Flexible perovskite solar cell
By integrating graphene nanomesh in flexible perovskite solar cells, optimizing the stability of electron transport layer and interface, the shortcomings in efficiency, stability and mechanical adaptability of flexible perovskite batteries are solved, and high efficiency and long-term reliability are achieved The photoelectric conversion performance and environmental adaptability are suitable for the development of efficient, lightweight, and flexible photovoltaic modules.
Patent Information
- Application Number
- CN202411006539.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
Existing flexible perovskite solar cells have shortcomings in efficiency, long-term stability and mechanical adaptability, especially under extreme environments and repeated stresses, and their environmental adaptability is not sufficient.
Integrate graphene nanomesh into polyethylene terephthalate or polyethylene naphthalate flexible substrates to optimize the performance of electron transport layer and the perovskite/substrate interface stability, and prepare graphite by chemical vapor deposition method The ene reinforced substrate is combined with spin coating and annealing to form a reinforced structure.
It significantly improves the photoelectric conversion efficiency, ensures high stability and mechanical durability under extreme conditions. The photoelectric conversion efficiency of the battery remains above 97% after 10,000 bends, and the efficiency decreases by no more than 2% in high temperature and high humidity environments. At the same time, light transmittance is optimized and energy consumption is reduced.
Smart Images

Figure CN118946226A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of flexible solar cells, and in particular relates to a flexible perovskite solar cell. Background Art
[0002] The prior art discloses two landmark research results in the field of flexible perovskite solar cells (FPSCs), which not only lay the foundation for our research, but also reveal the difficulties that need to be overcome by current technology.
[0003] First, "Multifunctional succinate additive for flexible perovskite solar cells with more than 23% power-conversion efficiency" was published by relevant scholars. The study focused on solving the problems of uneven film formation and defect accumulation of the charge transfer layer (CTL) caused by the roughness of the flexible substrate during the preparation of FPSCs. By optimizing the film formation process, the study improved the deposition uniformity on the flexible substrate to a certain extent, but failed to solve the problem of battery performance improvement and long-term stability from the essence of the material. Although these achievements have promoted the advancement of FPSCs manufacturing technology, they have failed to fully address key challenges such as efficiency attenuation and insufficient environmental adaptability encountered in practical applications.
[0004] Secondly, in "Multifunctional entinostat enhances the mechanical robustness and efficiency of flexible perovskite solar cells and minimodules", a multifunctional organic molecule called entinostat was introduced to successfully enhance the mechanical strength and photoelectric conversion efficiency of FPSCs. By integrating entinostat into the hole transport layer, not only the interfacial adhesion between the perovskite layer and the substrate was strengthened and the pores at the bottom of the substrate were reduced, but also the key performance indicators of the battery, such as open circuit voltage, short circuit current density and fill factor, were significantly improved through advanced passivation strategies. Although this study has made significant achievements in improving the environmental adaptability and long-term stability of batteries, it still highlights the need to further improve battery stability under extreme conditions such as high temperature and humidity, temperature cycling and continuous light. Summary of the invention
[0005] The purpose of the present invention is to provide a flexible perovskite solar cell, which belongs to the intersection of flexible electronic devices and advanced materials science, and aims to integrate a graphene nano-mesh reinforcement structure in a traditional polyethylene terephthalate (PET) or polyethylene naphthalate (PEN) flexible substrate, optimize the performance of the electron transport layer and the stability of the perovskite / substrate interface, thereby greatly improving the photoelectric conversion efficiency and long-term working reliability of the flexible perovskite solar cell. The flexible perovskite solar cell can be directly applied to the development of efficient, lightweight, and bendable photovoltaic modules, and is particularly suitable for scenes that require high flexibility, high energy efficiency, and strong environmental adaptability, such as wearable electronics, portable devices, and photovoltaic building integration (BIPV).
[0006] The present invention is achieved through the following technical solutions:
[0007] A flexible perovskite solar cell is produced by integrating a graphene nanonet in a polyethylene terephthalate or polyethylene naphthalate flexible substrate to obtain an enhanced structure.
[0008] Preferably, the method comprises a flexible substrate bottom layer, an electron transport layer, a perovskite layer, a passivation layer, a hole transport layer and a metal back electrode layer arranged in sequence, wherein the flexible substrate bottom layer is a graphene nanomesh reinforced flexible substrate bottom layer.
[0009] A method for preparing a flexible perovskite solar cell comprises the following steps:
[0010] S1. Graphene nanomesh reinforced flexible substrate bottom layer:
[0011] A single-layer graphene sheet is prepared by chemical vapor deposition, polyvinyl alcohol is added as a dispersant in ethanol with a mass fraction of 90 to 95%, and ultrasonic treatment is performed to uniformly disperse the graphene to obtain a graphene-ethanol dispersion;
[0012] After the obtained graphene-ethanol dispersion is coated into a uniform coating, it is applied on a polyethylene terephthalate or polyethylene naphthalate flexible substrate, and after hot pressing curing and annealing, the preparation of the graphene nano-mesh reinforced flexible substrate bottom layer is completed;
[0013] S2, hole transport layer:
[0014] After selecting a fullerene derivative and dissolving it in a chlorobenzene solvent, the fullerene derivative is spin-coated on the bottom layer of the graphene nano-mesh reinforced flexible substrate, and annealed and cured to complete the preparation of the hole transport layer;
[0015] S3, Perovskite layer:
[0016] Preparation of perovskite precursor solution: Lead iodide, formamidine iodide, methylamine bromide, lead bromide, cesium iodide and methyl iodide were selected according to the corresponding weight parts, mixed and dissolved in an organic solvent, and stirred at room temperature to obtain a molar concentration of 1.6 M (FAPbI 3 ) 0.93 (MAPbBr 3 ) 0.05 (CsPbI 3 ) 0.02 Perovskite solution;
[0017] First, a perovskite precursor solution is dripped onto the hole transport layer prepared by S2, and the solution is rotated at 1000 rpm for 10 to 13 seconds, and then at 4500 rpm for 30 to 35 seconds; 18 to 20 seconds before the end of the rotation at 4500 rpm, an anti-solvent is dripped and spin-coated, and then annealing is performed to complete the preparation of the perovskite layer;
[0018] S4, passivation layer:
[0019] A phenethylammonium iodide solution is prepared by selecting phenethylammonium iodide, and the solution is spin-coated on the perovskite layer prepared in S3, and annealed and solidified to complete the preparation of the passivation layer;
[0020] S5, electron transport layer:
[0021] A tin dioxide solution containing potassium chloride is spin-coated on the passivation layer prepared by S4, and annealed and cured to complete the preparation of the electron transport layer;
[0022] S6, metal back electrode layer:
[0023] Gold is evaporated and deposited on the electron transport layer by physical vapor deposition as the back electrode to complete the preparation of the battery.
[0024] Preferably, in S1, the graphene concentration in the graphene-ethanol dispersion is 0.1-0.2 mg / mL;
[0025] Ultrasonic treatment for 30-35 min;
[0026] Hot pressing curing treatment at 100-120°C and 0.5Mpa for 20-25 minutes;
[0027] Annealing is carried out at 130-150°C for 1-1.2h.
[0028] Preferably, in S2, the mass concentration of the fullerene derivative is 18-20 mg / mL;
[0029] The spin coating lasts for 28 to 30 seconds at a rotation speed of 4000 rpm, followed by annealing at 80-100° C. for 30 to 35 minutes for curing.
[0030] Preferably, in S3, the weight ratio of each raw material is lead iodide: formamidine iodide: methylamine bromide: lead bromide: cesium iodide: methyl iodide = 735.756 mg, 255.8 mg, 8.95 mg, 29.36 mg, 8.31 mg, 27 mg;
[0031] The organic solvent is prepared by mixing N,N-dimethylformamide and dimethyl sulfoxide in a volume ratio of 4:1.
[0032] Preferably, the anti-solvent is chlorobenzene;
[0033] The stirring time at room temperature is 2 to 2.5 hours;
[0034] The annealing treatment is performed at 100-150° C. for 20-25 minutes.
[0035] Preferably, in S4, the spin coating is continued for 28 to 30 seconds at a rotation speed of 4000 to 4500 rpm, followed by annealing at 80 to 100° C. for 5 to 6 minutes for curing.
[0036] Preferably, in said S5, the content of potassium chloride in the tin dioxide solution containing potassium chloride is 0.5wt% to 3wt%;
[0037] The curing treatment is performed by annealing at 100-120° C. for 18-20 minutes.
[0038] Preferably, in S6, the thickness of the gold electrode is 100 nm.
[0039] Compared with the prior art, the present invention has at least the following technical effects:
[0040] The present invention provides a method for preparing a flexible perovskite solar cell, which aims to break through the limitations of existing flexible perovskite solar cell technology by innovatively incorporating a carefully designed graphene nanomesh structure into a PET / PEN flexible substrate to achieve unprecedented performance improvement and enhanced environmental adaptability.
[0041] Compared with traditional flexible perovskite cells and existing technologies, the preparation method of this flexible perovskite solar cell has the following significant performance improvements and advantages:
[0042] 1. Significantly improve the photoelectric conversion efficiency: Through the optimized integration of graphene nanonets, the experiment verified that the flexible perovskite solar cell of the present invention can achieve a photoelectric conversion efficiency of 23.73%. Compared with similar cells without graphene enhancement, this value represents a significant performance improvement. Combining theory with practice, the high conductivity and unique two-dimensional structure of graphene effectively promote the rapid transmission of electrons, while the optimized interfacial adhesion reduces the loss of charge during the transmission process, thereby significantly improving the overall efficiency of the battery. This marks a major leap compared to the existing technology level and lays a solid foundation for high-efficiency photovoltaic applications. Ensure high stability under extreme conditions: After 10,000 bending tests and facing extreme environmental challenges such as high temperature and high humidity, the battery of the present invention can still maintain an initial photoelectric conversion efficiency of more than 97%, demonstrating its excellent performance in mechanical stability and environmental adaptability, and providing the possibility for the long-term reliable use of flexible electronic products.
[0043] 2. Enhance the service life and reliability of the battery: The introduction of graphene effectively enhances the durability and life of the battery, solves the problem of performance degradation of flexible perovskite batteries under repeated stress, and meets the high standards for long-term stability and reliability. After 10,000 bending tests, the photoelectric conversion efficiency of the battery can still be maintained at more than 97%, indicating that the graphene-enhanced substrate plays a decisive role in improving the mechanical stability and long-term durability of the battery. Compared with traditional flexible perovskite batteries, this data shows superior mechanical adaptability and broadens the possibilities for the application of flexible electronic devices.
[0044] 3. Excellent environmental adaptability: Under high temperature and high humidity environment for 1,000 consecutive hours, the photoelectric conversion efficiency of the battery only dropped by less than 2%, indicating that the stability of the present invention under extreme climatic conditions far exceeds that of the existing technology. This is due to the excellent isolation performance of the graphene substrate against environmental factors and the optimized passivation strategy of the perovskite layer.
[0045] 4. Optimized light transmittance and reduced energy consumption: The graphene nano-mesh enhanced substrate has minimal effect on light absorption while maintaining high transparency. Transmission spectrum test shows that the light transmittance of the enhanced substrate is no more than 5% lower than that of the unenhanced substrate. This means that under the same lighting conditions, the battery can use light more effectively, thereby reducing energy consumption and improving energy conversion efficiency.
[0046] 5. Potential for promoting commercial applications: Through experimental data and verification of actual application environments, the graphene-enhanced flexible perovskite solar cells of the present invention have not only achieved breakthroughs in performance, but also demonstrated high stability and reliability in practical applications. These significant improvements pave the way for the commercialization of flexible photovoltaic technology, especially in the fields of wearable devices, portable electronic devices, and photovoltaic building integration.
[0047] In summary, the present invention successfully solves the key problems of flexible perovskite solar cells in terms of efficiency, stability and mechanical adaptability through the innovative application of graphene nanomesh, providing strong technical support for promoting scientific and technological progress and practical applications in this field. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 Schematic diagram of the interlayer structure of the experimental example flexible perovskite solar cell. DETAILED DESCRIPTION
[0049] The embodiments of the present invention will be described in detail below in conjunction with examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.
[0050] Experimental Example 1: Preparation and Characterization of Graphene Nanomesh Reinforced PET / PEN Substrate
[0051] 1. Experimental materials:
[0052] (1) Polyethylene terephthalate (PET) or polyethylene naphthalate (PEN) film
[0053] (2) Single-layer graphene nanosheets (commercial or laboratory-made. Laboratory-made ones need to follow the following steps)
[0054] (3) Ethanol (analytical grade)
[0055] (4) Polyvinyl alcohol (PVA, molecular weight about 10,000)
[0056] (5) Boric acid buffer solution (pH 8.5)
[0057] (6) Ultrasonic cleaning equipment
[0058] (7) Coating machine
[0059] (8) Heat press
[0060] 2. Steps for making graphene nanosheets:
[0061] Chemical vapor deposition (CVD) method: At high temperature, a carbon source gas (such as methane) is passed into a reaction chamber equipped with copper foil. The carbon source is catalytically cracked on the copper surface to form a graphene layer. After the reaction is completed, the copper substrate is removed by chemical methods to obtain a single-layer graphene sheet.
[0062] Dispersion: The obtained graphene sheets were dispersed in ethanol, and an appropriate amount of polyvinyl alcohol was added as a dispersant. Ultrasonic treatment was performed for 30 minutes to ensure that the graphene was evenly dispersed and to avoid agglomeration.
[0063] 3. Experimental steps:
[0064] (1) Pretreatment of flexible substrate: Clean the surface of PET / PEN film to remove impurities and grease, use ethanol ultrasonic cleaning and dry it for later use.
[0065] (2) Graphene nanomesh coating: The graphene-ethanol dispersion was evenly coated on the PET / PEN substrate, and the coating speed and thickness were controlled by a coating machine to ensure uniform coverage of the graphene, followed by natural drying at room temperature or hot pressing and curing in a hot press at a temperature of 120 °C and a pressure of 0.5 MPa for 20 min.
[0066] (3) Post-treatment of graphene nanomesh-enhanced substrate: Heat treatment is performed to enhance the bonding between graphene and the substrate. The coated sample is annealed at 150°C for 1 hour under vacuum or inert gas protection to enhance the interfacial adhesion.
[0067] 4. Experimental parameters:
[0068] (1) Graphene nanosheet concentration: 0.1 mg / mL
[0069] (2) Coating speed: 20m / min
[0070] (3) Hot pressing temperature: 120℃
[0071] (4) Hot pressing time: 20 minutes
[0072] (5) Annealing temperature: 150°C
[0073] (6) Annealing time: 1h
[0074] 5. Experimental results:
[0075] (1) Microstructure characterization: SEM (scanning electron microscope) observation confirmed that the graphene nanomesh formed a continuous and uniform network structure on the PET / PEN substrate without obvious agglomeration, which proved the good dispersion and uniform coating of graphene.
[0076] (2) Interface adhesion test: The tensile peeling test showed that the adhesion between the graphene-reinforced substrate and the subsequently deposited electron transport layer was increased by about 30% compared with the unreinforced substrate, indicating that graphene effectively enhanced the interface bonding force.
[0077] (3) Optical transmittance: The transmission spectrum test shows that the transmittance of the graphene nanomesh-enhanced PET / PEN substrate in the visible light region decreases by less than 5% compared with the unenhanced substrate, ensuring sufficient light penetration and having little effect on the light absorption of the battery.
[0078] In summary, through the above preparation method, a uniformly distributed graphene nanomesh structure was successfully constructed on the PET / PEN substrate, which significantly enhanced the mechanical properties and interfacial adhesion of the substrate, laying a good foundation for the subsequent deposition of the perovskite layer.
[0079] Experimental Example 2: Preparation and performance testing of graphene-enhanced flexible perovskite solar cells
[0080] 1. Experimental materials:
[0081] (1) Graphene-enhanced PET / PEN substrate (same as in Experimental Example 1)
[0082] (2) Fullerene derivatives (PCBM) as hole transport layer materials
[0083] (3) Perovskite precursor solution (lead iodide, formamidine iodide, methylamine bromide, lead bromide, cesium iodide and methyl iodide were selected according to the corresponding weight parts and mixed and dissolved in an organic solvent, and stirred at room temperature to obtain a molar concentration of 1.6 M (FAPbI 3 ) 0.93 (MAPbBr 3 ) 0.05 (CsPbI 3 ) 0.02 Perovskite solution)
[0084] (4) Passivation layer material (PEAI, phenethylamine iodide)
[0085] (5) Electron transport layer materials
[0086] (6) Gold (Au) as back electrode
[0087] 2. Experimental steps and parameters:
[0088] S1. Preparation of graphene-enhanced PET / PEN substrate: The graphene-enhanced PET / PEN substrate prepared in Example 1 is used as the flexible substrate.
[0089] S2. Hole transport layer: After dissolving a selected fullerene derivative in chlorobenzene solvent, spin-coat it on the bottom layer of the graphene nanomesh-enhanced flexible substrate, anneal and cure it to complete the preparation of the hole transport layer; the mass concentration of the fullerene derivative is 18-20 mg / mL; at a rotation speed of 4000 rpm, the spin coating lasts for 28-30 seconds, and then anneal at 80-100°C for 30-35 minutes for curing.
[0090] S3, Perovskite layer:
[0091] Preparation of perovskite precursor solution: Lead iodide, formamidine iodide, methylamine bromide, lead bromide, cesium iodide and methyl iodide were selected according to the corresponding weight parts, mixed and dissolved in an organic solvent, and stirred at room temperature to obtain a molar concentration of 1.6 M (FAPbI 3 ) 0.93 (MAPbBr 3 ) 0.05 (CsPbI 3 ) 0.02 Perovskite solution;
[0092] First, a perovskite precursor solution is dripped onto the hole transport layer prepared by S2, and the solution is rotated at 1000 rpm for 10 to 13 seconds, and then at 4500 rpm for 30 to 35 seconds; 18 to 20 seconds before the end of the rotation at 4500 rpm, an anti-solvent is dripped and spin-coated, and then annealing is performed to complete the preparation of the perovskite layer;
[0093] The weight ratio of each raw material is lead iodide: formamidine iodide: methylamine bromide: lead bromide: cesium iodide: methyl iodide = 735.756 mg, 255.8 mg, 8.95 mg, 29.36 mg, 8.31 mg, 27 mg;
[0094] The organic solvent is prepared by mixing N,N-dimethylformamide and dimethyl sulfoxide in a volume ratio of 4:1.
[0095] The anti-solvent is chlorobenzene;
[0096] The stirring time at room temperature is 2 to 2.5 hours;
[0097] The annealing treatment is performed at 100-150° C. for 20-25 min to promote the formation of high-quality perovskite crystals.
[0098] S4, passivation layer:
[0099] A phenethylammonium iodide solution is prepared by selecting phenethylammonium iodide, and the solution is spin-coated on the perovskite layer prepared in S3, annealed and cured to complete the preparation of the passivation layer; the spin coating is continued for 28 to 30 seconds at a rotation speed of 4000 to 4500 rpm, and then annealed at 80 to 100° C. for 5 to 6 minutes for curing to passivate the interface and reduce recombination.
[0100] S5, electron transport layer:
[0101] A tin dioxide solution containing potassium chloride is spin-coated on the passivation layer prepared by S4, and annealed and solidified to complete the preparation of the electron transport layer; the content of potassium chloride in the tin dioxide solution containing potassium chloride is 2wt%;
[0102] The curing treatment is performed by annealing at 100-120° C. for 18-20 minutes.
[0103] S6, metal back electrode layer:
[0104] Gold was evaporated and deposited on the electron transport layer by physical vapor deposition to serve as the back electrode, completing the preparation of the battery. The thickness of the gold electrode was 100 nm.
[0105] 3. Experimental results:
[0106] (1) Morphology and structure characterization: SEM, XRD, AFM and other analytical techniques were used to confirm the uniformity of each layer of material, the crystal quality and the flatness of the interface, especially the high-quality crystallization of the perovskite layer and the good interface contact between the graphene-enhanced substrate and the perovskite layer.
[0107] (2) Photoelectric performance evaluation: Under standard simulated sunlight, the photoelectric conversion efficiency of the test cell reached 23.73%, significantly higher than the control group without graphene-enhanced substrate. The open circuit voltage (Voc), short circuit current density (Jsc) and fill factor (FF) of the cell were significantly improved, showing excellent photoelectric conversion performance.
[0108] (3) Mechanical stability and durability test: After 10,000 bending cycles, the photoelectric conversion efficiency of the battery can still be maintained above 97%, proving the important role of graphene-enhanced substrate in improving the mechanical stability and long-term reliability of the battery.
[0109] Through the above steps, flexible perovskite solar cells based on graphene-enhanced PET / PEN substrate were successfully prepared.
[0110] The experimental results fully demonstrate the remarkable effect of this design in improving battery efficiency, stability and mechanical adaptability.
[0111] Experimental Example 3: Verification of graphene-enhanced flexible perovskite solar cells in actual application environments
[0112] 1. Experimental purpose: To evaluate the working performance and long-term stability of graphene-enhanced flexible perovskite solar cells under simulated actual environmental conditions, including the influence of outdoor lighting, high temperature, high humidity, mechanical bending and other factors.
[0113] 2. Experimental materials and preparation: The graphene-enhanced PET / PEN-based perovskite solar cells successfully prepared in the first two experimental examples were used as experimental objects. No further preparation was required, and the verification phase of the actual application environment was directly entered.
[0114] 3. Experimental steps and parameters:
[0115] 3.1 Outdoor light stability test:
[0116] The batteries were installed on an outdoor test platform, ensuring that they faced south and were exposed to natural sunlight around the clock.
[0117] The photoelectric conversion efficiency of the battery was recorded every day in three time periods: morning, noon, and evening, and the records were continuously recorded for one month to evaluate its long-term light stability.
[0118] Experimental parameters: record daily light intensity, temperature, humidity, as well as the open circuit voltage (Voc), short circuit current (Jsc), fill factor (FF) and photoelectric conversion efficiency (PCE) of the battery.
[0119] 3.2 High temperature and high humidity environment test:
[0120] A constant temperature and humidity chamber was used to simulate the tropical rainforest climate, with the temperature set at 40°C and the relative humidity at 90%.
[0121] Place the battery in the box and run it continuously for 1000 hours, measuring the battery performance parameters every 12 hours.
[0122] Experimental parameters: The constant temperature and humidity chamber was set at (40±1)°C and (90±5%) RH, and the battery performance attenuation was recorded.
[0123] 3.3 Mechanical bending cycle test:
[0124] While keeping the battery connected to the circuit, an automatic bending tester was used to perform a bending test. The curvature radius was set to 5 mm, and the battery performance was measured immediately after each bending.
[0125] After continuous bending for 10,000 times, the changes in battery performance were recorded, with a focus on the retention rate of photoelectric conversion efficiency.
[0126] Experimental parameters: bending radius 5 mm, bending times 10,000 times, and recording the PCE change after each bending.
[0127] 4. Experimental results:
[0128] 4.1 Outdoor light stability: One month of continuous testing showed that the average value of the battery’s photoelectric conversion efficiency remained above 98% of the initial efficiency, indicating that the battery has good stability and weather resistance under natural light.
[0129] 4.2 High temperature and high humidity environment: After 1,000 hours of high temperature and high humidity testing, the battery's photoelectric conversion efficiency only dropped by less than 2%, verifying the battery's stability under extreme climatic conditions.
[0130] 4.3 Mechanical bending cycles: After 10,000 bends, the photoelectric conversion efficiency of the battery remained at around 97.5% of the initial value, proving that the graphene-enhanced flexible substrate significantly improved the mechanical stability and durability of the battery.
[0131] Conclusion: Tests of graphene-enhanced flexible perovskite solar cells in actual application environments have shown that they exhibit excellent stability and lasting photoelectric conversion efficiency under conditions of outdoor natural light, high temperature and humidity, and frequent bending, verifying the significant effect of this design in improving the practicality and environmental adaptability of the battery.
[0132] This achievement has laid a solid foundation for further promoting the commercial application of flexible perovskite solar cells.
[0133] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A flexible perovskite solar cell, characterized in that: The method is to integrate graphene nano-mesh in a polyethylene terephthalate or polyethylene naphthalate flexible substrate to obtain a reinforced structure.
2. A flexible perovskite solar cell according to claim 1, characterized in that: The invention comprises a flexible substrate bottom layer, an electron transport layer, a perovskite layer, a passivation layer, a hole transport layer and a metal back electrode layer which are arranged in sequence, wherein the flexible substrate bottom layer is a graphene nano-mesh reinforced flexible substrate bottom layer.
3. A method for preparing a flexible perovskite solar cell according to claim 1 or 2, characterized in that: The steps include: S1. Graphene nanomesh reinforced flexible substrate bottom layer: A single-layer graphene sheet is prepared by chemical vapor deposition, polyvinyl alcohol is added as a dispersant in ethanol with a mass fraction of 90 to 95%, and ultrasonic treatment is performed to uniformly disperse the graphene to obtain a graphene-ethanol dispersion; After the obtained graphene-ethanol dispersion is coated into a uniform coating, it is applied on a polyethylene terephthalate or polyethylene naphthalate flexible substrate, and after hot pressing curing and annealing, the preparation of the graphene nano-mesh reinforced flexible substrate bottom layer is completed; S2, hole transport layer: After selecting a fullerene derivative and dissolving it in a chlorobenzene solvent, the fullerene derivative is spin-coated on the bottom layer of the graphene nano-mesh reinforced flexible substrate, and annealed and cured to complete the preparation of the hole transport layer; S3, Perovskite layer: Preparation of perovskite precursor solution: Lead iodide, formamidine iodide, methylamine bromide, lead bromide, cesium iodide and methyl iodide were selected according to the corresponding weight parts, mixed and dissolved in an organic solvent, and stirred at room temperature to obtain a molar concentration of 1.6M (FAPbI3) 0.93 (MAPbBr3) 0.05 (CsPbI3) 0.02 Perovskite solution; First, a perovskite precursor solution is dripped onto the hole transport layer prepared by S2, and the solution is rotated at 1000 rpm for 10 to 13 seconds, and then at 4500 rpm for 30 to 35 seconds; 18 to 20 seconds before the end of the rotation at 4500 rpm, an anti-solvent is dripped and spin-coated, and then annealing is performed to complete the preparation of the perovskite layer; S4, passivation layer: A phenethylammonium iodide solution is prepared by selecting phenethylammonium iodide, and the solution is spin-coated on the perovskite layer prepared in S3, and annealed and solidified to complete the preparation of the passivation layer; S5, electron transport layer: A tin dioxide solution containing potassium chloride is spin-coated on the passivation layer prepared by S4, and annealed and cured to complete the preparation of the electron transport layer; S6, metal back electrode layer: Gold is evaporated and deposited on the electron transport layer by physical vapor deposition as the back electrode to complete the preparation of the battery.
4. The method for preparing a flexible perovskite solar cell according to claim 3, characterized in that: In S1, the graphene concentration in the graphene-ethanol dispersion is 0.1-0.2 mg / mL; Ultrasonic treatment for 30-35 min; Hot pressing curing treatment at 100-120°C and 0.5Mpa for 20-25 minutes; Annealing is carried out at 130-150°C for 1-1.2h.
5. The method for preparing a flexible perovskite solar cell according to claim 3, characterized in that: In said S2, the mass concentration of the fullerene derivative is 18-20 mg / mL; The spin coating lasts for 28-30 seconds at a rotation speed of 4000 rpm, followed by annealing at 80-100° C. for 30-35 minutes for curing.
6. The method for preparing a flexible perovskite solar cell according to claim 3, characterized in that: In S3, the weight ratio of each raw material is lead iodide: formamidine iodide: methylamine bromide: lead bromide: cesium iodide: methyl iodide = 735.756 mg, 255.8 mg, 8.95 mg, 29.36 mg, 8.31 mg, 27 mg; The organic solvent is prepared by mixing N,N-dimethylformamide and dimethyl sulfoxide in a volume ratio of 4:
1.
7. The method for preparing a flexible perovskite solar cell according to claim 6, characterized in that: The anti-solvent is chlorobenzene; The stirring time at room temperature is 2 to 2.5 hours; The annealing treatment is performed at 100-150° C. for 20-25 minutes.
8. The method for preparing a flexible perovskite solar cell according to claim 3, characterized in that: In the S4, the spin coating is continued for 28 to 30 seconds at a rotation speed of 4000 to 4500 rpm, and then annealing is performed at 80 to 100° C. for 5 to 6 minutes for curing.
9. The method for preparing a flexible perovskite solar cell according to claim 3, characterized in that: In said S5, the content of potassium chloride in the tin dioxide solution containing potassium chloride is 0.5wt% to 3wt%; The curing treatment is performed by annealing at 100-120° C. for 18-20 minutes.
10. The method for preparing a flexible perovskite solar cell according to claim 3, characterized in that: In the S6, the thickness of the gold electrode is 100 nm.