Single-domain nanoscale pyroelectric single crystal film and preparation method thereof
By adding a pyroelectric elimination layer with opposite polarity at the interface between the substrate layer and the pyroelectric thin film layer, the charge accumulation problem is solved, and a nano-scale pyroelectric single crystal thin film with a polarization strength close to the bulk material is prepared, which solves the existing The polarization reversal problem caused by thermal annealing in the technology achieves high voltage electrical performance and stability, reducing production costs and process complexity.
Patent Information
- Application Number
- CN202410845420.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-06-27
AI Technical Summary
In the preparation of nano-scale pyroelectric single crystal thin films, polarization reversal caused by charge accumulation during thermal annealing, resulting in a decrease in piezoelectricity, which makes it difficult to meet performance requirements. The traditional method is costly and cumbersome, so it cannot be realized. Mass production.
By adding a pyroelectric elimination layer with opposite polarity at the interface between the substrate layer and the pyroelectric thin film layer, a conductive domain wall is formed, the charge accumulation problem is solved, the polarization strength is improved, and single domain is prepared by double bonding and polishing steps. Nano-scale pyroelectric single crystal thin film.
The polarization characteristics of nano-scale pyroelectric single crystal thin film are close to that of bulk materials, maintain high voltage electrical coefficient, reduce production costs and process complexity, ensure the stability of piezoelectric performance and the electromechanical coupling coefficient of the device. consistency.
Smart Images

Figure HDA0004915551550000011 
Figure HDA0004915551550000012
Abstract
Description
Technical Field
[0001] The invention relates to a single-domain nanometer-level pyroelectric single crystal film and a preparation method thereof, belonging to the technical field of semiconductors. Background Art
[0002] Oxide single crystals such as lithium niobate (LN), lithium tantalate (LT), and quartz, as piezoelectric materials, are widely used in materials for components such as surface acoustic wave (SAW) filters due to their good electromechanical coupling coefficient, which can enable filters to achieve high bandwidth characteristics. The traditional polishing process can obtain oxide single crystal thin films of several microns to tens of microns, but with the development trend of miniaturization of communication equipment, the volume of parts in the equipment is also required to be further miniaturized and high-performance, so the method of preparing nanometer-level thickness thin films using smart peeling technology is also used to prepare nanometer-level thickness oxide single crystal thin films.
[0003] Smart stripping technology mainly uses light ions, such as H+, He, etc., to bombard the wafer, so that the charged ions enter the wafer and form an ion implantation layer inside the wafer, and then undergoes a heat treatment process to peel the single crystal film from the original wafer at the location of the ion implantation layer. However, during the preparation process, since a higher energy, such as 500KeV, is required to bombard the oxide single crystal wafer, more defects will be generated in the single crystal film; therefore, the appropriate temperature must be selected to anneal the obtained nanoscale single crystal film in order to eliminate the defects caused by ion implantation.
[0004] Generally, the charge mainly accumulates near the bonding surface between the crystal and the substrate. Taking lithium niobate as an example, when lithium niobate is in the paraelectric phase, Li and Nb are located at the oxygen plane and the center of the oxygen octahedron respectively, and there is no spontaneous polarization; in the ferroelectric phase, Li and Nb both have electric dipole moments along the Z axis, that is, spontaneous polarization occurs, and the spontaneous polarization vector Ps is along the Z axis. It can be seen that the lithium niobate crystal obtained by Z-cutting (hereinafter referred to as Z-cut lithium niobate crystal) has spontaneous polarization and can undergo polarization reversal under the action of an external electric field.
[0005] Since lithium niobate crystal has a very high pyroelectric coefficient, up to 4×10 -5 C / m 2 K, and due to its high resistivity (10 13Ωcm or more). During the production process of the film, as the temperature changes, a large amount of static charge is easily accumulated on the wafer surface. Although these static charges can be spontaneously released in a natural state, the release process is very slow. Therefore, the formed charge will accumulate between the substrate and the pyroelectric film, thereby forming an electric field. In this way, the spontaneous polarization vector Ps of the Z-cut lithium niobate wafer can undergo polarization reversal under the action of the electric field, which eventually leads to the formation of polarization defects in the Z-cut lithium niobate wafer during the heat treatment of the composite film. Specifically, multiple polarization spots appear on the surface of the Z-cut lithium niobate wafer. Although these polarization spots may have no effect on the ferroelectric properties of the composite film, they will cause the piezoelectricity of the composite film to decrease. If the composite film is applied to the piezoelectric direction, it is difficult to meet the corresponding performance requirements; taking the z-cut lithium niobate crystal as an example, the piezoelectric coefficient d33 of the single-domain lithium niobate is about 28pC / N, and polarization reversal will cause the piezoelectric coefficient to decrease, and in severe cases it may even decrease by 90%.
[0006] The existing method for monodomainization of piezoelectric crystals is to place electrodes on both ends of the crystal, heat it to above the Curie temperature, pass current, and then gradually cool it down. However, this method is not suitable for making thin film substrate materials because each piece needs to have electrodes on both sides, which makes mass production cost high, the process is complicated, and it is impossible to achieve mass production. In addition, due to the large difference in thermal expansion coefficients between silicon substrates and lithium niobate and lithium tantalate, the film is very likely to break when heated above the Curie temperature.
[0007] How to make the nanoscale pyroelectric single crystal film obtained by smart peeling technology have a polarization strength close to that of bulk material has become an urgent problem to be solved. Summary of the invention
[0008] In view of the deficiencies in the prior art, the present invention provides a single-domain nanoscale pyroelectric single crystal film and a preparation method thereof.
[0009] The method of the present invention avoids polarization reversal caused by charges generated by pyroelectric properties during thermal annealing of the film, improves the polarization strength performance of the nanoscale pyroelectric single crystal film, and makes the polarization characteristics of the obtained nanoscale single crystal film close to those of bulk materials.
[0010] To achieve the above object, the present invention is implemented by the following technical solutions:
[0011] A method for preparing a single-domain nanoscale pyroelectric single crystal film comprises the following steps:
[0012] 1) providing a substrate wafer, and after cleaning, preparing a layer of silicon dioxide as an isolation layer on the substrate wafer;
[0013] 2) providing a pyroelectric thin film wafer a, and after cleaning, implanting helium ions (He+) into the pyroelectric thin film wafer a by ion implantation;
[0014] 3) performing a first bonding of the +Z polarization plane of the pyroelectric thin film wafer a implanted with ions in step 2) with the silicon dioxide layer of the substrate wafer in step 1) to obtain a bonding body a;
[0015] 4) Keeping the bonded body a at a constant temperature of 150° C. to 400° C. to achieve the first peeling of the pyroelectric thin film to form a pyroelectric elimination layer a with a +Z polarization surface facing the silicon dioxide;
[0016] 5) providing a pyroelectric thin film wafer b, and after cleaning, implanting helium ions (He+) into the pyroelectric thin film wafer b by ion implantation;
[0017] 6) performing a second bonding between the -Z polarization surface of the pyroelectric thin film wafer b implanted with ions in step 5) and the -Z polarization surface of the pyroelectric elimination layer of the bonding body a obtained in step 4) to obtain a bonding body b;
[0018] 7) The bond body b is kept at a constant temperature of 150° C. to 400° C. to achieve a second peeling of the pyroelectric film sheet, forming a pyroelectric film layer with a +Z polarization plane facing away from the bond body b, and the pyroelectric film layer is polished to obtain a single-domain pyroelectric crystal film b.
[0019] Preferably according to the present invention, in step 1), the substrate wafer is selected from silicon, silicon carbide, sapphire, quartz, fused quartz, has a size of 3 to 12 inches, and a thickness of 0.2 to 1 mm.
[0020] Further preferably, in step 1), the substrate wafer is selected from a silicon wafer having a size of 4 inches.
[0021] Preferably according to the present invention, in step 1), the smooth surface of the substrate wafer is cleaned, and after cleaning, a silicon dioxide layer is prepared on the substrate wafer by thermal oxidation, PECVD, LPCVD or CVD, and the thickness of the silicon dioxide layer is 50nm to 5μm.
[0022] Further preferably, in step 1), the deposited silicon dioxide layer is annealed to eliminate impurity ions in the deposited silicon dioxide layer to reduce absorption loss.
[0023] Further preferably, in step 1), the roughness of the silicon dioxide layer is less than or equal to 0.5 nm.
[0024] Preferably according to the present invention, in step 2), the pyroelectric thin film wafer a is lithium niobate, lithium tantalate or silicon carbide, with a size of 3 to 12 inches and a thickness of 0.2 to 1 mm.
[0025] Further preferably, in step 2), the pyroelectric thin film wafer a is a z-tangent lithium niobate wafer with a size of 4 inches and an injection surface being a +Z polarization surface.
[0026] According to the preferred embodiment of the present invention, in step 2), the helium ion implantation energy is 30KeV to 5MeV, and the dose is 1×10 15 ions / cm 2 ~1×10 17 ions / cm 2 Helium ions are injected to form a thin film wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer.
[0027] Preferably according to the present invention, in step 3), bonding is performed by plasma bonding, and the structure of the bonding body a from top to bottom is a lithium niobate thin film sheet with a -Z polarization plane facing away from silicon dioxide, a silicon dioxide isolation layer, and a silicon substrate sheet.
[0028] Preferably according to the present invention, in step 4), the pyroelectric elimination layer a with the +Z polarization plane facing the silicon dioxide is polished and thinned to 5nm-100nm with a surface roughness of less than or equal to 0.5nm to obtain a bonded body a having a pyroelectric elimination layer.
[0029] Preferably according to the present invention, in step 5), the pyroelectric film wafer b is the same as the pyroelectric film wafer a in step 2), but the ion implantation surface is a -Z polarization surface, which is opposite to the implantation surface of the pyroelectric film wafer a.
[0030] According to the preferred embodiment of the present invention, in step 5), the helium ion implantation energy is 30KeV to 5MeV, and the dose is 1×10 15 ions / cm 2 ~1×10 17 ions / cm 2 The implantation energy and dosage of helium ions may be the same as or different from those in step 2).
[0031] Preferably according to the present invention, in step 6), bonding is performed by plasma bonding, and the implantation surface of the ion-implanted pyroelectric thin film wafer b is bonded for a second time with the pyroelectric elimination surface of the bonding body a obtained in step 4) which is away from the silicon dioxide layer.
[0032] Preferably, according to the present invention, in step 7), the pyroelectric thin film layer is polished to thin the pyroelectric thin film layer to 50 nm-20 μm.
[0033] A single-domain nanoscale pyroelectric single crystal film is prepared by the method.
[0034] The monodomain nanoscale pyroelectric single crystal film is provided with a substrate layer, an isolation layer, a pyroelectric elimination layer and a pyroelectric film layer in sequence from bottom to top.
[0035] Preferably according to the present invention, the material of the pyroelectric film layer is lithium niobate or lithium tantalate pyroelectric film layer.
[0036] Preferably according to the present invention, the material of the pyroelectric elimination layer is the same as that of the pyroelectric film layer, but the polarity is reversed.
[0037] The present invention forms a conductive layer with good conductivity by forming a conductive domain wall at the interface between the pyroelectric elimination layer and the pyroelectric film layer, solves the problem of charge accumulation at the bonding interface, and eliminates the depolarization of the single-domain piezoelectric film.
[0038] Preferably according to the present invention, the isolation layer is made of silicon dioxide or silicon nitride amorphous material, and its refractive index is smaller than the refractive index of the pyroelectric thin film layer material.
[0039] Preferably according to the present invention, the substrate layer material is silicon, silicon carbide, sapphire, quartz, or fused quartz.
[0040] The single-domain nanoscale pyroelectric single crystal film of the present invention adds a thinner pyroelectric elimination layer between the insulating pyroelectric film layer and the isolation layer. The material of the layer is consistent with the material of the pyroelectric film layer, but the polarity in the direction of the surface normal is reversed, which not only achieves the effect of improving the charge accumulation of the pyroelectric crystal film, but also has the same material and physical properties as the pyroelectric film layer material, and has no effect on the piezoelectricity, pyroelectricity, electro-optical coefficients, etc. of the film. The pyroelectric film layer in the structure of the present invention has the characteristics of high polarization strength.
[0041] The beneficial effects of the present invention are as follows:
[0042] 1. Due to the pyroelectric effect of the pyroelectric crystal film, the annealing process causes a large amount of charge to accumulate near the bonding surface between the crystal and the substrate. By adding a film of the same material with opposite polarity near the bonding interface, the phenomenon of charge accumulation at the bonding interface is solved, the possibility of depolarization of the single-domain piezoelectric film is eliminated, and the single-domain nature of the pyroelectric film is ensured.
[0043] 2. The present invention adds a pyroelectric elimination layer at the bonding interface between the pyroelectric film layer and the substrate layer, wherein the pyroelectric elimination layer is characterized by: the same material as the pyroelectric film layer; and the polarity opposite to the normal direction of the pyroelectric film layer. Compared with the prior art method of making electrodes on both sides of the composite film, no additional electrodes or other materials heterogeneous to the film are introduced, the process is relatively simple, the cost is low, the stress is small, and the problem of film shedding between the pyroelectric film layer and the electrode is avoided.
[0044] 3. The lithium niobate single crystal piezoelectric film prepared by the present invention has good single domain property and well retains the piezoelectric coefficient of the lithium niobate bulk material. The piezoelectric coefficient d33 of the single-domain lithium niobate bulk material is about 28pC / N. The piezoelectric coefficient of the lithium niobate single crystal piezoelectric film prepared by the present invention is 98% to 100% of the bulk material, while the piezoelectric coefficient of the prior art is 10% to 90% of the bulk material. The single-domain single crystal film has stable piezoelectric performance when in use, the electromechanical coupling coefficient of the device will not decrease, the bandwidth is wide, the loss is low, and the consistency is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The flowchart of the preparation of single-domain nanoscale pyroelectric single crystal thin film;
[0046] Figure 2 This is a schematic diagram of the structure of a single-domain nanoscale pyroelectric single crystal film;
[0047] Among them, 1. LN film b, 2. LN film a, 3. Silicon dioxide layer, 4. Substrate. DETAILED DESCRIPTION
[0048] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. The specific details set forth in the following description are for a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.
[0049] Injection stop layer: Plasma carries a certain amount of charge, and the positive ions can be accelerated by the electric field, and the direction of their movement can be changed by the magnetic field. In this way, the ions can be controlled to enter the wafer with a certain energy. After the ions are injected into the wafer, they will collide with the atoms and nuclei of the wafer and lose energy. When the energy is exhausted, the ions will stop at a certain depth in the wafer, which is the injection stop layer.
[0050] Example 1
[0051] A method for preparing a single-domain nanoscale pyroelectric single crystal thin film, the preparation process is as follows Figure 1 As shown, the steps are as follows:
[0052] 1) Providing a silicon substrate wafer with a smooth surface, a size of 4 inches and a thickness of 0.5 mm;
[0053] 2) Cleaning the smooth surface of the silicon substrate wafer, and preparing a layer of silicon dioxide as an isolation layer thereon by thermal oxidation; the thickness of the silicon dioxide layer is 500 nm, and the deposited silicon dioxide is annealed to eliminate impurity ions in the deposited silicon dioxide layer to reduce absorption loss, and the roughness of the silicon dioxide layer is less than 0.5 nm;
[0054] 3) Provide a pyroelectric thin film wafer a, which is a z-cut lithium niobate wafer with a size of 4 inches. After cleaning, helium ions (He+) are implanted into the pyroelectric thin film wafer a by ion implantation. The implantation energy of the helium ions is 50 KeV (corresponding to a thickness of about 200 nm of the implantation stop layer in the lithium niobate crystal) and the dose is 1×10 16 ions / cm 2 , the injection surface is the polarization surface of +Z, forming a thin film wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer;
[0055] 4) Using a plasma bonding method, the +Z polarization plane of the ion-implanted pyroelectric film wafer a in step 3) is bonded to the silicon dioxide layer of the substrate wafer in step 1) for the first time to obtain a bonded body a; the structure of the bonded body is, from top to bottom, a lithium niobate film sheet (-Z polarization plane facing away from silicon dioxide), a silicon dioxide isolation layer, and a silicon substrate sheet.
[0056] 5) The bonded body a is kept at a constant temperature of 260° C. to realize the first peeling of the pyroelectric thin film, and to form a pyroelectric elimination layer a with a +Z polarization surface facing the silicon dioxide, that is, to form a pyroelectric elimination layer with a top layer of -Z polarization surface facing away from the silicon dioxide, and the pyroelectric elimination layer a is polished and thinned to 20 nm, with a surface roughness of <0.5 nm, to obtain a bonded body a having a pyroelectric elimination layer;
[0057] 6) A pyroelectric thin film wafer b is provided. The pyroelectric thin film wafer b is a z-cut lithium niobate wafer with a size of 4 inches. The smooth surface is cleaned and helium ions (He+) are implanted into the pyroelectric thin film wafer b by ion implantation. The implantation energy of the helium ions is 400 KeV and the dose is 5×10 16 ions / cm 2 , the injection surface is the polarization surface of -Z, forming a thin film wafer having a three-layer structure of a thin film layer, a separation layer and a residual material layer;
[0058] 7) The implantation surface (-Z polarization surface) of the pyroelectric thin film wafer b implanted with ions in step 6) is bonded for the second time with the -Z polarization surface (facing away from the silicon dioxide layer) of the pyroelectric elimination layer bonding body a having the pyroelectric elimination layer obtained in step 5) to obtain a bonding body b; the structure of the bonding body b is, from top to bottom, lithium niobate wafer b (+Z polarization surface facing away from the first bonding body), pyroelectric elimination layer (-Z polarization surface facing away from silicon dioxide), silicon dioxide isolation layer, and silicon substrate;
[0059] 8) The bonded body b is kept at a constant temperature of 300°C to achieve the second peeling of the pyroelectric film sheet, forming a pyroelectric film layer with a +Z polarization plane facing away from the bonded body b. At this time, the thickness of the pyroelectric film layer is about 1100nm. Finally, the pyroelectric film layer is polished and thinned to 900nm (50nm-20μm) to obtain a second bonded body with a pyroelectric film layer, forming the final single-domain nano-scale pyroelectric single crystal film. The structure of the single-domain nano-scale pyroelectric single crystal film is as follows: Figure 2 shown.
Claims
1. A method for preparing a single-domain nanoscale pyroelectric single crystal thin film, comprising the following steps: 1) providing a substrate wafer, and after cleaning, preparing a layer of silicon dioxide as an isolation layer on the substrate wafer; 2) providing a pyroelectric thin film wafer a, and after cleaning, implanting helium ions (He+) into the pyroelectric thin film wafer a by ion implantation; 3) performing a first bonding of the +Z polarization plane of the pyroelectric thin film wafer a implanted with ions in step 2) with the silicon dioxide layer of the substrate wafer in step 1) to obtain a bonding body a; 4) Keeping the bonded body a at a constant temperature of 150° C. to 400° C. to achieve the first peeling of the pyroelectric thin film to form a pyroelectric elimination layer a with a +Z polarization surface facing the silicon dioxide; 5) providing a pyroelectric thin film wafer b, and after cleaning, implanting helium ions (He+) into the pyroelectric thin film wafer b by ion implantation; 6) performing a second bonding between the -Z polarization plane of the pyroelectric thin film wafer b implanted with ions in step 5) and the -Z polarization plane of the pyroelectric elimination layer of the bonding body a obtained in step 4) to obtain a bonding body b; 7) The bond body b is kept at a constant temperature of 150° C. to 400° C. to achieve a second peeling of the pyroelectric film sheet, forming a pyroelectric film layer with a +Z polarization plane facing away from the bond body b, and the pyroelectric film layer is polished to obtain a single-domain pyroelectric crystal film b.
2. The preparation method according to claim 1, characterized in that: In step 1), the substrate wafer is selected from silicon, silicon carbide, sapphire, quartz, fused quartz, with a size of 3 to 12 inches and a thickness of 0.2 to 1 mm. The smooth surface of the substrate wafer is cleaned. After cleaning, a layer of silicon dioxide is prepared on the substrate wafer by thermal oxidation, PECVD, LPCVD or CVD. The thickness of the silicon dioxide layer is 50 nm to 5 μm, and the roughness of the silicon dioxide layer is less than or equal to 0.5 nm.
3. The preparation method according to claim 1, characterized in that: In step 2), the pyroelectric film wafer a is lithium niobate, lithium tantalate or silicon carbide, with a size of 3 to 12 inches and a thickness of 0.2 to 1 mm. Preferably, the pyroelectric film wafer a is a z-tangent lithium niobate wafer with a size of 4 inches and an injection surface with a +Z polarization surface.
4. The preparation method according to claim 1, characterized in that: In step 2), the helium ion implantation energy is 30 KeV to 5 MeV, and the dose is 1×10 15 ions / cm 2 ~1×10 17 ions / cm 2 .
5. The preparation method according to claim 1, characterized in that: In step 3), bonding is performed by plasma bonding, and the structure of the bonding body a from top to bottom is a lithium niobate thin film sheet with a -Z polarization plane facing away from silicon dioxide, a silicon dioxide isolation layer, and a silicon substrate sheet.
6. The preparation method according to claim 1, characterized in that: In step 4), the pyroelectric elimination layer a with the +Z polarization plane facing the silicon dioxide is polished and thinned to 5nm-100nm with a surface roughness of less than or equal to 0.5nm, thereby obtaining a bonded body a having a pyroelectric elimination layer.
7. The preparation method according to claim 1, characterized in that: In step 5), the pyroelectric film wafer b is the same as the pyroelectric film wafer a in step 2), but the ion implantation surface is the -Z polarization surface, which is opposite to the implantation surface of the pyroelectric film wafer a. The implantation energy of the helium ions is 30 KeV to 5 MeV, and the dose is 1×10 15 ions / cm 2 ~1×10 17 ions / cm 2 The implantation energy and dosage of helium ions may be the same as or different from those in step 2).
8. The preparation method according to claim 1, characterized in that: In step 6), bonding is performed by plasma bonding, and the injection surface of the ion-implanted pyroelectric film wafer b is bonded for the second time with the pyroelectric elimination layer of the bonding body a obtained in step 4) which is away from the silicon dioxide layer. In step 7), the pyroelectric film layer is polished to thin the pyroelectric film layer to 50nm-20μm.
9. A single-domain nanoscale pyroelectric single crystal thin film, prepared by the method according to any one of claims 1 to 8.
10. The single-domain nanoscale pyroelectric single crystal thin film according to claim 9, characterized in that: The monodomain nanoscale pyroelectric single crystal film is provided with a substrate layer, an isolation layer, a pyroelectric elimination layer, and a pyroelectric film layer in sequence from bottom to top. The pyroelectric film layer material is a lithium niobate or lithium tantalate pyroelectric film layer. The pyroelectric elimination layer material is the same as the pyroelectric film layer material, but the polarity is reversed. The isolation layer is a silicon dioxide or silicon nitride amorphous material, and its refractive index is less than the refractive index of the pyroelectric film layer material. The substrate layer material is silicon, silicon carbide, sapphire, quartz, or fused quartz.
Citation Information
Patent Citations
Making method of lithium tantalate black wafer
CN106544735A
Single crystal single domain piezoelectric film and preparation method thereof
CN110581212A
Formation of polycrystalline silicon thin film
JP1995288228A
Composite single crystal thin film and method for manufacturing composite single crystal thin film
WO2017032199A1
Single-crystal film bonding body and manufacturing method therefor
WO2017092378A1