 12 hours, and cut to obtain the negative electrode sheet;
[0109] The positive electrode sheet, the negative electrode sheet, the separator and the electrolyte are assembled into a lithium-ion battery according to a conventional method in the art, and then the electrochemical performance is tested.
[0110] After testing, in the voltage range of 2.7-4.2V, after 100 cycles at a rate of 1C, the capacity retention rate can reach 79.89%, and the discharge specific capacity is 45mAh / g at a rate of 10C.
[0111] This indicates that after direct hydrothermal treatment and water washing, there is no lithium hydroxide shell coating the outside of the particles, resulting in a large amount of unrepaired rock salt phase inside the particles after the same calcination time, and the electrical performance of the obtained regenerated positive electrode material is significantly reduced.
[0112] Comparative Example 3
[0113] A method for recovering positive electrode layered materials by hydrothermal calcination comprises the following steps:
[0114] S1. After the used NCM811 batteries were discharged to below 2V at a current density of 0.1C, they were disassembled and sorted in a fume hood to obtain positive electrode sheets, negative electrode sheets, shells, diaphragms, and tabs;
[0115] S2, soaking the positive electrode sheet in a dimethyl carbonate solution for 2 hours, then washing it with deionized water three times, and drying it in a vacuum drying oven at 80° C. for 6 hours to obtain a pretreated positive electrode sheet;
[0116] S3, the pretreated positive electrode sheet was mixed with a LiOH solution with a concentration of 3 mol / L, the solid-liquid ratio of the positive electrode sheet to the LiOH solution was 1 g: 6 mL, and ultrasonic treatment was performed at 25°C, the ultrasonic power was 100 W, and the ultrasonic time was 1 h; after ultrasonic treatment, it was poured into a flotation machine, methyl isobutyl methanol was added at an amount of 2 mg / g, the slurry pH was adjusted to 8.5, the slurry mass concentration was 8%, and it was stirred at a speed of 1000 r / min, and flotation was performed for 30 min. After the flotation was completed, the solid-liquid separation was performed, and the waste positive electrode material and aluminum hydroxide were separated;
[0117] S4, adding the waste positive electrode material to a LiNO3 solution with a concentration of 5 mol / L, the solid-liquid ratio of the waste positive electrode material to the LiNO3 solution is 1 g: 10 mL, and performing a hydrothermal reaction at 120°C for 8 hours, followed by solid-liquid separation and drying to obtain a precursor material;
[0118] S5. Place the precursor material obtained in step S4 in a tube furnace, heat it to 750°C at a rate of 3°C / min, and then keep it warm for 5 hours to obtain a regenerated NCM811 positive electrode material. The electrochemical performance of the regenerated NCM811 positive electrode material prepared in this comparative example is tested as follows:
[0119] Preparation of positive electrode sheet: Grind and mix the regenerated NCM811 positive electrode material, conductive carbon and PVDF in a mass ratio of 8:1:1, stir them into slurry in NMP medium, apply them on aluminum foil, dry and cut them into pieces to obtain positive electrode sheets;
[0120] Preparation of negative electrode sheet: CMC was dissolved in deionized water according to the mass ratio of CMC: conductive carbon agent: graphite = 1.5:1.5:7, and then the mixed powder of graphite and carbon conductive agent was slowly added several times, stirred on a magnetic stirrer until uniformly dispersed, and then coated on copper foil, dried at 80°C for 12 hours, and cut to obtain the negative electrode sheet;
[0121] The positive electrode sheet, the negative electrode sheet, the separator and the electrolyte are assembled into a lithium-ion battery according to a conventional method in the art, and then the electrochemical performance is tested.
[0122] After testing, in the voltage range of 2.7-4.2V, after 100 cycles at a rate of 1C, the capacity retention rate can reach 83.89%, and the discharge specific capacity at a rate of 10C is 97mAh / g.
[0123] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0124] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for recovering layered positive electrode materials by hydrothermal calcination, It is characterized in that The following steps are involved: S1. Soak and clean the surface of the positive electrode of the waste battery with an organic solvent; S2, placing the cleaned positive electrode sheet into the first solution, ultrasonically treating it, and then placing it in a flotation device, adding a frother, and flotation; after the flotation is completed, filtering and drying to separate the waste positive electrode material; S3, adding the waste positive electrode material to the second solution to carry out a hydrothermal reaction; after the reaction is completed, the solid-liquid separation and drying are performed to obtain a precursor material; S4, calcining the precursor material to obtain a regenerated positive electrode material; The first solution in step S2 and the second solution in step S3 respectively include a lithium-containing compound and an alkali.
2. The method for recovering layered positive electrode materials by hydrothermal calcination according to claim 1, It is characterized in that In the first solution, Li + and OH - The molar ratio is 1:1-3, Li + The molar concentration of OH- is ≥0.5M and the molar concentration of OH- is ≥2M.
3. The method for recovering layered positive electrode materials by hydrothermal calcination according to claim 2, It is characterized in that Li in the second solution + The molar ratio of Li and OH- is 1-3:
1. + The molar concentration of OH- is ≥2M, and the molar concentration of OH- is ≥1M.
4. The method for recovering layered positive electrode materials by hydrothermal calcination according to claim 3, It is characterized in that OH of the first solution - The concentration is greater than that of the second solution - Concentration, Li of the first solution + Less than the second solution Li + concentration.
5. The method for recovering layered positive electrode materials by hydrothermal calcination according to claim 1, It is characterized in that The lithium-containing compounds selected in the first solution and the second solution are each independently at least one of an inorganic lithium salt, an organic lithium salt, and lithium hydroxide, and the bases include at least one of LiOH, NaOH, and KOH.
6. The method for recovering layered positive electrode materials by hydrothermal calcination according to claim 5, It is characterized in that The inorganic lithium salt includes LiNO 3 、LiCl、Li 2 SO 4 At least one of the organic lithium salts; the organic lithium salt comprises at least one of lithium formate, lithium acetate, lithium propionate, lithium oxalate, lithium salicylate, lithium lactate, and lithium citrate.
7. The method for recovering layered positive electrode materials by hydrothermal calcination according to claim 1, It is characterized in that In step S1, the organic solvent is at least one of dimethyl carbonate and diethyl carbonate; and / or in step S3, the solid-liquid ratio of the waste positive electrode material to the second solution is 1g:3-12mL; and / or the hydrothermal temperature is 120-220°C; and / or the hydrothermal time is 0.5-8h.
8. The method for recovering layered positive electrode materials by hydrothermal calcination according to claim 1, It is characterized in that In step S4, the calcination temperature is 700-850° C.; and / or the calcination time is 1-10 h.
9. The method for recovering layered positive electrode materials by hydrothermal calcination according to claim 1, It is characterized in that In step S2, the solid-liquid ratio of the positive electrode sheet and the first solution is 1g:4-15mL, and / or the ultrasonic treatment temperature is 20-45°C; and / or the treatment time is 0.5-2h; and / or the ultrasonic power is 50-1000W; and / or, during the flotation process, the amount of the frother is 0.5-5mg / g; the rotation speed is 800-1400r / min; the slurry pH is maintained between 4.5-11; the slurry mass concentration is 0-10% and not 0.
10. A regenerated layered cathode material, It is characterized in that The material is prepared by the method for recovering layered positive electrode materials by hydrothermal calcination as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Method for repair and regeneration of waste lithium iron phosphate battery cathode material
CN102208707A
Dry repairing method for positive electrode active material of failed lithium ion battery and material obtained through repairing
CN110838601A
Lithium battery anode recycled material dry purification separation and regeneration method and obtained lithium battery anode recycled material
CN110842006A
Process for the recovery of active material from the cathodes of lithium-ion batteries
DE102014014894A1
Direct repair method for waste lithium-ion battery ternary positive electrode material
WO2022166197A1
Cited By
Method for upgrading and reconstructing single-crystal positive electrode material of lithium ion battery
CN121700494A