Circuit board production process capable of preventing board warping and circuit board
By optimizing the design and process flow in circuit board manufacturing, including semi-cured sheet pressing, vertical continuous plating and bar fixing, combined with hot pressing and cold pressing, the deformation problem of circuit board is solved, the pass rate and symmetry are improved, and the Functional implementation of the board.
Patent Information
- Application Number
- CN202411183960.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
During the circuit board manufacturing process, thin plates are prone to deformation due to the bend of the substrate, which affects the functional realization of subsequent patches. The existing leveling methods pose great risks and are difficult to meet the strict requirements for deformation of special circuit boards, affecting the pass rate.
By optimizing the circuit during the circuit board design stage, the difference in copper residual ratio of the inner symmetric layer and the difference in copper foil area of the outer layer are less than or equal to the predetermined threshold, and semi-cured sheet pressing, vertical continuous plating and carding are used during the manufacturing process. The strips are fixed, combined with hot pressing and cold pressing leveling technology to ensure that the plate is within the predetermined range.
Effectively reduce the curve deformation of the circuit board, improve the pass rate, ensure the symmetry and function of the board, especially to eliminate stress when the assembly is heated, and reduce correction operations after assembly.
Smart Images

Figure CN118946009A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the technical field of circuit board production, and in particular to a circuit board production process and a circuit board for preventing the circuit board from warping. Background Art
[0002] In the process of circuit board manufacturing, if the control is not good, it is easy to cause the substrate to bend and deform, affecting the subsequent mounting. For deformed boards, the general treatment method is to straighten them by hot pressing. After hot pressing and straightening, the diagonal length is used as the reference. If the bow value is less than 0.75%, it meets the shipping standard. There is usually no requirement for the deformation after the SMT reflow soldering of the installed components, as long as it does not affect its use function.
[0003] However, for some special thin boards, a small deformation is still required after the components are installed by SMT to ensure the function of the board. For example, after the components are installed by SMT on one or both sides of the board, the bow value reaches 0.75% or even 0.5%. If the deformation requirement is not met, a fixture with hollowed-out corresponding component positions is generally used for leveling. This leveling effect is generally mediocre and there are great risks. Therefore, how to reduce the deformation of such circuit boards during the production process and improve the qualified rate has become a problem to be solved. Summary of the invention
[0004] In view of the above problems, an embodiment of the present invention provides a circuit board production process and a circuit board for preventing board warping, which are used to solve the problem of circuit board deformation existing in the prior art.
[0005] According to one aspect of an embodiment of the present invention, a circuit board production process for preventing board warping is provided, the production process includes circuit board design and circuit board manufacturing, the circuit board manufacturing includes inner layer manufacturing, inner layer lamination, drilling and copper plating, outer layer manufacturing, outer layer electroplating, etching, solder mask, solder mask text, surface treatment and molding of the circuit board:
[0006] Designing the circuit of the circuit board in the design stage so that the difference of the residual copper rate of the inner symmetrical layer and the difference of the percentage of the copper foil area of the outer symmetrical layer are both less than or equal to a predetermined threshold;
[0007] When laminating the inner layer, use a prepreg sheet between the layers and extend the cold pressing time;
[0008] When electroplating the two outer layers, vertical continuous electroplating is used and electroplating is performed twice, so that the difference in copper plating thickness at the same position of the two outer layers is less than a predetermined thickness after electroplating;
[0009] Inserting the plurality of circuit boards on the inserting rack after the solder mask text, and fixing the plurality of circuit boards with clamping strips before baking the boards;
[0010] After the circuit board is formed, if it is detected that the circuit board is warped, straightening and leveling are repeatedly performed until the bow value of the circuit board is within a predetermined range. The straightening and leveling includes first performing hot pressing and then cold pressing.
[0011] In an optional manner, the step of designing the circuit of the circuit board in the design stage so that the difference in residual copper rate of the inner symmetrical layer and the difference in copper foil area percentage of the outer symmetrical layer are both less than or equal to a predetermined threshold value includes:
[0012] If the residual copper rate difference of the inner symmetric layer or the copper foil area percentage difference of the outer symmetric layer is greater than a predetermined threshold, the process edge of the inner symmetric layer or the process edge of the outer symmetric layer is increased or decreased.
[0013] In an optional manner, when laminating the inner layer, a prepreg is used between the layers for lamination, and after the step of extending the cold pressing time during cold pressing, the method further comprises:
[0014] After lamination, the board thickness is measured by a multi-point method, and the thickness uniformity of the circuit board is evaluated based on the board thickness and a predetermined center value of the board thickness, so as to select a circuit board with uniform thickness.
[0015] In an optional manner, when electroplating the two outer layers, vertical continuous electroplating is used and electroplating is performed twice, and the step of making the difference in copper plating thickness at the same position of the two outer layers less than a predetermined thickness after electroplating includes:
[0016] A clamp is used to clamp one side of the circuit board for a first vertical continuous electroplating, and then the opposite side of the circuit board is clamped for a second vertical continuous electroplating. After electroplating, the difference in copper plating thickness at the same position of the two outer layers is less than a predetermined thickness.
[0017] In an optional manner, the process of electroplating the two outer layers by using vertical continuous electroplating and performing electroplating twice, and making the difference in copper plating thickness at the same position of the two outer layers less than a predetermined thickness after electroplating, further comprises:
[0018] Acid etching is performed on the circuit board so that the substrate is etched out from all sides of the circuit board.
[0019] In an optional manner, after the step of performing acid etching on the circuit board so that the substrate is etched out of all sides of the circuit board, the method further includes:
[0020] Prior to solder masking, the circuit board is pickled and sandblasted.
[0021] In an optional manner, the step of inserting the plurality of circuit boards into a rack after the solder mask text, fixing the plurality of circuit boards with a clamping strip, and then baking the boards comprises:
[0022] After the solder mask text is applied, the plurality of circuit boards are inserted into the inserting rack, and at least one clip is used to fix the plurality of circuit boards on the side where the plurality of circuit boards are not in contact with the inserting rack before the boards are baked.
[0023] According to another aspect of an embodiment of the present invention, a circuit board is provided. The circuit board is produced by the above-mentioned circuit board production process for preventing board warping.
[0024] In an optional manner, the circuit board is a touch circuit board.
[0025] In an optional manner, the predetermined threshold is 5%, the predetermined thickness is 2.5 um, and the straightening machine leveling includes first performing hot pressing at 160 degrees Celsius for 90 minutes and then performing cold pressing for 60 minutes.
[0026] In the embodiment of the present invention, the circuit of the circuit board is designed in the design stage, so that the difference in the residual copper rate of the inner symmetrical layer and the difference in the percentage of the copper foil area of the outer symmetrical layer are both less than or equal to a predetermined threshold value; when the inner layer is pressed, a semi-cured sheet is used between the layers for pressing, and the cold pressing time is extended during cold pressing; when the two outer layers are electroplated, vertical continuous electroplating is used and electroplating is performed twice, and after electroplating, the difference in copper plating thickness at the same position of the two outer layers is less than a predetermined thickness; the circuit board is fixed with a clip after the solder mask text and then the board is baked; after the circuit board is formed, if it is detected that the circuit board is warped, it is repeatedly leveled by a straightening machine until the curvature value of the circuit board is within a predetermined range. The straightening machine leveling includes first hot pressing and then cold pressing. Through the above-mentioned production process, the structure of the circuit board can have a high degree of symmetry, and stress can be eliminated in the heating process, especially when heated during assembly, thereby reducing the curvature deformation of the circuit board and improving the qualified rate.
[0027] The above description is only an overview of the technical solution of the embodiment of the present invention. In order to more clearly understand the technical means of the embodiment of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the embodiment of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The accompanying drawings are only used to illustrate the embodiments and are not to be considered as limiting the present invention. In addition, the same reference symbols are used to represent the same components throughout the accompanying drawings. In the accompanying drawings:
[0029] Figure 1 A schematic diagram of a process flow of a circuit board production process for preventing board warping according to an embodiment of the present invention;
[0030] Figure 2 A schematic diagram of points for performing infrared testing according to an embodiment of the present invention. DETAILED DESCRIPTION
[0031] Exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the drawings, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein.
[0032] Figure 1 The flowchart of the circuit board production process for preventing board warping provided by an embodiment of the present invention is shown. The production process of the embodiment of the present invention is applied to multilayer boards with an even number of layers, for example, two-layer boards, four-layer boards, six-layer boards and other multilayer boards. The production process includes circuit board design and circuit board manufacturing. Circuit board manufacturing includes inner layer production, inner layer lamination, drilling and copper plating, outer layer production, outer layer electroplating, etching, solder mask, solder mask text, surface treatment and molding of the circuit board. Among them, the inner layer production, drilling and copper plating, outer layer production, solder mask, solder mask text, surface treatment and molding of the circuit board are basically the same as the existing process. The differences include the following processes, such as Figure 1 As shown:
[0033] Step a: designing the circuit of the circuit board in the design stage so that the difference in residual copper rate of the inner symmetrical layer and the difference in copper foil area percentage of the outer symmetrical layer are both less than or equal to a predetermined threshold.
[0034] In this embodiment, there are multiple pairs of symmetrical layers for a multilayer board with an even number of layers. For example, the outer layers L1 and L4 of a four-layer board are symmetrical layers, and the inner layers L2 and L3 are symmetrical layers. The residual copper rate refers to the percentage of the inner layer circuit pattern to the entire board surface, and the residual copper rate = the area of copper in the current layer / the total area of the board. The copper foil area percentage refers to the area ratio of the copper foil on the surface of the circuit board.
[0035] At present, circuit board manufacturing is generally customized according to drawings. Circuit board manufacturing is not responsible for the layout design of the circuit, which easily leads to a large difference in the copper foil area of the symmetrical layer. Taking a four-layer board as an example, the difference in the percentage of the copper foil area of the two outer symmetrical layers L1 and L4 and the difference in the residual copper rate of the inner symmetrical layers L2 and L3 may be large, making it difficult to ensure that the difference in the copper plating thickness of the symmetrical layer is small during the manufacturing process. This large difference makes it obvious that the circuit board structure is not completely symmetrical. When heated during assembly, the thermal conductivity of copper is very high, about 380W. Therefore, during reflow soldering, the copper surface will quickly conduct heat and expand due to heat. The expansion and contraction of the material will produce stress, causing the circuit board to deform, affecting the functional realization of the product. In the design stage of the circuit board, this embodiment requires that the difference in the residual copper rate of the inner symmetrical layer of the designed circuit board is less than or equal to a predetermined threshold, and the difference in the percentage of the copper foil area of the outer symmetrical layer is also less than or equal to a predetermined threshold. The predetermined threshold can be determined according to the actual needs of the circuit board. Optionally, the predetermined threshold can be 5%. For example, the percentage of the copper foil area of the L1 layer is 50%, then the percentage of the copper foil area of the L4 layer can be designed within the range of 50% ± 5. Of course, the two differences may also be other larger or smaller values.
[0036] By designing the residual copper rate difference of the inner symmetrical layer of the circuit board and the copper foil area percentage difference of the outer symmetrical layer to be less than or equal to a predetermined threshold, the symmetry of the symmetrical layer structure can be improved. When the assembly is heated, the stress generated is also symmetrical, thereby eliminating the stress, and the circuit board will basically not deform or deform very little.
[0037] Optionally, step a includes: if the residual copper rate difference of the inner symmetrical layer or the copper foil area percentage difference of the outer symmetrical layer is greater than a predetermined threshold, the process edge of the inner symmetrical layer or the outer symmetrical layer is increased or decreased until the residual copper rate difference of the inner symmetrical layer and the copper foil area percentage difference of the outer symmetrical layer are both less than or equal to the predetermined threshold.
[0038] The process edge of the circuit board is the copper edge. The process edge is the part added on both sides or four sides of the circuit board. It is mainly used to assist the SMT plug-in welding and board walking, that is, to facilitate the SMT placement machine track to clamp the circuit board and flow through the placement machine. It is not part of the circuit board. The process edge can be adjusted, and each layer has a process edge. In this embodiment, if the residual copper rate difference of the inner symmetrical layer is greater than the predetermined threshold, then during the manufacturing process, that is, side electroplating, the process edge of the inner symmetrical layer is increased or decreased, so that the residual copper rate difference of the inner symmetrical layer is less than or equal to the predetermined threshold, or if the copper foil area percentage difference of the outer symmetrical layer is greater than the predetermined threshold, then during the manufacturing process, that is, side electroplating, the process edge of the outer symmetrical layer is increased or decreased, so that the copper foil area percentage difference of the outer symmetrical layer is less than or equal to the predetermined threshold. In this embodiment, by increasing or decreasing the process edge of the symmetrical layer, the problem of causing deformation caused by the circuit board in the design stage can be solved, and the degree of symmetry of the symmetrical layer structure can be improved, thereby eliminating the corresponding stress.
[0039] Step b: When pressing the inner layer, use a semi-cured sheet between the layers for pressing, and extend the cold pressing time.
[0040] Lamination is to cut the semi-cured sheet into sheets, place them between the inner board and the copper foil, and then use a press with high temperature and high pressure to melt the resin on the semi-cured sheet and fill the copper-free area on the board. After cooling, the resin solidifies and the board and the copper foil are bonded together. In this embodiment, a semi-cured sheet is used between the layers for lamination, which can make the cumulative tolerance small and the laminated structure completely symmetrical, thereby eliminating stress. During lamination, the glass transition temperature corresponding to the circuit board is used for lamination, and the cold pressing time is extended during cold pressing. Extending the cold pressing time can eliminate stress more thoroughly, so that the circuit board will basically not deform or deform less. Among them, the cold pressing time can be selected according to actual needs. Optionally, the cold pressing time can be extended from 60 minutes to 90 minutes.
[0041] Optionally, after step b, the method further includes: after lamination, measuring the board thickness by a multi-point method, and evaluating the thickness uniformity of the circuit board according to the board thickness and a predetermined center value of the board thickness, so as to select a circuit board with uniform thickness.
[0042] In this embodiment, after lamination, the board thickness is measured by a multi-point method. Optionally, the board thickness is measured by a five-point method. The five-point method refers to corresponding points at five positions on the circuit board, including points corresponding to four corners and points corresponding to the middle position. The board thickness is measured at five points, and the thickness uniformity of the circuit board is evaluated based on the measured board thickness data and the predetermined board thickness center value. First, the thickness difference index is calculated based on the board thickness data, and the degree difference index is compared with the predetermined board thickness center value. If the difference between the board thickness data is smaller, the closer the thickness difference index is to the board thickness center value, the better the thickness uniformity of the circuit board is, and vice versa, the worse the thickness uniformity of the circuit board is. In this embodiment, a circuit board whose thickness difference index is closest to the board thickness center value is selected. It can be seen that the higher the symmetry of the lamination, the smaller the difference between the board thickness data, the better the thickness uniformity of the circuit board, and the higher the degree of symmetry of the circuit board, so that stress can be eliminated.
[0043] Step c: When electroplating the two outer layers, vertical continuous electroplating is used and electroplating is performed twice, so that the difference in copper plating thickness at the same position of the two outer layers is less than a predetermined thickness after electroplating.
[0044] Electroplating is the process of transferring positively charged metal ions in a solution to the surface of a conductor at the cathode by direct current. Specifically, copper ions are reduced to copper metal at the cathode, so that the required coating thickness is obtained on the board surface and in the hole. Vertical continuous electroplating is an electroplating process characterized by electroplating the workpiece in a vertical and continuous manner to obtain a uniform and high-quality coating. This embodiment uses vertical continuous electroplating and performs electroplating twice. Control is performed during the electroplating process so that the difference in copper plating thickness at the same position of the two outer layers after electroplating is less than a predetermined thickness, so as to improve the symmetry of the two outer layer structures and facilitate stress elimination. Optionally, the predetermined thickness is 2.5um.
[0045] Optionally, step c includes: using a clamp to clamp one side of the circuit board for a first vertical continuous electroplating, and then clamping the opposite side of the circuit board for a second vertical continuous electroplating, wherein the position of the clamp clamping the circuit board is different each time during the second vertical continuous electroplating, and after electroplating, the difference in copper plating thickness at the same position of the two outer layers is less than a predetermined thickness.
[0046] In this embodiment, a clamp is used to clamp one side of the circuit board for a vertical continuous electroplating, and the electroplating is performed to half the amount or half the time. At this time, the thickness of the circuit board clamping point position is different from that of the non-clamping point position. The clamping point position is not plated with metal because it is clamped, and its thickness is small, while the non-clamping point position is plated with metal because it is not clamped, and its thickness is large. In the second vertical continuous electroplating, the opposite side is clamped for electroplating. In this way, the clamping point position in the first vertical continuous electroplating can be plated with metal in this electroplating, and the clamping point position in this time is also plated with metal in the first vertical continuous electroplating. Therefore, both clamping point positions can be plated with metal, and the difference in metal thickness between the clamping point position and the non-clamping point position is not large. In the prior art, the vertical continuous electroplating is performed once continuously, so the metal thickness difference between the clamping point position and the non-clamping point position is large. In this embodiment, the method of clamping the opposite side for the second vertical continuous electroplating can reduce the difference in metal thickness of the electroplating compared with the prior art, thereby making the circuit board more uniform and conducive to stress elimination.
[0047] Optionally, after step c, the method further includes: performing acid etching on the circuit board so that the substrate is etched out from all sides of the circuit board.
[0048] In this embodiment, the circuit board is plated with positive electroplating, and the positive electroplating needs to be clamped, so there is metal conductive on the edge, that is, there will be metal conductive positions on the edges around, and the substrate will not leak out. When this structure is assembled and heated, the metal heat conduction causes the circuit board to deform. Therefore, the circuit board is acid-etched to etch away the metal around, so that the substrate is etched out on all sides of the circuit board. In this way, there is no metal around, and the circuit board will not be deformed due to metal heat conduction.
[0049] Optionally, after the acid etching of the above embodiment, the method further includes: before solder masking, acid washing and sandblasting the circuit board.
[0050] During the manufacturing process of the circuit board, mechanical stress may be generated due to various factors, which may cause the performance of the circuit board to deteriorate or be damaged. In order to reduce these mechanical stresses, pickling and sandblasting can be used. In this embodiment, before solder masking, the circuit board is pickled and sandblasted to roughen the circuit board with a cleaning agent.
[0051] In the circuit board manufacturing process, pickling can help remove impurities such as oxides on the metal surface by forming salts that dissolve in the acid solution and are removed, thereby improving cleanliness and reducing stress concentration caused by these impurities. Pickling can provide a more uniform surface and help improve the mechanical strength and stability of the circuit board. In this embodiment, 3% to 5% sulfuric acid can be used for pickling.
[0052] In the manufacture of circuit boards, sandblasting focuses on achieving different degrees of surface roughness by replacing abrasives of different particle sizes. Sandblasting can not only improve the adhesion of the circuit board, but also reduce mechanical stress by introducing a certain compressive stress. After sandblasting, the surface of the circuit board will be smoother, reducing the stress concentration caused by the uneven surface. In addition, sandblasting can also remove old coatings, oil stains and other contaminants on the surface to improve the finish. In this embodiment, sandblasting is a high-speed water pressure with corundum in it. The sandblasting speed is slow, and optionally, the speed is 2.0m / min. The corundum collides with the copper surface of the circuit board to clean the copper surface and form a certain degree of roughness on the copper surface.
[0053] This embodiment combines pickling and sandblasting to achieve better results. Pickling is first performed to thoroughly clean the surface of the circuit board, and then sandblasting is performed to improve surface roughness and introduce compressive stress, thereby working together to reduce mechanical stress.
[0054] Step d: inserting the plurality of circuit boards into the rack after the solder mask text, and fixing the plurality of circuit boards with clamp strips before baking the boards.
[0055] Baking the board after the solder mask text can play a curing role. In the prior art, the board is generally baked after the solder mask text is inserted into the rack. For thin boards, this method cannot correct the stress during the heating process, which may cause more and more serious deformation. In this embodiment, after multiple circuit boards are inserted into the rack, the circuit boards are fixed with clips before the boards are baked. Specifically, multiple circuit boards are inserted into the rack after the solder mask text, and at least one clip is used to fix the multiple circuit boards on the side (for example, the top side) where the multiple circuit boards are not in contact with the rack before the boards are baked. In this way, this side of the circuit board will basically not deform when heated during assembly due to the correction of the clip.
[0056] In step e, after the circuit board is formed, if it is detected that the circuit board is warped, the straightening machine is repeatedly performed until the bow value of the circuit board is within a predetermined range, and the straightening machine leveling includes first hot pressing and then cold pressing.
[0057] Straightening machine leveling is to level the circuit board by adjusting mechanical pressure and controlling temperature, using the principle of plastic deformation of the material. In this embodiment, after the circuit board is formed, an infrared board warpage inspection machine is used to inspect the front and back of the circuit board. If the circuit board is found to be warped, straightening machine leveling is performed until the bow value of the circuit board is within a predetermined range. Optionally, the bow value is less than 0.5% and is considered to meet the standard. Otherwise, straightening machine leveling is performed again. Optionally, the straightening machine leveling of this embodiment includes first performing hot pressing at 160 degrees Celsius for 90 minutes and then cold pressing for 60 minutes.
[0058] In this embodiment, the circuit board produced according to the above production process is as follows: Figure 2 As shown, Figure 2 This is a schematic diagram of the points for infrared testing of an embodiment of the present invention. The infrared test can be performed using a six-point method of upper left 1, upper middle 2, upper right 3, lower left 4, lower middle 5 and lower right 6. Taking the lower right point as a reference, other points are compared with the reference point to obtain the height difference. A height difference of <0.47mm is qualified.
[0059] Compared with the prior art, the embodiment of the present invention designs the circuit of the circuit board in the design stage so that the difference in the residual copper rate of the inner symmetrical layer and the difference in the percentage of the copper foil area of the outer symmetrical layer are both less than or equal to a predetermined threshold value; when the inner layer is pressed, a semi-cured sheet is used between the layers for pressing, and the cold pressing time is extended during cold pressing; when the two outer layers are electroplated, vertical continuous electroplating is used and electroplating is performed twice, and after electroplating, the difference in copper plating thickness at the same position of the two outer layers is less than a predetermined thickness; the circuit board is fixed with a clip after the solder mask text and then the board is baked; after the circuit board is formed, if it is detected that the circuit board is warped, it is repeatedly leveled by a straightening machine until the bow value of the circuit board is within a predetermined range. The straightening machine leveling includes first hot pressing and then cold pressing. Through the above-mentioned production process, the structure of the circuit board can have a high degree of symmetry, and stress can be eliminated in the heating process, especially when heated during assembly, thereby reducing the bow deformation of the circuit board and improving the qualified rate.
[0060] The embodiment of the present invention provides a circuit board, which is a circuit board produced by the above-mentioned circuit board production process for preventing board warping. Optionally, the circuit board is a touch circuit board, which is a thin and small circuit board with high requirements for board deformation. It needs to meet the smaller deformation of the board so as to realize the corresponding function after being assembled on the touch device. Optionally, for the touch circuit board, the difference in the residual copper rate of the inner symmetrical layer and the difference in the percentage of the copper foil area of the outer symmetrical layer are both less than or equal to 5%, and the difference in the copper plating thickness at the same position of the two outer layers is less than 2.5um after electroplating, and the straightening machine is first hot-pressed at 160 degrees Celsius for 90 minutes and then cold-pressed for 60 minutes. The touch circuit board produced by the above-mentioned production process can make the structure of the touch circuit board have a high degree of symmetry, and can eliminate stress in the heating process, especially when heated during assembly, thereby reducing the bow deformation of the circuit board. Compared with the existing production process, the bow deformation of the touch circuit board after assembly is very small, basically within 0.5%, which greatly improves the qualified rate, and the qualified rate reaches more than 99%, and at the same time, it can greatly reduce the correction operation after assembly.
[0061] In the description provided herein, a large number of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. In some instances, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this description.
[0062] Similarly, it should be understood that in order to streamline the present invention and aid in understanding one or more of the various inventive aspects, in the above description of exemplary embodiments of the present invention, various features of the embodiments of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, this method of disclosure should not be interpreted as reflecting an intention that the claimed invention requires more features than those expressly recited in each claim.
[0063] Those skilled in the art will appreciate that the modules in the computer device in the embodiment can be adaptively changed and set in one or more computer devices different from the embodiment. The modules or units or components in the embodiment can be combined into one module or unit or component, and they can be divided into multiple sub-modules or sub-units or sub-components. Except that at least some of such features and / or processes or units are mutually exclusive, all features disclosed in this specification (including the accompanying claims, abstracts and drawings) and all processes or units of any method or computer device disclosed in this manner can be combined in any combination. Unless otherwise explicitly stated, each feature disclosed in this specification (including the accompanying claims, abstracts and drawings) can be replaced by an alternative feature that provides the same, equivalent or similar purpose.
[0064] It should be noted that the above embodiments illustrate the present invention rather than limit it, and that those skilled in the art may devise alternative embodiments without departing from the scope of the appended claims. In the claims, any reference symbol between brackets shall not be construed as a limitation on the claims. The word "comprising" does not exclude the presence of elements or steps not listed in the claims. The word "one" or "an" preceding an element does not exclude the presence of a plurality of such elements. The present invention may be implemented by means of hardware comprising a number of different elements and by means of a suitably programmed computer. In a unit claim enumerating a number of devices, several of these devices may be embodied by the same hardware item. The use of the words first, second, and third, etc. does not indicate any order. These words may be interpreted as names. The steps in the above embodiments, unless otherwise specified, should not be understood as limitations on the order of execution.
Claims
1. A circuit board production process for preventing board warping, the production process includes circuit board design and circuit board manufacturing, the circuit board manufacturing includes inner layer production, inner layer lamination, drilling and copper plating, outer layer production, outer layer electroplating, etching, solder mask, solder mask text, surface treatment and molding of the circuit board, Features: Designing the circuit of the circuit board in the design stage so that the difference of the residual copper rate of the inner symmetrical layer and the difference of the percentage of the copper foil area of the outer symmetrical layer are both less than or equal to a predetermined threshold; When laminating the inner layer, use a prepreg sheet between the layers and extend the cold pressing time; When electroplating the two outer layers, vertical continuous electroplating is used and electroplating is performed twice, so that the difference in copper plating thickness at the same position of the two outer layers is less than a predetermined thickness after electroplating; Inserting the plurality of circuit boards on the inserting rack after the solder mask text, and fixing the plurality of circuit boards with clamping strips before baking the boards; After the circuit board is formed, if it is detected that the circuit board is warped, straightening and leveling are repeatedly performed until the bow value of the circuit board is within a predetermined range. The straightening and leveling includes first performing hot pressing and then cold pressing.
2. The circuit board production process for preventing board warping according to claim 1, It is characterized in that The step of designing the circuit of the circuit board in the design stage so that the difference in residual copper rate of the inner symmetrical layer and the difference in copper foil area percentage of the outer symmetrical layer are both less than or equal to a predetermined threshold value includes: If the residual copper rate difference of the inner symmetric layer or the copper foil area percentage difference of the outer symmetric layer is greater than a predetermined threshold, the process edge of the inner symmetric layer or the process edge of the outer symmetric layer is increased or decreased.
3. The circuit board production process for preventing board warping according to claim 1, It is characterized in that After the step of laminating the inner layer with a prepreg between the layers and prolonging the cold pressing time during the cold pressing, the method further comprises: After lamination, the board thickness is measured by a multi-point method, and the thickness uniformity of the circuit board is evaluated based on the board thickness and a predetermined center value of the board thickness, so as to select a circuit board with uniform thickness.
4. The circuit board production process for preventing board warping according to claim 1, It is characterized in that When electroplating the two outer layers, vertical continuous electroplating is used and electroplating is performed twice, and the step of making the difference in copper plating thickness at the same position of the two outer layers less than a predetermined thickness after electroplating includes: A clamp is used to clamp one side of the circuit board for a first vertical continuous electroplating, and then the opposite side of the circuit board is clamped for a second vertical continuous electroplating. After electroplating, the difference in copper plating thickness at the same position of the two outer layers is less than a predetermined thickness.
5. The circuit board production process for preventing board warping according to claim 1, It is characterized in that The method further comprises: when electroplating the two outer layers, vertical continuous electroplating is used and electroplating is performed twice, and after electroplating, the difference in copper plating thickness at the same position of the two outer layers is less than a predetermined thickness, and the method further comprises: Acid etching is performed on the circuit board so that the substrate is etched out around the circuit board.
6. The circuit board production process for preventing board warping according to claim 5, It is characterized in that After the step of performing acid etching on the circuit board so that the substrate is etched out of all sides of the circuit board, the method further includes: Prior to solder masking, the circuit board is pickled and sandblasted.
7. The circuit board production process for preventing board warping according to claim 1, It is characterized in that The step of inserting the plurality of circuit boards on the insert rack after the solder mask text, fixing the plurality of circuit boards with a clamping strip, and then baking the boards comprises: After the solder mask text is applied, the plurality of circuit boards are inserted into the inserting rack, and at least one clip is used to fix the plurality of circuit boards on the side where the plurality of circuit boards are not in contact with the inserting rack before the boards are baked.
8. A circuit board, It is characterized in that The circuit board is a circuit board produced by the circuit board production process for preventing board warping according to any one of claims 1 to 7.
9. The circuit board according to claim 8, It is characterized in that The circuit board is a touch circuit board.
10. The circuit board according to claim 9, It is characterized in that The predetermined threshold is 5%, the predetermined thickness is 2.5 um, and the straightening machine leveling includes first performing hot pressing at 160 degrees Celsius for 90 minutes and then performing cold pressing for 60 minutes.