Method for manufacturing silicon-based OLED (Organic Light Emitting Diode) through evaporation and micro display
The preparation of RGB color filter layer through the evaporation process solves the problems of uneven coating and abnormal development in silicon-based OLEDs, improves the color gamut and brightness performance of the display device, and achieves a more accurate and realistic display effect.
Patent Information
- Application Number
- CN202411014010.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The existing silicon-based OLEDs have problems of uneven coating or abnormal development by spin-coating photoresist, which affects the color gamut and brightness performance of the display device.
The RGB color filter layer was prepared by evaporation deposition process, and a monochrome color film layer was prepared by vacuum evaporation, and some color film layers were removed through exposure and development operations to ensure the uniformity and accuracy of the color filter layer.
The uniformity of the RGB color filter layer is improved, the color gamut performance and brightness of the display device are improved, and more accurate and realistic display effects are ensured.
Smart Images

Figure CN118946222A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor display, and in particular relates to a method for manufacturing silicon-based OLED by evaporation and a micro display. Background Art
[0002] At present, the colorization of silicon-based OLED micro-display modules mostly adopts the solution of white light plus color filter (CF), and the brightness is basically within 800cd / ㎡, while more and more products in the market require the brightness to be between 1000cd / ㎡ and 20000cd / ㎡. The existing OLED devices rely on material and device optimization, and the brightness improvement is limited. Moreover, as the brightness increases, the life of the device will also be affected.
[0003] In addition to the above-mentioned CF solution, the silicon-based OLED industry also has a method of making RGB color photoresists through exposure and development of photoresists. However, this silicon-based OLED preparation solution has many limitations. For example, after the photoresist is spin-coated, there will be problems such as uneven coating or abnormal development. The uniformity of photoresist coating is strongly related to performance indicators such as color gamut and brightness of silicon-based OLED display devices. Summary of the invention
[0004] The invention discloses a method for manufacturing silicon-based OLED by evaporation and a micro display, which solves the problem of uneven coating or abnormal development in the existing silicon-based OLED by spin coating photoresist.
[0005] A method for manufacturing a silicon-based OLED by evaporation, comprising the following steps:
[0006] S1, taking a silicon substrate, coating a photoresist on one side thereof to form a photoresist layer;
[0007] S2, performing exposure and development operations on the photoresist layer to prepare an anode pixel structure;
[0008] S3, taking the silicon substrate with the anode pixel structure in step S2, coating the side where the anode pixel structure is located to form an anode metal film layer;
[0009] S4, taking the silicon substrate with the anode metal film layer in step 33, and processing the side where the anode metal film layer is located by an etching process to obtain a pixel definition area;
[0010] S5, transferring the silicon substrate with the pixel definition area in step S4 into the evaporation equipment to sequentially prepare the hole transport layer, hole injection layer, light emitting layer, electron transport layer, and electron injection layer through a high-precision mask plate to complete the deposition preparation of the OLED light emitting layer and functional layer;
[0011] S6, sealing the silicon substrate obtained in step S5 above the OLED light-emitting layer and the functional layer to form a sealing layer;
[0012] S7, preparing a single-color film layer by vacuum evaporation on the silicon substrate after step S6;
[0013] S8, selectively performing exposure and development operations on the silicon substrate obtained by step S7 to remove a portion of the single-color filter layer and retain a designated portion of the single-color filter layer;
[0014] S9, looping through step S7 and step S8 three times to complete the preparation of single-color filter layers corresponding to the three primary colors of RGB, and obtain a color filter pixel layer;
[0015] S10, transferring the silicon substrate with the RGB three primary color film pixel layer in step S9 to a coating device for coating a protective layer to complete the preparation.
[0016] The RGB color filter layer is prepared by vacuum evaporation, and the thickness is controllable and the RGB color filter layer prepared with finer control has better uniformity, which can effectively solve the problem of abnormal development caused by uneven coating of the RGB color filter layer and the problem of poor color gamut performance of the display device derived from the abnormal development.
[0017] Several optional methods are also provided below, but they are not intended to be additional limitations on the above-mentioned overall solution, but are merely further supplements or preferences. Under the premise that there are no technical or logical contradictions, each optional method can be combined with the above-mentioned overall solution separately, and multiple optional methods can also be combined.
[0018] Optionally, the photoresist in step S1 is an AZ type positive photoresist, and the thickness of the photoresist layer is in the range of between.
[0019] Optionally, in the exposure and development operation in step S2, the development time of the photoresist layer after exposure is 20s to 60s, and the Post Bake temperature is 70°C to 200°C.
[0020] Optionally, in step S3, the anode metal film layer is prepared by using a PVD evaporation device or an ion sputtering device, and the thickness of the anode metal film layer is in the range of between.
[0021] Optionally, the anode pixel structure in step S2 has relative convex portions and concave portions, and the concave portions correspond to the pixel definition areas in step S4.
[0022] Optionally, in step S6, the sealing layer includes a first inorganic sealing layer and a second inorganic sealing layer, the first inorganic sealing layer is atomic-level sealing, and the second inorganic sealing layer is molecular-level sealing.
[0023] Optionally, the single-color filter layer in step S7 includes a red filter layer, a blue filter layer, and a green filter layer.
[0024] Optionally, the thickness of the red filter layer is in the range of The thickness of the blue filter layer ranges from The thickness of the green filter layer ranges from between.
[0025] Optionally, the red filter layer is made by evaporating one of copper phthalocyanine, acridine orange, phenanthroline, and hepazolide dyes, the blue filter layer is made by evaporating isophenanthroline dyes, and the green filter layer is made by evaporating isophenanthroline dyes.
[0026] The present application also discloses a micro display, which uses the silicon-based OLED made by the above-mentioned method of making silicon-based OLED by evaporation as a display module.
[0027] The beneficial effects of this application are as follows:
[0028] 1. The evaporation process can achieve high photoresist accuracy and has angstrom and nanometer evaporation accuracy control, laying the foundation for product color gamut and resolution performance;
[0029] 2. Evaporation to produce the RGB color filter layer can effectively ensure the uniformity of the RGB color filter layer, making the display effect more accurate and realistic, and making the RGB color filter layer restore the required color range. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a schematic diagram of the structure of the silicon substrate and the photoresist layer in step S1 of this application;
[0031] Figure 2 This is a schematic structural diagram of a silicon substrate with an anode pixel structure in step S2 of the present application;
[0032] Figure 3 This is a schematic structural diagram of a silicon substrate with an anode metal film layer in step S3 of the present application;
[0033] Figure 4 This is a schematic structural diagram of a silicon substrate with a pixel definition area in step S4 of the present application;
[0034] Figure 5 This is a schematic diagram of the structure of the silicon substrate after the evaporation and sealing in step S5 and step S6 of the present application;
[0035] Figure 6 This is a schematic structural diagram of a silicon substrate on which a single-color film layer is evaporated in step S7 of the present application;
[0036] Figure 7 This is a schematic diagram of the structure of the silicon-based OLED in this application.
[0037] The reference numerals in the figures are described as follows:
[0038] 1. Silicon substrate; 2. Photoresist layer; 21. Protrusion; 22. Concave portion; 3. Anode metal film layer; 31. Pixel definition area; 41. First inorganic sealing layer; 42. Second inorganic sealing layer; 5. Monochrome color film layer; 51. Red pixel; 52. Blue pixel; 53. Green pixel; 6. Protective layer. DETAILED DESCRIPTION
[0039] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0040] It should be noted that when a component is referred to as being "connected" to another component, it may be directly connected to the other component or there may be a central component. When a component is referred to as being "disposed on" another component, it may be directly disposed on the other component or there may be a central component at the same time.
[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0042] In one embodiment of the present application, a method for manufacturing a silicon-based OLED by evaporation is disclosed, comprising the following steps:
[0043] S1, taking a silicon substrate, coating a photoresist on one side thereof to form a photoresist layer;
[0044] refer to Figure 1 , a photoresist layer 2 is located above a silicon substrate 1, wherein the silicon substrate 1 has a CMOS driving circuit and a tungsten plug.
[0045] S2, performing exposure and development operations on the photoresist layer to prepare an anode pixel structure;
[0046] refer to Figure 2 The anode pixel structure is made by exposing and developing the photoresist layer, and has a relative convex portion 21 and a concave portion 22, and the concave portion 22 corresponds to a pixel point.
[0047] S3, take the silicon substrate with the anode pixel structure in step S2, and perform film coating on the side where the anode pixel structure is located to form an anode metal film layer 3 (such as Figure 3 shown);
[0048] S4, taking the silicon substrate with the anode metal film layer in step 33, and processing the side where the anode metal film layer is located by an etching process to obtain a pixel definition area;
[0049] refer to Figure 4 , the side where the anode metal film layer 3 is located is processed by an etching process, and the anode metal film layer 3 corresponding to the concave portion 22 is retained, thereby obtaining a pixel definition area 31.
[0050] S5, transferring the silicon substrate with the pixel definition area in step S4 into the evaporation equipment to sequentially prepare the hole transport layer, hole injection layer, light emitting layer, electron transport layer, and electron injection layer through a high-precision mask plate to complete the deposition preparation of the OLED light emitting layer and functional layer;
[0051] S6, sealing the silicon substrate obtained in step S5 above the OLED light-emitting layer and the functional layer to form a sealing layer;
[0052] S7, preparing a single-color film layer 5 by vacuum evaporation on the silicon substrate after step S6;
[0053] S8, selectively performing exposure and development operations on the silicon substrate obtained by step S7 to remove a portion of the single-color filter layer and retain a designated portion of the single-color filter layer;
[0054] S9, looping through step S7 and step S8 three times to complete the preparation of single-color filter layers corresponding to the three primary colors of RGB, and obtain a color filter pixel layer;
[0055] S10, transferring the silicon substrate with the RGB three primary color film pixel layer in step S9 to a coating device for coating a protective layer to complete the preparation.
[0056] The anode pixel structure in step S2 has a convex portion and a concave portion opposite to each other, and the concave portion corresponds to the pixel definition area in step S4.
[0057] refer to Figure 6 and Figure 7 The steps S7 to S9 can be understood as performing multiple evaporation deposition on the silicon substrate according to the three primary colors of RGB, and the single-color film layer 5 can be one of red, green and blue.
[0058] For example, a red monochrome color film layer 5 is first prepared by vacuum evaporation, and after the red monochrome color film layer 5 is completed, some pixels are removed by exposure and development operations, and local red pixels 51 are retained; then a blue monochrome color film layer 5 is prepared by vacuum evaporation again, and after the blue monochrome color film layer 5 is completed, some pixels are removed by exposure and development operations, and local blue pixels 52 are retained; finally, a green monochrome color film layer 5 is prepared by vacuum evaporation, and after the green monochrome color film layer 5 is completed, some pixels are removed by exposure and development operations, and local green pixels 53 are retained.
[0059] The color filter pixel layer is composed of the red pixel points 51 , the blue pixel points 52 , and the green pixel points 53 .
[0060] In the art, the red pixel points, blue pixel points, and green pixel points are generally referred to as RGB photoresists.
[0061] Furthermore, in the present application, the anode pixel structure on one side of the silicon substrate is evaporated by CF RGB monochrome full-surface evaporation, and the CF color film layer is prepared by vacuum evaporation, which can achieve the advantages of high precision, high color gamut, high resolution controllability, etc. of the display device, and solve the problem of uneven coating on the edge of the wafer due to the traditional spin coating process affecting the color gamut of the display device.
[0062] The evaporation process can achieve a tiny 0.1um~5umCD size RGB photoresist pattern (i.e. the size of the above-mentioned pixel points), making electronic devices more compact and thinner. The use of evaporation to make RGB photoresist can achieve micron-level pattern size control, meeting the needs of high resolution and compact design.
[0063] Furthermore, the single-color filter layer in step S7 includes a red filter layer, a blue filter layer, and a green filter layer.
[0064] In one embodiment, the thickness of the red filter layer is The thickness of the blue filter layer is The thickness of the green filter layer is
[0065] In another embodiment, the thickness of the red filter layer is The thickness of the blue filter layer Thickness of green filter layer
[0066] In another embodiment, the thickness of the red filter layer is The thickness of the blue filter layer is The thickness of the green filter layer is
[0067] The red filter layer is made by evaporating one of copper phthalocyanine, acridine orange, phenanthroline and hepazolide dyes, the blue filter layer is made by evaporating isophenanthroline dyes, and the green filter layer is made by evaporating isophenanthroline dyes.
[0068] In some embodiments, the photoresist in step S1 is AZ type positive photoresist.
[0069] In one embodiment, the thickness of the photoresist layer is
[0070] In the exposure and development operation in step S2, the development time of the photoresist layer after exposure is 20 seconds, and the Post Bake temperature is 70°C.
[0071] In another embodiment, the thickness of the photoresist layer is
[0072] In the exposure and development operation in step S2, the development time of the photoresist layer after exposure is 40s, and the Post Bake temperature is 130°C.
[0073] In another embodiment, the thickness of the photoresist layer is
[0074] In the exposure and development operation in step S2, the development time of the photoresist layer after exposure is 60s, and the Post Bake temperature is 7200°C.
[0075] In some embodiments, the anode metal film layer in step S3 is prepared by using a PVD evaporation device or an ion sputtering device, and the thickness of the anode metal film layer is in the range of between.
[0076] Preferably, the thickness of the anode metal film layer is or or
[0077] Furthermore, the material for preparing the anode metal film layer may be selected from transparent conductive oxide (TCO) materials, tin oxide (SnO2), indium tin oxide (ITO, containing indium-doped SnO2), zinc oxide (ZnO), and the like.
[0078] refer to Figure 5 In some embodiments, the sealing layer in step S6 includes a first inorganic sealing layer 41 and a second inorganic sealing layer 42, the first inorganic sealing layer 41 is an atomic-level seal, and the second inorganic sealing layer 42 is a molecular-level seal, for providing better sealing.
[0079] In some embodiments, the silicon substrate with the color filter pixel layer prepared in step SS9 can be exposed and developed to remove the redundant part first, and then the protective layer 6 can be coated in step S10.
[0080] Furthermore, a transparent resin polymer can be selected as the raw material of the protective layer 6, and the protective layer 6 can be obtained by baking and curing, so that the protective layer 6 has better waterproof performance.
[0081] The present application also discloses a micro display, which uses the silicon-based OLED made by the above-mentioned method of making silicon-based OLED by evaporation as a display module.
[0082] In addition to the above contents, this application also has the following beneficial effects:
[0083] Process reliability: Evaporation is a mature process technology with high reliability and stability.
[0084] Better cost-effectiveness: RGB photoresist produced by evaporation has low cost, can achieve efficient photoresist production, reduce the waste of materials and energy, and can achieve mass production.
[0085] The technical features of the above-mentioned embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. When the technical features in different embodiments are embodied in the same figure, it can be regarded that the figure also discloses the combination examples of the various embodiments involved.
[0086] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application.
Claims
1. A method for producing a silicon-based OLED by evaporation, characterized in that: The following steps are involved: S1, taking a silicon substrate, coating a photoresist on one side thereof to form a photoresist layer; S2, performing exposure and development operations on the photoresist layer to prepare an anode pixel structure; S3, taking the silicon substrate with the anode pixel structure in step S2, coating the side where the anode pixel structure is located to form an anode metal film layer; S4, taking the silicon substrate with the anode metal film layer in step 33, and processing the side where the anode metal film layer is located by an etching process to obtain a pixel definition area; S5, transferring the silicon substrate with the pixel definition area in step S4 into the evaporation equipment to sequentially prepare the hole transport layer, hole injection layer, light emitting layer, electron transport layer, and electron injection layer through a high-precision mask plate to complete the deposition preparation of the OLED light emitting layer and functional layer; S6, sealing the silicon substrate obtained in step S5 above the OLED light-emitting layer and the functional layer to form a sealing layer; S7, preparing a single-color film layer by vacuum evaporation on the silicon substrate after step S6; S8, selectively performing exposure and development operations on the silicon substrate obtained by step S7 to remove a portion of the single-color filter layer and retain a designated portion of the single-color filter layer; S9, looping through step S7 and step S8 three times to complete the preparation of single-color filter layers corresponding to the three primary colors of RGB, and obtain a color filter pixel layer; S10, transferring the silicon substrate with the RGB three primary color film pixel layer in step S9 to a coating device for coating a protective layer to complete the preparation.
2. The method for manufacturing a silicon-based OLED by evaporation according to claim 1, characterized in that: In step S1, the photoresist is an AZ type positive photoresist, and the thickness of the photoresist layer is in the range of between.
3. The method for manufacturing silicon-based OLED by evaporation according to claim 1, characterized in that: In the exposure and development operation in step S2, the photoresist layer is developed for 20s to 60s after exposure, and the post bake temperature is 70°C to 200°C.
4. The method for manufacturing silicon-based OLED by evaporation according to claim 1, characterized in that: In step S3, the anode metal film layer is prepared by using a PVD evaporation device or an ion sputtering device, and the thickness of the anode metal film layer is in the range of between.
5. The method for manufacturing silicon-based OLED by evaporation according to claim 1, characterized in that: The anode pixel structure in step S2 has a convex portion and a concave portion opposite to each other, and the concave portion corresponds to the pixel definition area in step S4.
6. The method for manufacturing silicon-based OLED by evaporation according to claim 1, characterized in that: In the step S6, the sealing layer includes a first inorganic sealing layer and a second inorganic sealing layer, wherein the first inorganic sealing layer is atomic-level sealing and the second inorganic sealing layer is molecular-level sealing.
7. The method for manufacturing silicon-based OLED by evaporation according to claim 1, characterized in that: The single-color filter layer in step S7 includes a red filter layer, a blue filter layer, and a green filter layer.
8. The method for manufacturing silicon-based OLED by evaporation according to claim 7, characterized in that: The thickness of the red filter layer is in the range of The thickness of the blue filter layer ranges from The thickness of the green filter layer ranges from between.
9. The method for manufacturing silicon-based OLED by evaporation according to claim 8, characterized in that: The red filter layer is made by evaporating one of copper phthalocyanine, acridine orange, phenanthroline and hepazolide dyes, the blue filter layer is made by evaporating isophenanthroline dyes, and the green filter layer is made by evaporating isophenanthroline dyes.
10. A micro display, characterized in that: The silicon-based OLED manufactured by the method for manufacturing silicon-based OLED by evaporation as claimed in claim 1 is used as a display module.