Molecular solid solution film, preparation method and photoelectric application thereof
The molecular solid solution film prepared by grinding method uses small cationic fillings connected by hydrogen bonds and van der Waals forces to construct a two-dimensional layered structure, which solves the problem of poor photoresponsiveness of existing thin film devices and achieves excellent photoelectricity under 405nm circular polarization light Responsive, suitable for optoelectronic devices and simplifies the preparation process.
Patent Information
- Application Number
- CN202410965416.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
AI Technical Summary
The low carrier mobility, poor photoresponsibility and complex preparation process in photoelectric systems limit their application in industrial deployment, especially the potential of flexible films in wearable devices has not been fully utilized.
Preparation of (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, (IBA)2(EA)2Pb3I10, (IBA)2(DMA)Pb2I7, (IBA)2(GA)Pb2I7, etc. by grinding method The molecular solid solution film formed by the crystal mixing is connected by hydrogen bonds and van der Waals forces, filled with small cations, and constructed a two-dimensional layered structure to achieve excellent photoelectric response.
It achieves excellent photoelectric response under 405nm circularly polarized light, has good application prospects, and simplifies the preparation process, and is suitable for spin coating and annealing treatment of optoelectronic devices, especially on flexible substrates.
Smart Images

Figure CN118946233A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a method for preparing a molecular solid solution film and its optoelectronic application, and belongs to the field of optoelectronic functional materials. Background Art
[0002] A solid solution, also known as an alloy, is a complex material made by adding two or more single-phase materials together so that the overall material is homogeneous. Solid solutions can be formed in several ways: grinding, solution, melting, and vapor deposition. However, compared to those energy-consuming, environmentally harmful, and difficult-to-scale methods, grinding is a simple, green synthesis method that is of great significance.
[0003] Compared with crystal devices, thin film devices have attracted extensive attention from researchers due to their advantages in miniaturization and integration. So far, many thin film devices have been explored. However, most of these thin films have relatively low carrier mobility, poor photoresponsivity, and complex preparation processes, which greatly limits their industrial deployment in optoelectronic systems. In particular, flexible films with excellent flexibility have created great potential in wearable devices, so there is an urgent need to develop flexible thin film devices with excellent photoresponse. Since solid solution films can adjust the band structure, thereby affecting the emission wavelength, absorption cutoff edge, and electrical transport process, the study of solid solution films has become a hot topic. Summary of the invention
[0004] The present invention provides a molecular solid solution film, a preparation method and optoelectronic applications thereof. The present invention obtains a molecular solid solution film, and the molecular solid solution film can achieve excellent photoelectric response under 405nm circularly polarized light, and has good application prospects in the application of optoelectronic devices.
[0005] The present invention is achieved through the following technical solutions:
[0006] Solution 1)
[0007] A molecular solid solution film composed of (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, (IBA)2(EA)2Pb3I 10 , (IBA)2(DMA)Pb2I7, (IBA)2(GA)Pb2I7 or a solid solution formed by mixing two or more crystals in any proportion;
[0008] Where IBA is 4-isopropylbenzylamine, MA is methylamine, FA is formamidine, EA is ethylamine, DMA is dimethylamine, and GA is guanidine.
[0009] The above five single crystal structures are all two-dimensional layered structures. PbI6 octahedron constitutes the inorganic skeleton, IBA is connected between layers through hydrogen bonds and van der Waals forces, and small cations MA, FA, EA, DMA or GA are filled in the pores respectively.
[0010] Specifically, the (IBA)2(MA)Pb2I7 crystallizes in the orthorhombic system, Pna21 space group, and the unit cell parameters are α=90°, β=90°, γ=90°, Z=4
[0011] The (IBA)2(MA)Pb2I7 is prepared by the following method:
[0012] Add lead acetate to the hydroiodic acid solution, heat to 80-100°C on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and methylamine in sequence, heat to 80-100°C and stir until completely dissolved;
[0013] Finally, cooling, filtering, washing and drying are performed to obtain the (IBA)2(MA)Pb2I7;
[0014] The molar ratio of lead acetate, 4-isopropylbenzylamine, methylamine and hydroiodic acid is 6:6:3:21.
[0015] Specifically, the (IBA)2(FA)Pb2I7 crystallizes in the orthorhombic system, Pna21 space group, and the unit cell parameters are α=90°, β=90°, γ=90°, Z=4
[0016] The (IBA)2(FA)Pb2I7 is prepared by the following method:
[0017] Add lead acetate to the hydroiodic acid solution, heat to 80-100°C on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and formamidine in sequence, heat to 80-100°C and stir until completely dissolved;
[0018] Finally, cooling, filtering, washing and drying are performed to obtain the (IBA)2(FA)Pb2I7;
[0019] The molar ratio of lead acetate, 4-isopropylbenzylamine, formamidine and hydroiodic acid is 6:6:3:21.
[0020] Specifically, the (IBA)2(EA)2Pb3I 10 Crystallized in monoclinic system, P c The space group and unit cell parameters are b=9.0067(13), c=8.9294(12), α=90°, β=95.230(5)°, γ=90°, Z=2;
[0021] The (IBA)2(EA)2Pb3I 10 Prepared by the following method:
[0022] Lead acetate is added to the hydroiodic acid solution, and heated to 80-100°C on a magnetic stirrer and stirred until the solution is clear; then 4-isopropylbenzylamine and ethylamine are added in sequence, heated to 80-100°C and stirred until completely dissolved;
[0023] Finally, cooling, filtration, washing and drying are performed to obtain the (IBA)2(EA)2Pb3I 10 ;
[0024] The molar ratio of lead acetate, 4-isopropylbenzylamine, ethylamine and hydroiodic acid is 9:6:6:30.
[0025] Specifically, the (IBA)2(DMA)Pb2I7 crystallizes in the monoclinic system. c The space group and unit cell parameters are α=90°, β=95.746(4)°, γ=90°, Z=2;
[0026] The (IBA)2(DMA)Pb2I7 is prepared by the following method:
[0027] Add lead acetate to the hydroiodic acid solution, heat to 80-100°C on a magnetic stirrer and stir until the solution becomes clear; then add 4-isopropylbenzylamine and dimethylamine in sequence, heat to 80-100°C and stir until completely dissolved;
[0028] Finally, cooling, filtering, washing and drying are performed to obtain the (IBA)2(DMA)Pb2I7;
[0029] The molar ratio of lead acetate, 4-isopropylbenzylamine, dimethylamine and hydroiodic acid is 6:6:3:21.
[0030] Specifically, the (IBA)2(GA)Pb2I7 is a monoclinic system, C c The space group and unit cell parameters are b=9.0851(8), c=8.9156(8), α=90°, β=95.508(4)°, γ=90°, Z=4;
[0031] The (IBA)2(GA)Pb2I7 is prepared by the following method:
[0032] Add lead acetate to the hydroiodic acid solution, heat to 80-100°C on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and guanidine carbonate in sequence, heat to 80-100°C and stir until completely dissolved;
[0033] Finally, the mixture is cooled, filtered, washed and dried to obtain the (IBA)2(GA)Pb2I7; the molar ratio of lead acetate, 4-isopropylbenzylamine, guanidine carbonate and hydroiodic acid is 6:6:1.5:21.
[0034] Preferably, the solid solution is a binary solid solution, a ternary solid solution, a quaternary solid solution or a quinary solid solution.
[0035] Among them, the binary solid solution is:
[0036] (IBA)2(MA)Pb2I7-(IBA)2(EA)2Pb3I 10 , (IBA)2(MA)Pb2I7-(IBA)2(DMA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I 10 , (IBA)2(FA)Pb2I7-(IBA)2(DMA)Pb2I7, (IBA)2(FA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7, (IBA)2(EA)2Pb3I 10 -(IBA)2(GA)Pb2I7, (IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7;
[0037] The ternary solid solution is:
[0038] (IBA)2(MA)Pb2I7-(IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I 10 , (IBA)2(MA)Pb2I7-(IBA)2(FA)Pb2I7-(IBA)2(DMA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(FA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(EA)2Pb3I 10-(IBA)2(GA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7, (IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(GA)Pb2I7, (IBA)2(FA)Pb2I7-(IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7;
[0039] The quaternary solid solution is:
[0040] (IBA)2(MA)Pb2I7-(IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(GA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(FA)Pb2I7-(IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7;
[0041] The quinary solid solution is:
[0042] (IBA)2(MA)Pb2I7-(IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7.
[0043] Scheme II)
[0044] The preparation method of the molecular solid solution thin film includes the following steps:
[0045] According to the need, (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, (IBA)2(EA)2Pb3I 10 Any two or more crystals of (IBA)2(DMA)Pb2I7 and (IBA)2(GA)Pb2I7 are ground and mixed uniformly in any proportion, and then dried and calcined in a constant temperature oven at 50-80° C. for 1-3 hours to obtain a solid solution;
[0046] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4-2:3.
[0047] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0048] Specifically, the flexible substrate is polyethylene terephthalate.
[0049] During spin coating, the rotation speed is set to 1000-2500 r / s, the spin coating time is 10-30 s, and the spin-coated film is annealed at 50-80° C. for 5-10 minutes.
[0050] Option 3)
[0051] Application of molecular solid solution film in optoelectronic device, wherein the optoelectronic device comprises the molecular solid solution film.
[0052] Compared with the prior art, the present invention has the following beneficial effects:
[0053] The present invention obtains a molecular solid solution film and provides a specific preparation method thereof. The molecular solid solution film can achieve excellent photoelectric response under 405nm circularly polarized light and has good application prospects in the application of photoelectric devices.
[0054] The molecular solid solution preparation method is simple and universal, and provides an innovative preparation method for future optoelectronic application materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 The crystal photos obtained in Examples 1-5, where a is (IBA)2(MA)Pb2I7, b is (IBA)2(FA)Pb2I7, and c is (IBA)2(EA)2Pb3I 10 , d is the crystal photograph of (IBA)2(DMA)Pb2I7, and e is the crystal photograph of (IBA)2(GA)Pb2I7.
[0056] Figure 2This is the crystal structure diagram of (IBA)2(MA)Pb2I7.
[0057] Figure 3 This is the crystal structure diagram of (IBA)2(FA)Pb2I7.
[0058] Figure 4 Yes(IBA)2(EA)2Pb3I 10 Crystal structure diagram.
[0059] Figure 5 This is the crystal structure diagram of (IBA)2(DMA)Pb2I7.
[0060] Figure 6 This is the crystal structure diagram of (IBA)2(GA)Pb2I7.
[0061] Figure 7 This is a schematic diagram of the process of obtaining 25 solid solutions by grinding method.
[0062] Figure 8 Example 8 obtained (IBA)2(EA)2Pb3I 10 -(IBA)2(GA)Pb2I7 (EG for short) solid solution film process.
[0063] Fig. 9 This is a schematic diagram of the EG flexible thin film device.
[0064] Fig.10 is the circularly polarized light response of the EG flexible film measured at 405 nm.
[0065] Fig.11 These are photos of the EG flexible film with a curvature radius ranging from ∞ to 2.5 mm.
[0066] Fig.12 This is the circularly polarized light response of the EG flexible film measured at 405nm and different curvature radii. DETAILED DESCRIPTION
[0067] The present application is described in detail below in conjunction with the examples, but the present application is not limited to these examples. Unless otherwise specified, the raw materials and reagents used in the present application are purchased from commercial sources and used directly without treatment, and the instruments and equipment used adopt the schemes and parameters recommended by the manufacturers.
[0068] Example 1
[0069] Add lead acetate to the hydroiodic acid solution, heat to 80°C (any temperature between 80-100°C) on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and methylamine in sequence, heat to 80°C and stir until completely dissolved;
[0070] Finally, cooling, filtration, washing and drying were performed to obtain (IBA)2(MA)Pb2I7;
[0071] The molar ratio of lead acetate, 4-isopropylbenzylamine, methylamine and hydroiodic acid is 6:6:3:21.
[0072] The structure of the samples was analyzed using single crystal X-ray diffraction.
[0073] The (IBA)2(MA)Pb2I7 crystallizes in the orthorhombic system, Pna21 space group, and the unit cell parameters are α=90°, β=90°, γ=90°, Z=4.
[0074] Example 2
[0075] Add lead acetate to the hydroiodic acid solution, heat to 80°C (any temperature between 80-100°C) on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and formamidine in sequence, heat to 80°C and stir until completely dissolved;
[0076] Finally, cooling, filtering, washing and drying are performed to obtain the (IBA)2(FA)Pb2I7;
[0077] The molar ratio of lead acetate, 4-isopropylbenzylamine, formamidine and hydroiodic acid is 6:6:3:21.
[0078] The (IBA)2(FA)Pb2I7 is an orthorhombic system with a space group of Pna21 and a unit cell parameter of α=90°, β=90°, γ=90°, Z=4.
[0079] Example 3
[0080] Add lead acetate to the hydroiodic acid solution, heat to 80°C (any temperature between 80-100°C) on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and ethylamine in sequence, heat to 80°C and stir until completely dissolved;
[0081] Finally, cooling, filtration, washing and drying are performed to obtain the (IBA)2(EA)2Pb3I 10 ;
[0082] The molar ratio of lead acetate, 4-isopropylbenzylamine, ethylamine and hydroiodic acid is 9:6:6:30.
[0083] The (IBA)2(EA)2Pb3I 10 Crystallized in monoclinic system, P c The space group and unit cell parameters are b=9.0067(13), c=8.9294(12), α=90°, β=95.230(5)°, γ=90°, Z=2.
[0084] Example 4
[0085] Add lead acetate to the hydroiodic acid solution, heat to 80°C (any temperature between 80-100°C) on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and dimethylamine in sequence, heat to 80°C and stir until completely dissolved;
[0086] Finally, cooling, filtering, washing and drying are performed to obtain the (IBA)2(DMA)Pb2I7;
[0087] The molar ratio of lead acetate, 4-isopropylbenzylamine, dimethylamine and hydroiodic acid is 6:6:3:21.
[0088] The (IBA)2(DMA)Pb2I7 crystallizes in the monoclinic system, P c The space group and unit cell parameters are α=90°, β=95.746(4)°, γ=90°, Z=2.
[0089] Example 5
[0090] Add lead acetate to the hydroiodic acid solution, heat to 80°C (any temperature between 80-100°C) on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and guanidine carbonate in sequence, heat to 80°C and stir until completely dissolved;
[0091] Finally, the mixture is cooled, filtered, washed and dried to obtain the (IBA)2(GA)Pb2I7; the molar ratio of lead acetate, 4-isopropylbenzylamine, guanidine carbonate and hydroiodic acid is 6:6:1.5:21.
[0092] The (IBA)2(GA)Pb2I7 crystallizes in the monoclinic system, C c The space group and unit cell parameters are b=9.0851(8), c=8.9156(8), α=90°, β=95.508(4)°,
[0093] γ=90°,Z=4;
[0094] The types, proportions, and cooling ranges of the raw materials used in the above examples are shown in Table 1. Figure 1 shown.
[0095] High-quality crystals with regular size and no obvious defects in the above-mentioned embodiments were selected under a microscope, and then glued to the end of a glass wire and exposed to Mo Kα radiation. The low temperature structural data of the compound were collected on a Bruker D8 diffractometer. The crystal structure was first directly solved, and then the SHELXLTL software package was used to further optimize the crystal structure. 2 The structure was refined using the full matrix least squares method. Diamond software was used to draw their molecular structures. In order to make the structure look clearer, hydrogen atoms were omitted during the drawing process.
[0096] Among them, the single crystal X-ray diffraction results show that the chemical formula, crystal system, space group, and crystallographic parameters of each embodiment are as described in Table 2. The compounds all adopt a two-dimensional layered structure, in which PbI6 octahedrons constitute an inorganic skeleton, IBA is connected between layers through hydrogen bonds and van der Waals forces, and small cations MA, FA, EA, DMA, and GA are filled in the voids ( Figure 2-Figure 6 ). The distortion of the inorganic framework and the directional arrangement of organic cations are conducive to the formation of polarization.
[0097] Table 1 Types and amounts of raw materials used in the examples, and cooling ranges
[0098]
[0099]
[0100] Table 2 Chemical formula, crystal system, space group, crystallographic parameters of various examples
[0101]
[0102] The following is an example of the preparation of a binary solid solution film:
[0103] Example 6
[0104] Combine (IBA)2(MA)Pb2I7 and (IBA)2(EA)2Pb3I 10 Grind and mix evenly according to a molar ratio of 1:1 (or any other ratio), and then dry and calcine in a constant temperature oven at 50° C. for 3 hours to obtain a solid solution;
[0105] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4.
[0106] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0107] The flexible substrate is polyethylene terephthalate.
[0108] The rotation speed during spin coating was set to 1000 r / s, the spin coating time was 10 s, and the spin-coated film was annealed at 50° C. for 10 minutes.
[0109] Example 7
[0110] Grind and mix (IBA)2(MA)Pb2I7 and (IBA)2(DMA)Pb2I7 in a molar ratio of 1:1 (or any other ratio), and then dry and calcine in a constant temperature oven at 80°C for 1 hour to obtain a solid solution;
[0111] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 2:3
[0112] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0113] The flexible substrate is polyethylene terephthalate.
[0114] The rotation speed during spin coating was set to 2500 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 80° C. for 5 minutes.
[0115] Example 8
[0116] Will (IBA)2(EA)2Pb3I 10 and (IBA)2(GA)Pb2I7 in a molar ratio of 1:1 (or any other ratio), and then dried and calcined in a constant temperature oven at 60°C for 2 hours to obtain a solid solution;
[0117] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 2:4
[0118] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0119] The flexible substrate is polyethylene terephthalate.
[0120] The rotation speed during spin coating was set to 2000 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 60° C. for 7 minutes.
[0121] Figure 8 Example 8 obtained (IBA)2(EA)2Pb3I 10-(IBA)2(GA)Pb2I7 (EG for short) solid solution film process.
[0122] The binary solid solution can also be (IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I 10 , (IBA)2(FA)Pb2I7-(IBA)2(DMA)Pb2I7, (IBA)2(FA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7.
[0123] The following is an example of the preparation of a ternary solid solution film:
[0124] Example 9
[0125] Combine (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, (IBA)2(EA)2Pb3I 10 Grind and mix evenly according to a molar ratio of 1:1:1 (or any other ratio), and then dry and calcine in a constant temperature oven at 60° C. for 2 hours to obtain a solid solution;
[0126] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4.
[0127] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0128] The flexible substrate is polyethylene terephthalate.
[0129] The rotation speed during spin coating was set to 2000 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 60° C. for 7 minutes.
[0130] Example 10
[0131] Grind and mix (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, and (IBA)2(DMA)Pb2I7 in a molar ratio of 1:1:1 (or any other ratio), and then dry and calcine in a constant temperature oven at 60° C. for 2 hours to obtain a solid solution;
[0132] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4
[0133] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0134] The flexible substrate is polyethylene terephthalate.
[0135] The rotation speed during spin coating was set to 2000 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 60° C. for 7 minutes.
[0136] Embodiment 11
[0137] Grind and mix (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, and (IBA)2(GA)Pb2I7 in a molar ratio of 1:1:1 (or any other ratio), and then dry and calcine in a constant temperature oven at 60°C for 2 hours to obtain a solid solution;
[0138] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4.
[0139] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0140] The flexible substrate is polyethylene terephthalate.
[0141] The rotation speed during spin coating was set to 2000 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 60° C. for 7 minutes.
[0142] The ternary solid solution can also be:
[0143] (IBA)2(MA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(GA)Pb2I7, (IBA)2(MA)Pb2I7-(IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7, (IBA)2(FA)Pb2I7-(IBA)2(EA)2Pb3I10 -(IBA)2(GA)Pb2I7, (IBA)2(FA)Pb2I7-(IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7, (IBA)2(EA)2Pb3I 10 -(IBA)2(DMA)Pb2I7-(IBA)2(GA)Pb2I7;
[0144] The following is an example of the preparation of a quaternary solid solution film:
[0145] Example 12
[0146] Combine (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, (IBA)2(EA)2Pb3I 10 , (IBA)2(DMA)Pb2I7 are ground and mixed uniformly in a molar ratio of 1:1:1:1 (or any other ratio), and then dried and calcined in a constant temperature oven at 60° C. for 2 hours to obtain a solid solution;
[0147] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4
[0148] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0149] The flexible substrate is polyethylene terephthalate.
[0150] The rotation speed during spin coating was set to 2000 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 60° C. for 7 minutes.
[0151] Embodiment 13
[0152] Combine (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, (IBA)2(EA)2Pb3I 10 , (IBA)2(GA)Pb2I7 are ground and mixed uniformly in a molar ratio of 1:1:1:1 (or any other ratio), and then dried and calcined in a constant temperature oven at 60° C. for 2 hours to obtain a solid solution;
[0153] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4.
[0154] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0155] The flexible substrate is polyethylene terephthalate.
[0156] The rotation speed during spin coating was set to 2000 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 60° C. for 7 minutes.
[0157] Embodiment 14
[0158] Combine (IBA)2(MA)Pb2I7, (IBA)2(EA)2Pb3I 10 , (IBA)2(DMA)Pb2I7, (IBA)2(GA)Pb2I7, grind and mix evenly in a molar ratio of 1:1:1:1 (or any other ratio), and then dry and calcine in a constant temperature oven at 60° C. for 2 hours to obtain a solid solution;
[0159] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4.
[0160] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0161] The flexible substrate is polyethylene terephthalate.
[0162] The rotation speed during spin coating was set to 2000 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 60° C. for 7 minutes.
[0163] Embodiment 15
[0164] Grind and mix (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, (IBA)2(DMA)Pb2I7, and (IBA)2(GA)Pb2I7 in a molar ratio of 1:1:1:1 (or any other ratio), and then dry and calcine in a constant temperature oven at 60° C. for 2 hours to obtain a solid solution;
[0165] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4.
[0166] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0167] The flexible substrate is polyethylene terephthalate.
[0168] The rotation speed during spin coating was set to 2000 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 60° C. for 7 minutes.
[0169] Example 16
[0170] Combine (IBA)2(FA)Pb2I7, (IBA)2(EA)2Pb3I 10 , (IBA)2(DMA)Pb2I7, and (IBA)2(GA)Pb2I7 are ground and mixed uniformly in a molar ratio of 1:1:1:1 (or any other ratio), and then dried and calcined in a constant temperature oven at 60° C. for 2 hours to obtain a solid solution;
[0171] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4.
[0172] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0173] The flexible substrate is polyethylene terephthalate.
[0174] The rotation speed during spin coating was set to 2000 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 60° C. for 7 minutes.
[0175] The following is an example of the preparation of a five-element solid solution film:
[0176] Embodiment 17
[0177] Combine (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, (IBA)2(EA)2Pb3I 10 , (IBA)2(DMA)Pb2I7, and (IBA)2(GA)Pb2I7 are ground and mixed uniformly in a molar ratio of 1:1:1:1:1 (or any other ratio), and then dried and calcined in a constant temperature oven at 60° C. for 2 hours to obtain a solid solution;
[0178] Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4.
[0179] Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
[0180] The flexible substrate is polyethylene terephthalate.
[0181] The rotation speed during spin coating was set to 2000 r / s, the spin coating time was 20 s, and the spin-coated film was annealed at 60° C. for 7 minutes.
[0182] Figure 7 The figure is a schematic diagram of 25 solid solutions obtained by grinding. Among them, (a) keeping the inorganic framework and interlayer cations unchanged, MA, FA, EA, DMA, and GA are filled into the pores respectively to construct different compounds in sequence; (b) five single crystals are obtained by cooling crystallization, each of which is like a unique puzzle piece; (c) five single crystals obtained by cooling crystallization can be ground into any two or more crystals like puzzle pieces. Figure 1 By putting the fragments together, 25 solid solutions can be constructed.
[0183] The flexible substrates in the above embodiments need to be cleaned in acetone, N,N-dimethylformamide solution and anhydrous ethanol in sequence before use, and then treated in an ozone generator for 1 hour. The spin coating is performed in a vacuum glove box.
[0184] The molecular solid solution film of the above embodiment was subjected to an electrophotographic test. The electrometer used in the test was a Model 6517B from Keithley, USA. The specific steps were as follows:
[0185] A plurality of silver electrodes are evenly coated at equal intervals on the flexible film prepared in the above Example 8, and copper wires are introduced at the same time. The film is then placed in a constant temperature oven at 50-80° C. for drying and annealing for 1-3 hours before being connected to a circuit.
[0186] When using, Fig. 9 As shown, a laser with a wavelength of 405nm, a half-wave plate and a quarter-wave plate are introduced into the circuit respectively. When natural light enters the polarizer and the quarter-wave plate in sequence, the natural light can be converted into circularly polarized light. By rotating the quarter-wave plate, the conversion of left-right rotation can be achieved. The molecular solid solution film obtained in Example 8 realizes photoelectric response under 405nm natural light, and realizes photoelectric response under 405nm circularly polarized light ( Fig.10 ), other embodiments can also achieve photoelectric response under circularly polarized light. In order to quantify the distinguishable sensitivity of molecular solid solution films to circularly polarized light, according to g Iph =2(J R –J L ) / (J R +J L ) formula to deduce the asymmetry factor g of the photocurrent Iph , where J R and J L is the photocurrent density of right-handed and left-handed light. Under zero bias conditions, the g of our photodetector at 405 nm is Iph The value is ≈1.7. This is higher than the g of most chiral compounds. Iph(≈0.2). And when the film is bent into different radii of curvature ( Fig.11 ), the circularly polarized light response has almost no attenuation ( Fig.12 ).
[0187] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A molecular solid solution film, characterized in that: The solid solution is composed of (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, (IBA)2(EA)2Pb3I 10 , (IBA)2(DMA)Pb2I7, (IBA)2(GA)Pb2I7, or two or more crystals thereof are ground, mixed, and calcined in any proportion; Where IBA is 4-isopropylbenzylamine, MA is methylamine, FA is formamidine, EA is ethylamine, DMA is dimethylamine, and GA is guanidine.
2. A molecular solid solution film according to claim 1, characterized in that: The (IBA)2(MA)Pb2I7 crystallizes in the orthorhombic system, Pna21 space group, and the unit cell parameters are α=90°, β=90°, γ=90°, Z=4; The (IBA)2(MA)Pb2I7 is prepared by the following method: Add lead acetate to the hydroiodic acid solution, heat to 80-100°C on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and methylamine in sequence, heat to 80-100°C and stir until the solution is clear and transparent; Finally, cooling, filtering, washing and drying are performed to obtain the (IBA)2(MA)Pb2I7; The molar ratio of lead acetate, 4-isopropylbenzylamine, methylamine and hydroiodic acid is 6:6:3:
21.
3. A molecular solid solution film according to claim 1, characterized in that: The (IBA)2(FA)Pb2I7 crystallizes in the orthorhombic system, Pna21 space group, and the unit cell parameters are α=90°, β=90°, γ=90°, Z=4; The (IBA)2(FA)Pb2I7 is prepared by the following method: Add lead acetate to the hydroiodic acid solution, heat to 80-100°C on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and formamidine, heat to 80-100°C and stir until the solution is clear and transparent; Finally, cooling, filtering, washing and drying are performed to obtain the (IBA)2(FA)Pb2I7; The molar ratio of lead acetate, 4-isopropylbenzylamine, formamidine and hydroiodic acid is 6:6:3:
21.
4. A molecular solid solution film according to claim 1, characterized in that: The (IBA)2(EA)2Pb3I 10 Crystallized in monoclinic system, P c The space group and unit cell parameters are b=9.0067(13), c=8.9294(12), α=90°, β=95.230(5)°, γ=90°, Z=2; The (IBA)2(EA)2Pb3I 10 Prepared by the following method: Add lead acetate to the hydroiodic acid solution, heat to 80-100°C on a magnetic stirrer and stir until the solution is clear; then add 4-isopropylbenzylamine and ethylamine, heat to 80-100°C and stir until the solution is clear and transparent; Finally, cooling, filtration, washing and drying are performed to obtain the (IBA)2(EA)2Pb3I 10 ; The molar ratio of lead acetate, 4-isopropylbenzylamine, ethylamine and hydroiodic acid is 9:6:6:
30.
5. A molecular solid solution film according to claim 1, characterized in that: The (IBA)2(DMA)Pb2I7 crystallizes in the monoclinic system, P c The space group and unit cell parameters are α=90°, β=95.746(4)°, γ=90°, Z=2; The (IBA)2(DMA)Pb2I7 is prepared by the following method: Add lead acetate to the hydroiodic acid solution, heat to 80-100°C on a magnetic stirrer and stir until the solution becomes clear; then add 4-isopropylbenzylamine and dimethylamine in sequence, heat to 80-100°C and stir until completely dissolved; Finally, cooling, filtering, washing and drying are performed to obtain the (IBA)2(DMA)Pb2I7; The molar ratio of lead acetate, 4-isopropylbenzylamine, dimethylamine and hydroiodic acid is 6:6:3:
21.
6. A molecular solid solution film according to claim 1, characterized in that: The (IBA)2(GA)Pb2I7 crystallizes in the monoclinic system, C c The space group and unit cell parameters are b=9.0851(8), c=8.9156(8), α=90°, β=95.508(4)°, γ=90°, Z=4; The (IBA)2(GA)Pb2I7 is prepared by the following method: Add lead acetate to the hydroiodic acid solution, heat to 80-100°C on a magnetic stirrer and stir until the solution becomes clear; then add 4-isopropylbenzylamine and guanidine carbonate respectively, heat to 80-100°C and stir until they are completely dissolved; Finally, the mixture is cooled, filtered, washed and dried to obtain the (IBA)2(GA)Pb2I7; the molar ratio of lead acetate, 4-isopropylbenzylamine, guanidine carbonate and hydroiodic acid is 6:6:1.5:
21.
7. A molecular solid solution film according to claim 1, characterized in that: The solid solution is a binary solid solution, a ternary solid solution, a quaternary solid solution or a quinary solid solution.
8. The method for preparing a molecular solid solution thin film according to any one of claims 1 to 7, characterized in that: The steps include: According to the need, (IBA)2(MA)Pb2I7, (IBA)2(FA)Pb2I7, (IBA)2(EA)2Pb3I 10 Any two or more crystals of (IBA)2(DMA)Pb2I7 and (IBA)2(GA)Pb2I7 are ground and mixed uniformly in any proportion, and then dried and calcined in a constant temperature oven at 50-80° C. for 1-3 hours to obtain a solid solution; Then, the obtained solid solution is dissolved in N,N-dimethylformamide solution to obtain a precursor solution; the mass ratio of the solid solution to the N,N-dimethylformamide solution is 1:4-2:3; Then, the obtained precursor solution is spin-coated on a clean flexible substrate in a vacuum glove box to obtain the solid solution film.
9. The method for preparing a molecular solid solution thin film according to claim 8, characterized in that: The flexible substrate is polyethylene terephthalate; The rotation speed during spin coating is set to 1000-2500 r / s, the spin coating time is 10-30 s, and the spin-coated film is annealed at 50-80° C. for 5-10 minutes.
10. Application of the molecular solid solution film according to any one of claims 1 to 7 in optoelectronic devices, characterized in that: The optoelectronic device comprises the molecular solid solution film according to any one of claims 1-7.