High-heat-resistance cellulose ester-based battery diaphragm and preparation method thereof

By using biomass cellulose ester materials and a non-solvent phase inversion method to prepare high heat-resistant cellulose ester-based battery separators, the problems of high cost and insufficient heat resistance of existing lithium battery separators are solved. This enables the low-cost and high-efficiency production of high heat-resistant separators, improving battery safety and fast-charging performance.

CN118943639APending Publication Date: 2024-11-12HEFEI GUOXUAN HIGH TECH POWER ENERGY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410975338.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing high heat-resistant lithium battery separator materials suffer from high manufacturing costs, difficult processing, and limited improvement in heat resistance, failing to meet the safety requirements of high-nickel, ultra-high-nickel, and lithium-rich manganese-based cathodes.

Method used

Using biomass cellulose ester as the separator material, a high heat-resistant cellulose ester-based battery separator is formed by dissolving it in a mixed solvent and adding a pore-forming agent, and then coating and creating pores using a non-solvent phase inversion method. This process includes coating, multi-stage coagulation bath extraction, and high-temperature setting.

Benefits of technology

It reduces the manufacturing cost of high heat-resistant separators, improves the heat resistance of separators and the safety performance of batteries, enhances battery wettability and fast-charging performance, and improves battery production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943639A_ABST
    Figure CN118943639A_ABST
Patent Text Reader

Abstract

The invention provides a high-heat-resistance cellulose ester-based battery diaphragm and a preparation method thereof, and belongs to the technical field of lithium ion battery diaphragm materials. The preparation method comprises the following steps: dissolving biomass cellulose ester in a mixed solvent, adding a pore-forming agent, and preparing coating film-forming slurry; coating a base material with the coating film-forming slurry to form a wet film; preparing a multi-stage coagulating bath, and extracting and pore-forming the wet film; drying and rolling the coating wet film containing the poor solvent; and performing high-temperature heat setting treatment after drying and rolling. The biomass polymer material with excellent heat resistance is selected as the diaphragm material, and compared with a synthesized high-heat-resistance material, the cost is low, and the diaphragm prepared from the material is excellent in heat resistance, small in water absorption and extremely small in heat shrinkage at high temperature; the non-solvent phase conversion method is adopted for pore forming, the pore diameter is uniform, the preparation process is simple, the performance is excellent under the high-rate and fast-charging condition, and the production efficiency of the high-heat-resistance diaphragm can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium-ion battery separator materials, and in particular relates to a high-heat-resistant cellulose ester-based battery separator and a preparation method thereof. Background Art

[0002] Lithium-ion battery is a secondary battery with high energy density, excellent cycle performance, long life, fast response speed, no memory effect, green and environmentally friendly, and no toxic and harmful substances. Therefore, it is widely used in consumer electronics, automotive power batteries, and energy storage fields. Usually, the four main materials of lithium-ion batteries are divided into positive electrode, negative electrode, diaphragm, and electrolyte. The diaphragm plays a key role in preventing the contact between the positive and negative electrodes and transmitting lithium ions in lithium-ion batteries. Its comprehensive cost accounts for about 15% of lithium-ion batteries, and it occupies an important position in lithium-ion batteries. At present, the main commercial separators are polyolefin separators, including wet-process biaxial polyethylene (PE) separators, dry-process monoaxial polyethylene separators, dry-process monoaxial polypropylene (PP) separators and dry-process biaxial polypropylene separators. The heat resistance temperature of polyolefin separators is low. For example, the thermal deformation temperature of PE separators is 80-100°C, the glass transition temperature is 135-140°C, and the thermal deformation temperature of PP separators is about 100°C, the glass transition temperature is about 160°C, and the safety boundary temperature is generally below 170°C, which makes traditional polyolefin separators unable to meet the requirements of today's 3C products and power batteries. It is urgent to develop lithium battery separators with higher service temperatures.

[0003] The preparation of traditional high heat-resistant lithium battery separators includes high heat-resistant separator base membranes and coated high heat-resistant battery separators. Existing high heat-resistant base membranes include polyethylene terephthalate (PET), polyimide (PI), meta-aramid (PMIA), etc. However, due to the difficulty in synthesis, the complex pore-making process for preparing micropores with suitable pore sizes, the high difficulty of processing technology, and the high cost, these high heat-resistant separator base membranes have not been industrialized on a large scale. The coated high heat-resistant battery separator is based on a polyolefin separator base membrane and is coated with a layer of organic (meta-aramid, para-aramid, PVDF (polyvinylidene fluoride)) organic material or inorganic ceramic (alumina, boehmite, etc.) material, but it is still essentially based on polyolefins. The heat resistance is indeed improved, but the improvement is quite limited. Currently, lithium batteries are continuously developing towards high-nickel, ultra-high-nickel and lithium-rich manganese-based positive electrodes. There is an urgent need for diaphragms with a safety boundary temperature of 200°C or even higher than 200°C. In view of the problems existing in the above two solutions, the development of a new type of high-heat-resistant diaphragm is particularly necessary. Summary of the invention

[0004] In the preparation process of high heat-resistant lithium-ion battery separators, it is necessary to comprehensively consider the process difficulty, production cost, and the best performance that can be achieved. The present invention designs a high heat-resistant cellulose ester-based battery separator and a preparation method thereof, which can effectively reduce the preparation cost of the high heat-resistant separator. At the same time, the lithium-ion battery separator provided by the present invention has an extremely low heat shrinkage rate at high temperatures. The separator adopts biomass polymer materials, which can improve the safety performance of the battery; and can increase the wettability of the surface, shorten the wetting time, and effectively improve the battery capacity and improve the safety performance of the battery under extreme heat conditions, solving the problems of high cost, difficult processing, and difficult dissolution of slurry of traditional high temperature resistant separators. In order to achieve the above purpose, the present invention provides the following technical solutions:

[0005] In one aspect of the present invention, a method for preparing a high heat-resistant cellulose ester-based battery separator is provided, comprising the following steps:

[0006] Dissolve the biomass cellulose ester in a mixed solvent, add a pore-forming agent, and apply strong stirring for a long time to completely dissolve the biomass polymer to prepare a coating film slurry;

[0007] Applying the coating film-forming slurry on the substrate to form a wet film;

[0008] Prepare multi-stage coagulation bath to extract pores in wet membrane;

[0009] Drying and rolling up the coated wet film containing the poor solvent;

[0010] High temperature heat setting treatment.

[0011] The present invention selects a biomass polymer material with excellent heat resistance as the diaphragm material. The raw material cellulose is the most abundant resource in nature and has a wide source. Compared with synthetic high-heat-resistant materials, it has low cost. The cellulose is esterified, and the addition of acetyl side groups increases the distance between the cellulose main chains, weakens the hydrogen bonding effect, and can be dissolved using common solvents under normal temperature conditions in the laboratory, thereby improving its solubility.

[0012] Furthermore, the general chemical formula of the biomass cellulose ester is as shown in formula (I),

[0013]

[0014] Among them, R 1 , R 2 and R 3 Each independently includes hydrogen, acetyl, and the degree of substitution of formula (I) is that acetyl occupies R 1 , R 2 and R 3The proportion of the site, with the degree of substitution in the range of 2.5 < DS < 3; the degree of polymerization n is an integer in the range of 200 - 400; the molecular weight range is 100,000 - 200,000.

[0015] Its main source is natural biomass cellulose. Natural cellulose has excellent heat resistance, with a glass transition temperature higher than 200 °C and a melting point higher than 300 °C. It has a high hydroxyl content and strong hydrogen bonding. Under conventional conditions, it is difficult to dissolve in common solvents. After esterifying it to form biomass cellulose ester, that is, converting R in formula (Ⅰ) 1 、R 2 and R 3 from -H to acetyl groups, the hydroxyl groups of biomass cellulose ester are greatly reduced. At the same time, the acetyl side groups increase the distance between the cellulose main chains, weakening the hydrogen bonding, and it can be dissolved using common solvents at room temperature in the laboratory. Among them, R1, R2, and R3 are converted from -H to acetyl groups during esterification.

[0016] The biomass cellulose ester of the present invention is preferably cellulose triacetate, and the degree of substitution is preferably 2.8 < DS < 3, more preferably 2.9 < DS < 3, further preferably 2.95 < DS < 3, and more preferably 2.98 ≤ DS < 3. Its glass transition temperature is preferably greater than 220 °C, and the melting point is preferably greater than 300 °C.

[0017] Furthermore, the mixed solvent is a good solvent and a poor solvent; in the mixed solvent, the mass proportion of the poor solvent is 3% - 10%; the mass ratio of the mixed solvent to the coating and film-forming slurry is 70% - 90%.

[0018] Furthermore, the pore-forming agent accounts for 1% - 10% of the mass of the coating and film-forming slurry.

[0019] Furthermore, the mass ratio of the biomass cellulose ester to the coating and film-forming slurry is 0% - 20%.

[0020] Furthermore, the good solvent includes chlorine-containing good solvents and non-chlorine-containing good solvents;

[0021] The chlorine-containing good solvents include dichloromethane or chloroform; the non-chlorine-containing good solvents include ethyl formate, propyl formate, amyl formate, methyl acetate, ethyl acetate, amyl acetate, acetone, methyl ethyl ketone, diethyl ketone, diisopropyl ether, or tetrahydrofuran;

[0022] The poor solvents include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol, 1-pentanol, 2-methyl-2-butanol, or cyclohexanol;

[0023] The good solvent of the present invention is preferably chlorine-containing, and the poor solvent is preferably alcohols with relatively low molecular weights and relatively low boiling points.

[0024] Furthermore, the pore-forming agent includes an inorganic pore-forming agent or an organic pore-forming agent;

[0025] The inorganic pore-forming agent includes any one or more of ammonium bicarbonate, ammonium carbonate, lithium chloride, sodium chloride, magnesium chloride, calcium carbonate or calcium chloride;

[0026] Organic pore-forming agents include any one or more of small molecule alcohols (methanol, ethanol, propanol, glycerol, acetone), acetic acid, tetrahydrofuran, dibutyl phthalate (DBP), dioctyl phthalate (DOP) and ionic liquids, dimethyl carbonate, or petroleum ether, low molecular weight polyethylene glycol (PEG), low molecular weight polyvinyl pyrrolidone (PVP), and low molecular weight polyvinyl alcohol (PVA).

[0027] The present invention prefers organic small molecules and low molecular weight polymer pore formers, and they have good solubility in both good solvents and poor solvents.

[0028] Furthermore, the coating film forming method is selected from one of blade coating and extrusion coating processes, and the coating layer is selected from one of single-layer coating and double-layer coating;

[0029] The viscosity of the coating slurry ranges from 15000 to 35000 mPa·s, the coating wet thickness is preferably 20 to 100 μm, most preferably 20 to 80 μm, and the coating dry thickness is preferably 5 to 30 μm, most preferably 5 to 15 μm.

[0030] The cellulose ester-based diaphragm prepared by the present invention has uniform pore size, and the porosity, air permeability and wettability have reached or exceeded the level of commercial polyolefin diaphragms, and has obvious physical property advantages. After being assembled into a battery, it can reduce the time required for the liquid injection and formation steps in the battery manufacturing process, and improve the production efficiency of lithium-ion batteries. The diaphragm prepared by this method has a larger pore size than the polyolefin diaphragm, at the order of hundreds of nanometers, while the polyolefin diaphragm is at the order of tens of nanometers. Its performance under high-rate fast charging (greater than 3C) conditions may be even better.

[0031] Furthermore, the number of stages of the multi-stage coagulation bath is 3 to 7, specifically 3, 4, 5 or more stages;

[0032] The multi-stage coagulation bath is prepared with a good solvent and a poor solvent in a proportional gradient, wherein the proportion of the good solvent decreases as the number of stages increases, and the proportion of the poor solvent increases as the number of stages increases; wherein the poor solvent and the good solvent should be completely miscible, and the boiling point of the poor solvent should be relatively low, so as to facilitate the subsequent volatilization and drying step to remove the poor solvent, and the boiling point of the poor solvent is preferably less than 120°C, more preferably less than 90°C.

[0033] Among them, the specific working principle of the coagulation bath and the pore-forming agent is: the coated wet film enters the multi-stage coagulation bath in turn, the good solvent and the poor solvent in the coagulation bath are mutually soluble in any proportion, the poor solvent diffuses into the coating, the good solvent diffuses into the coagulation bath, the polymer in the coating will undergo phase separation, and after passing through the multi-stage coagulation bath, a two-phase region of pores and polymer containing poor solvent is finally formed; adding a pore-forming agent can make the phase separation more uniform, so as to avoid the surface densification phenomenon, and finally the coated wet film is peeled off from the substrate.

[0034] Furthermore, during the extraction process, the coated wet film is subjected to a longer time in the first coagulation bath, preferably greater than 5 minutes, and most of the solvent in the coating is exchanged by the solvent. The coagulation bath times of each stage after the second stage can be equal or decrease, and the time is preferably less than 60 to 150 seconds, and more preferably less than 60 to 120 seconds.

[0035] The present invention adopts a non-solvent phase conversion method to form pores. After the coating film-forming slurry is coated on the base film, it can be supported by the substrate and continuously pass through a multi-stage coagulation bath to form pores. The coating and pore forming can be a continuous process. The preparation process is simple and the production process is efficient, which is conducive to improving the production efficiency of high heat-resistant diaphragms and increasing the added value of products.

[0036] Furthermore, the drying method is selected from one of hot air drying, infrared heating drying, and microwave drying; the drying temperature is selected near the boiling point of the poor solvent (50-120°C).

[0037] Furthermore, the heat setting temperature is 240-270° C., and the heat setting time is 10-30 minutes.

[0038] Furthermore, another aspect of the present invention provides a high heat-resistant cellulose ester-based battery separator, which is prepared by the above preparation method.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The present invention selects biomass polymer materials with excellent heat resistance as the diaphragm material. The raw material cellulose is the most abundant resource in nature and has a wide source. Compared with synthetic high-heat-resistant materials, it is low in cost. The diaphragm prepared from this material has excellent heat resistance, low water absorption, and extremely small thermal shrinkage at high temperatures.

[0041] (2) The cellulose ester-based diaphragm prepared by the present invention has a uniform pore size, and its porosity, air permeability and wettability have reached or exceeded the level of commercial polyolefin diaphragms, which can improve the production efficiency of lithium-ion batteries; and the diaphragm prepared by this method has a larger pore size than that of polyolefin diaphragms, at the order of hundreds of nanometers, and its performance under high-rate fast charging (greater than 3C) conditions will be even better.

[0042] (3) The present invention adopts a non-solvent phase conversion method to form pores, and the preparation process is simple, which is conducive to improving the production efficiency of high-heat-resistant diaphragms and increasing the added value of products. At present, there is no precedent for using such a method to prepare cellulose-based diaphragms. The present invention is original.

[0043] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by implementing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 A schematic diagram of the steps for preparing the battery separator provided by the present invention;

[0045] Figure 2 is a temperature rise heat flow curve of biomass cellulose triacetate involved in an embodiment of the present invention;

[0046] Figure 3 The following are SEM photos of samples of Examples 1-5 and Comparative Example 2. DETAILED DESCRIPTION

[0047] In order to make the purpose, technical scheme and advantages of the present invention clearer, the implementation scheme of the present application will be described in detail below in conjunction with specific examples. The technical terms and scientific terms used in the present invention have the meanings generally understood by ordinary technicians in the technical field to which the present invention belongs, without other definitions. Without departing from the concept of the present invention, those skilled in the art may make various improvements and changes to the specific implementation methods of the present invention specification, which all belong to the protection scope of the present invention. The raw materials involved in the following content can be obtained from commercial channels unless otherwise specified.

[0048] Figure 1 The schematic diagram of the preparation steps of the battery separator provided by the present invention shows the following embodiments in combination with the preparation steps:

[0049] Example 1

[0050] A high heat-resistant cellulose ester-based battery separator and a preparation method thereof, comprising the following steps:

[0051] Step 1: Prepare coating film slurry. The biomass cellulose ester selected in Example 1 is cellulose triacetate with an acetyl substitution degree of 2.98 (DS=2.98). Its thermal analysis curve is as follows: Figure 2As shown, its glass transition temperature is as high as 185°C and its melting point is as high as 296°C. Its coating film slurry is composed of a mixture of a good solvent and a poor solvent. The good solvent is a chlorine-based good solvent dichloromethane, and the poor solvent is methanol. The mass ratio of dichloromethane to methanol is 95:5. The pore-forming agent is a low molecular weight polyethylene glycol (PEG) with a molecular weight of 600. According to the calculated slurry solid content, the slurry ratio is shown in Table 1. A certain mass of cellulose triacetate and PEG are weighed, and a certain volume of dichloromethane and methanol are added. The cellulose triacetate accounts for 15% of the mass of the coating film slurry, and the pore-forming agent accounts for 5% of the mass of the coating film slurry. The slurry dissolution temperature is preferably 30°C, the stirring rate is 200rpm, and the stirring is for more than 5h, and then it is left to stand for 2h to defoam. The sealing of the dissolving kettle is good. Under the above conditions, it is stirred and mixed into a coating film slurry. At this time, the slurry viscosity is 23300mPa·s.

[0052] Step 2: coating to form a film. The coating film slurry prepared in step 1 is evenly coated on the polycarbonate film substrate by single-sided coating. The thickness of the polycarbonate substrate is 100 μm. This embodiment uses a doctor blade coating, the coating wet thickness is 80 μm, the coating dry thickness is 15 μm, and the coating speed is 20 mm / s.

[0053] Step 3: Multi-stage extraction and pore formation, prepare multi-stage coagulation bath. The coagulation bath can be prepared according to the gradient ratio of good solvent and poor solvent. The good solvent of the coagulation bath is dichloromethane, and the poor solvent of the coagulation bath is ethanol. The boiling point of dichloromethane is 39.8°C, and the boiling point of ethanol is 78°C. The boiling points of both are lower than 80°C, which is convenient for subsequent drying. In this embodiment, 5-stage coagulation baths are prepared: Level 1, dichloromethane: ethanol = 70:30; Level 2, dichloromethane: ethanol = 50:50; Level 3, dichloromethane: ethanol = 30:70; Level 4, dichloromethane: ethanol = 10:90; Level 4, dichloromethane: ethanol = 0:100; After the coating wet film prepared in step 2 is coated, it can enter the five-stage coagulation bath in sequence. The good solvent and the poor solvent in the coagulation bath are mutually soluble in any proportion. The poor solvent diffuses into the coating, and the good solvent diffuses into the coagulation bath. The polymer in the coating will undergo Phase separation, after multi-stage coagulation bath, finally forms pores and polymer two-phase region containing poor solvent. Adding pore-forming agent can make phase separation more uniform and avoid surface density. The residence time of the first stage coagulation bath is 600s; the residence time of the second stage coagulation bath is 120s; the residence time of the third stage coagulation bath is 120s; the residence time of the fourth stage coagulation bath is 60s; the residence time of the fifth stage coagulation bath is 60s. After five-stage coagulation bath, the solvent exchange process is basically completed, the solvent dichloromethane in the coated wet film is extracted, and finally the coated film is peeled off from the polycarbonate film substrate.

[0054] Step 4: Drying: subjecting the coated wet film containing the poor solvent in step 3 to hot air drying at a drying temperature of 50° C. for 80 seconds. After drying, the coated separator is rolled up.

[0055] Step 5: heat setting, the coating film obtained by drying in step 4 is subjected to heat setting treatment, the heat setting temperature is 250°C, the heat setting time is 3h, the high temperature heat setting treatment eliminates the internal stress during the processing and improves the crystallinity of the film, and increases the dimensional stability and mechanical strength of the film. After the heat setting is completed, the biomass triacetate cellulose ester separator of Example 1 is prepared, and its surface morphology is as follows Figure 3 shown.

[0056] Example 2

[0057] Step 1: Prepare coating film slurry. The biomass cellulose ester selected in Example 2 is cellulose triacetate with an acetyl substitution degree of 2.98 (DS=2.98). Its thermal analysis curve is as follows: Figure 1 As shown, its glass transition temperature is as high as 185°C and its melting point is as high as 296°C. Its coating film-forming slurry is composed of a mixture of a good solvent and a poor solvent. The good solvent is dichloromethane, a chlorine-based good solvent, and the poor solvent is methanol. The mass ratio of dichloromethane to methanol is 95:5. The pore-forming agent is a low molecular weight polyethylene glycol (PEG) with a molecular weight of 600. According to the calculated slurry solid content, the slurry ratio is shown in Table 1. A certain mass of cellulose triacetate and PEG are weighed, and a certain volume of dichloromethane and methanol are added. The cellulose triacetate accounts for 15% of the mass of the coating film-forming slurry, and the pore-forming agent accounts for 2.5% of the mass of the coating film-forming slurry. The slurry dissolution temperature is preferably 30°C, the stirring rate is 200rpm, and the stirring is for more than 5h, and then it is left to stand for 2h to defoam. The sealing of the dissolving kettle is good. Under the above conditions, it is stirred and mixed into a coating film-forming slurry. At this time, the slurry viscosity is 25100mPa·s.

[0058] Step 2: coating to form a film. The coating film slurry prepared in step 1 is evenly coated on the polycarbonate film substrate by single-sided coating. The thickness of the polycarbonate substrate is 100 μm. This embodiment uses a doctor blade coating, the coating wet thickness is 85 μm, the coating dry thickness is 16 μm, and the coating speed is 20 mm / s.

[0059] Step 3: multi-stage extraction pore making, preparing multi-stage coagulation bath, the coagulation bath can be prepared according to the gradient ratio of good solvent and poor solvent, the good solvent of the coagulation bath is selected from dichloromethane, and the poor solvent of the coagulation bath is selected from ethanol, the boiling point of dichloromethane is 39.8°C, and the boiling point of ethanol is 78°C, both of which are lower than 80°C, which is convenient for subsequent drying. In this embodiment, 5-stage coagulation baths are prepared: the first stage, dichloromethane: ethanol = 70:30; the second stage, dichloromethane: ethanol = 50:50; the third stage, dichloromethane: ethanol = 30:70; the fourth stage, dichloromethane: ethanol = 10:90; the fourth stage, dichloromethane: ethanol = 0:100; After the coating of the wet film prepared in step 2 is completed, it can enter the five-stage coagulation bath in sequence. The good solvent and the poor solvent in the coagulation bath are mutually soluble in any proportion. The poor solvent diffuses into the coating, and the good solvent diffuses into the coagulation bath. The polymer in the coating will undergo phase separation. After multiple stages of coagulation baths, a two-phase region of pores and polymer containing poor solvents is finally formed. The addition of pore-forming agents can make the phase separation more uniform and avoid surface densification. The residence time of the first stage coagulation bath is 600s; the residence time of the second stage coagulation bath is 120s; the residence time of the third stage coagulation bath is 120s; the residence time of the fourth stage coagulation bath is 60s; and the residence time of the fifth stage coagulation bath is 60s. After the five-stage coagulation bath, the solvent exchange process is basically completed, the solvent dichloromethane in the wet film is extracted, and finally the coating film is peeled off from the polycarbonate film substrate.

[0060] Step 4: Drying: subjecting the coated wet film containing the poor solvent in step 3 to hot air drying at a drying temperature of 50° C. for 80 seconds. After drying, the coated separator is rolled up.

[0061] Step 5: heat setting, the coating film obtained by drying in step 4 is subjected to heat setting treatment, the heat setting temperature is 250°C, the heat setting time is 3h, the high temperature heat setting treatment eliminates the internal stress during the processing and improves the crystallinity of the film, and increases the dimensional stability and mechanical strength of the film. After the heat setting is completed, the biomass triacetate cellulose ester separator of Example 2 is prepared, and its surface morphology is as follows Figure 3 shown.

[0062] Example 3

[0063] Step 1: Prepare coating film slurry. The biomass cellulose ester selected in Example 3 is cellulose triacetate with an acetyl substitution degree of 2.98 (DS=2.98). Its thermal analysis curve is as follows: Figure 2As shown, its glass transition temperature is as high as 185°C and its melting point is as high as 296°C. Its coating film slurry is composed of a mixture of a good solvent and a poor solvent. The good solvent is a chlorine-based good solvent dichloromethane, and the poor solvent is methanol. The mass ratio of dichloromethane to methanol is 95:5. The pore-forming agent is a low molecular weight polyethylene glycol (PEG) with a molecular weight of 600. According to the calculated slurry solid content, the slurry ratio is shown in Table 1. A certain mass of cellulose triacetate and PEG are weighed, and a certain volume of dichloromethane and methanol are added. The cellulose triacetate accounts for 15% of the mass of the coating film slurry, and the pore-forming agent accounts for 5% of the mass of the coating film slurry. The slurry dissolution temperature is preferably 30°C, the stirring rate is 200rpm, and the stirring is for more than 5h, and then it is left to stand for 2h to defoam. The sealing of the dissolving kettle is good. Under the above conditions, it is stirred and mixed into a coating film slurry. At this time, the slurry viscosity is 23300mPa·s.

[0064] Step 2: coating and film formation. The coating film slurry prepared in step 1 is evenly coated on the untempered float glass substrate by single-sided coating. The float glass substrate is 3 mm thick. In this embodiment, doctor blade coating is used. The wet coating thickness is 80 μm, the dry coating thickness is 13 μm, and the coating speed is 20 mm / s.

[0065] Step 3: Multi-stage extraction pore making, preparing multi-stage coagulation bath, the coagulation bath can be prepared according to the gradient ratio of good solvent and poor solvent, the good solvent of the coagulation bath is selected from dichloromethane, and the poor solvent of the coagulation bath is selected from ethanol, the boiling point of dichloromethane is 39.8°C, and the boiling point of ethanol is 78°C, both of which are lower than 80°C, which is convenient for subsequent drying. In this embodiment, a 5-stage coagulation bath is prepared: the first stage, dichloromethane: ethanol = 70:30; the second stage, dichloromethane: ethanol = 50:50; the third stage, dichloromethane: ethanol = 30:70; the fourth stage, dichloromethane: ethanol = 10:90; the fourth stage, dichloromethane: ethanol = 0:100; after the coating wet film prepared in step 2 is coated, it can enter the five-stage coagulation bath in sequence In the coagulation bath, the good solvent and the poor solvent are mutually soluble in any proportion, the poor solvent diffuses into the coating, the good solvent diffuses into the coagulation bath, the polymer in the coating will undergo phase separation, and after multiple stages of coagulation baths, a two-phase region of pores and polymer containing poor solvents is finally formed. Adding a pore-forming agent can make the phase separation more uniform and avoid surface densification. The residence time of the first stage coagulation bath is 600s; the residence time of the second stage coagulation bath is 120s; the residence time of the third stage coagulation bath is 120s; the residence time of the fourth stage coagulation bath is 60s; the residence time of the fifth stage coagulation bath is 60s; after five stages of coagulation baths, the solvent exchange process is basically completed, the solvent dichloromethane in the coated wet film is extracted, and finally the coated film is peeled off from the polycarbonate film substrate.

[0066] Step 4: Drying: subjecting the coated wet film containing the poor solvent in step 3 to hot air drying at a drying temperature of 50° C. for 80 seconds. After drying, the coated separator is rolled up.

[0067] Step 5: heat setting, the coating film obtained by drying in step 4 is subjected to heat setting treatment, the heat setting temperature is 250°C, the heat setting time is 3h, the high temperature heat setting treatment eliminates the internal stress during the processing and improves the crystallinity of the film, and increases the dimensional stability and mechanical strength of the film. After the heat setting is completed, the biomass triacetate cellulose ester separator of Example 3 is prepared, and its surface morphology is as follows Figure 3 shown.

[0068] Example 4

[0069] Step 1: Prepare coating film slurry. The biomass cellulose ester selected in Example 4 is cellulose triacetate with an acetyl substitution degree of 2.98 (DS=2.98). Its thermal analysis curve is as follows: Figure 2 As shown, its glass transition temperature is as high as 185°C and its melting point is as high as 296°C. Its coating film slurry is composed of a mixture of a good solvent and a poor solvent. The good solvent is a chlorine-based good solvent dichloromethane, and the poor solvent is methanol. The mass ratio of dichloromethane to methanol is 95:5. The pore-forming agent is a low molecular weight polyethylene glycol (PEG) with a molecular weight of 600. According to the calculated slurry solid content, the slurry ratio is shown in Table 1. A certain mass of cellulose triacetate and PEG are weighed, and a certain volume of dichloromethane and methanol are added. The cellulose triacetate accounts for 15% of the mass of the coating film slurry, and the pore-forming agent accounts for 2.5% of the mass of the coating film slurry. The slurry dissolution temperature is preferably 30°C, the stirring rate is 200rpm, and the stirring is for more than 5h, and then it is left to stand for 2h to defoam. The sealing of the dissolving kettle is good. Under the above conditions, it is stirred and mixed into a coating film slurry. At this time, the slurry viscosity is 25100mPa·s.

[0070] Step 2: coating and film formation. The coating film slurry prepared in step 1 is evenly coated on the untempered float glass substrate by single-sided coating. The float glass substrate is 3 mm thick. In this embodiment, a doctor blade is used for coating. The wet coating thickness is 80 μm, the dry coating thickness is 14 μm, and the coating speed is 20 mm / s.

[0071] Step 3: Multi-stage extraction pore making, preparing multi-stage coagulation bath, the coagulation bath can be prepared according to the gradient ratio of good solvent and poor solvent, the good solvent of the coagulation bath is selected from dichloromethane, and the poor solvent of the coagulation bath is selected from ethanol, the boiling point of dichloromethane is 39.8°C, and the boiling point of ethanol is 78°C, both of which are lower than 80°C, which is convenient for subsequent drying. In this embodiment, a 5-stage coagulation bath is prepared: the first stage, dichloromethane: ethanol = 70:30; the second stage, dichloromethane: ethanol = 50:50; the third stage, dichloromethane: ethanol = 30:70; the fourth stage, dichloromethane: ethanol = 10:90; the fourth stage, dichloromethane: ethanol = 0:100; after the coating wet film prepared in step 2 is coated, it can enter the five-stage coagulation bath in sequence In the coagulation bath, the good solvent and the poor solvent are mutually soluble in any proportion, the poor solvent diffuses into the coating, the good solvent diffuses into the coagulation bath, the polymer in the coating will undergo phase separation, and after multiple stages of coagulation baths, a two-phase region of pores and polymer containing poor solvents is finally formed. Adding a pore-forming agent can make the phase separation more uniform and avoid surface densification. The residence time of the first stage coagulation bath is 600s; the residence time of the second stage coagulation bath is 120s; the residence time of the third stage coagulation bath is 120s; the residence time of the fourth stage coagulation bath is 60s; the residence time of the fifth stage coagulation bath is 60s; after five stages of coagulation baths, the solvent exchange process is basically completed, the solvent dichloromethane in the coated wet film is extracted, and finally the coated film is peeled off from the polycarbonate film substrate.

[0072] Step 4: Drying: subjecting the coated wet film containing the poor solvent in step 3 to hot air drying at a drying temperature of 50° C. for 80 seconds. After drying, the coated separator is rolled up.

[0073] Step 5: heat setting, the coating film obtained by drying in step 4 is subjected to heat setting treatment, the heat setting temperature is 250°C, the heat setting time is 3h, the high temperature heat setting treatment eliminates the internal stress during the processing and improves the crystallinity of the film, and increases the dimensional stability and mechanical strength of the film. After the heat setting is completed, the biomass triacetate cellulose ester diaphragm of Example 4 is prepared, and its surface morphology is as follows Figure 3 shown.

[0074] Example 5

[0075] Step 1: Prepare coating film slurry. The biomass cellulose ester selected in Example 4 is cellulose triacetate with an acetyl substitution degree of 2.98 (DS=2.98). Its thermal analysis curve is as follows: Figure 2As shown, its glass transition temperature is as high as 185°C and its melting point is as high as 296°C. Its coating film-forming slurry is composed of a mixture of a good solvent and a poor solvent. The good solvent is dichloromethane, a chlorine-based good solvent, and the poor solvent is methanol. The mass ratio of dichloromethane to methanol is 95:5. According to the calculated slurry solid content, the slurry ratio is shown in Table 1. A certain mass of cellulose triacetate is weighed, and a certain volume of dichloromethane and methanol are added. The cellulose triacetate accounts for 15% of the mass of the coating film-forming slurry. The slurry dissolution temperature is preferably 30°C, the stirring rate is 200rpm, and the stirring is for more than 5h, and then it is left to stand for 2h to defoam. The sealing of the dissolving kettle is good. Under the above conditions, it is stirred and mixed into a coating film-forming slurry. At this time, the slurry viscosity is 27200mPa·s.

[0076] Step 2: coating and film formation. The coating film slurry prepared in step 1 is evenly coated on the untempered float glass substrate by single-sided coating. The float glass substrate is 3 mm thick. This embodiment uses a doctor blade coating, with a coating wet thickness of 80 μm, a coating dry thickness of 15 μm, and a coating speed of 20 mm / s.

[0077] Step 3: Multi-stage extraction pore making, preparing multi-stage coagulation bath, the coagulation bath can be prepared according to the gradient ratio of good solvent and poor solvent, the good solvent of the coagulation bath is selected from dichloromethane, and the poor solvent of the coagulation bath is selected from ethanol, the boiling point of dichloromethane is 39.8°C, and the boiling point of ethanol is 78°C, both of which are lower than 80°C, which is convenient for subsequent drying. In this embodiment, a 5-stage coagulation bath is prepared: the first stage, dichloromethane: ethanol = 70:30; the second stage, dichloromethane: ethanol = 50:50; the third stage, dichloromethane: ethanol = 30:70; the fourth stage, dichloromethane: ethanol = 10:90; the fourth stage, dichloromethane: ethanol = 0:100; after the coating wet film prepared in step 2 is coated, it can enter the five-stage coagulation bath in sequence In the coagulation bath, the good solvent and the poor solvent are mutually soluble in any proportion, the poor solvent diffuses into the coating, the good solvent diffuses into the coagulation bath, the polymer in the coating will undergo phase separation, and after multiple stages of coagulation baths, a two-phase region of pores and polymer containing poor solvents is finally formed. Adding a pore-forming agent can make the phase separation more uniform and avoid surface densification. The residence time of the first stage coagulation bath is 600s; the residence time of the second stage coagulation bath is 120s; the residence time of the third stage coagulation bath is 120s; the residence time of the fourth stage coagulation bath is 60s; the residence time of the fifth stage coagulation bath is 60s; after five stages of coagulation baths, the solvent exchange process is basically completed, the solvent dichloromethane in the coated wet film is extracted, and finally the coated film is peeled off from the polycarbonate film substrate.

[0078] Step 4: Drying: subjecting the coated wet film containing the poor solvent in step 3 to hot air drying at a drying temperature of 50° C. for 80 seconds. After drying, the coated separator is rolled up.

[0079] Step 5: heat setting, the coating film obtained by drying in step 4 is subjected to heat setting treatment, the heat setting temperature is 250°C, the heat setting time is 3h, the high temperature heat setting treatment eliminates the internal stress during the processing and improves the crystallinity of the film, and increases the dimensional stability and mechanical strength of the film. After the heat setting is completed, the biomass triacetate cellulose ester diaphragm of Example 5 is prepared, and its surface morphology is as follows Figure 3 shown.

[0080] Comparative Example 1 is a commercial wet biaxially oriented polyethylene diaphragm, the thickness of the polyethylene diaphragm is 12 μm, and its surface morphology is as follows: Figure 3 shown.

[0081] Comparative Example 2 is a dry stretched polypropylene diaphragm, the thickness of the polypropylene diaphragm is 14 μm, and its surface morphology is as follows Figure 3 shown.

[0082] The coating film-forming slurry formulation parameters and coagulation bath ratio and time parameters of Examples 1-5 and Comparative Examples 1-2 are shown in Table 1 (CA is cellulose triacetate);

[0083] Table 1 Coating film slurry formula

[0084]

[0085] The basic physical properties of Examples 1-5 and Comparative Examples 1-2 are shown in Table 2;

[0086] Table 2 Basic physical properties of the diaphragms of the embodiments and comparative examples

[0087]

[0088] The high temperature heat shrinkage properties of Examples 1-5 and Comparative Examples 1-2 are shown in Table 3 (MD longitudinal direction, TD transverse direction);

[0089] Table 3 High temperature heat shrinkage of examples and comparative examples

[0090]

[0091] As can be seen from Table 3, the thermal shrinkage of the polyethylene-based film and the polypropylene-based film in Comparative Examples 1 and 2 at 150°C is already very large. The melting point of ultra-high molecular weight polyethylene is about 138°C, and the melting point of polypropylene is about 165°C. At 180°C, they are already in a molten state and have no mechanical strength. The biomass cellulose triacetate ester diaphragm prepared in Examples 1-5 can greatly reduce its thermal shrinkage, among which the effects of Examples 1-2 and Example 5 are more excellent. From the pore size data, if a pore-forming agent is added to the diaphragm prepared on the glass substrate, its pore size is extremely large. , reaching tens of microns. Such a diaphragm installed in a battery will cause a short circuit in the battery and cannot meet the battery's use conditions. If no pore-forming agent is added, there are no pores on the membrane surface, which cannot be called a diaphragm. It will cause a short circuit in the battery and does not meet the battery's use conditions. Only the biomass cellulose triacetate ester diaphragm prepared in Example 1 and Example 2 has a pore size of hundreds of nanometers, which will not cause a short circuit in the battery. Its pore size is larger than that of the polyolefin diaphragm, and its performance under high-rate fast charging (>3C) conditions may be more excellent, while the pore size of the polyolefin diaphragm is difficult to further expand. In terms of interfacial properties, polyethylene and polypropylene diaphragms are formed by the polymerization of non-polar monomers, and their interfaces are generally hydrophobic, and the electrolyte contact angle is large, reaching 50°. The hydrophilicity of biomass cellulose triacetate is greatly improved due to the presence of some hydroxyl groups. The electrolyte contact angle in Examples 1-5 is reduced to 11-13°, showing that the diaphragm has excellent electrolyte wettability in the subsequent battery assembly process, effectively shortening the electrolyte infiltration time and reducing the time required for battery injection. In summary, the preparation method of the present invention can reduce the preparation cost of high heat-resistant diaphragms. At the same time, the lithium-ion battery diaphragm provided by the present invention has an extremely low thermal shrinkage rate at high temperatures, which improves the safety performance of the battery under extreme thermal conditions; and can increase the wettability of the surface, shorten the wetting time, and effectively improve the battery production efficiency; and the pore size is relatively large compared to the polyolefin diaphragm, which can effectively improve the fast charging performance of the battery.

[0092] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a highly heat-resistant cellulose ester-based battery separator, It is characterized in that The following steps are involved: Dissolving biomass cellulose ester in a mixed solvent, adding a pore-forming agent, and preparing a coating film-forming slurry; Applying the coating film-forming slurry on the substrate to form a wet film; Prepare multi-stage coagulation bath to extract pores in wet membrane; Drying and rolling up the coated wet film containing the poor solvent; High temperature heat setting treatment.

2. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 1, It is characterized in that The general chemical formula of the biomass cellulose ester is shown in formula (I), wherein, R 1 , R 2 and R 3 each independently include a group such as hydrogen and acetyl group, and the degree of substitution of formula (I) is 2.5 < DS < 3; the degree of polymerization n is an integer in the range of 200 to 400; the molecular weight range is 100,000 to 200,000.

3. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 1, It is characterized in that The mixed solvent is a good solvent and a poor solvent; In the mixed solvent, the mass of the poor solvent accounts for 3% to 10%; The mass ratio of the mixed solvent to the coating film-forming slurry is 70% to 90%.

4. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 1, It is characterized in that The pore-forming agent accounts for 1% to 10% of the coating film-forming slurry mass.

5. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 1, It is characterized in that The mass ratio of the biomass cellulose ester to the coating film-forming slurry is 0% to 20%.

6. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 3, It is characterized in that The good solvent includes a chlorine-based good solvent and a non-chlorine-based good solvent.

7. A method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 6, It is characterized in that The chlorine-based good solvent includes dichloromethane or chloroform; the non-chlorine-based good solvent includes ethyl formate, propyl formate, pentyl formate, methyl acetate, ethyl acetate, pentyl acetate, acetone, methyl ethyl ketone, diethyl ketone, diisopropyl ether or tetrahydrofuran.

8. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 3, It is characterized in that The poor solvent includes methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol, 1-pentanol or 2-methyl-2-butanol or cyclohexanol.

9. A method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 1 or 4, It is characterized in that The pore formers include inorganic pore formers and organic pore formers.

10. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 9, It is characterized in that The inorganic pore-forming agent includes any one or more of ammonium bicarbonate, ammonium carbonate, lithium chloride, sodium chloride, magnesium chloride, calcium carbonate or calcium chloride.

11. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 9, It is characterized in that The organic pore-forming agent includes any one or more of small molecule alcohols, acetic acid, tetrahydrofuran, dibutyl phthalate, dioctyl phthalate, dimethyl carbonate, petroleum ether, polyethylene glycol, polyvinyl pyrrolidone, and polyvinyl alcohol; The small molecule alcohols include methanol, ethanol, propanol, glycerol and acetone.

12. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 1, It is characterized in that The coating film forming method is selected from one of blade coating and extrusion coating processes, and the coating layer is selected from one of single-layer coating and double-layer coating; The viscosity of the coating slurry ranges from 15000 to 35000 mPa·s, the coating wet thickness ranges from 20 to 100 μm, and the coating dry thickness ranges from 5 to 30 μm.

13. A method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 1 or 3, It is characterized in that The number of stages of the multi-stage coagulation bath is 3 to 7; The multi-stage coagulation bath is prepared with good solvent and poor solvent in a gradient ratio, the proportion of good solvent decreases with the increase of the stage number, and the proportion of poor solvent increases with the increase of the stage number.

14. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 1, It is characterized in that During the extraction process, the wet film is subjected to the first-level coagulation bath for 5 to 10 minutes, and the coagulation bath times after the second level are equal or decrease, ranging from 60 to 150 seconds.

15. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 1, It is characterized in that The drying method is selected from hot air drying, infrared heating drying and microwave drying.

16. The method for preparing a highly heat-resistant cellulose ester-based battery separator according to claim 1, It is characterized in that The high temperature heat setting temperature is 240-270° C., and the time is 10-30 minutes.

17. A high heat-resistant cellulose ester-based battery separator, prepared by the preparation method according to any one of claims 1 to 16.

Citation Information

Patent Citations

  • Separator with increased puncture resistance

    CN103026530A

  • Polyvinylidene fluoride / cyanoethyl cellulose composite lithium ion battery diaphragm and preparation method thereof

    CN107256936A

  • Modified aramid polymer, aramid membrane casting solution, lithium battery diaphragm, preparation methods and lithium battery

    CN112538162A

  • Method of manufacturing resin porous body

    CN113118005A

  • Polymer mixed slurry coated diaphragm and preparation method thereof

    CN113540687A