Post-processing material for absorbent article, absorbent article provided with said post-processing material, and method for manufacturing same
By using a combination of a nonwoven fabric layer and an elastomeric layer in the post-treatment material for absorbent articles, combined with ultrasonic or thermal welding technology, the fixing and appearance problems in post-treatment for absorbent articles are solved, and the absorbent articles are realized The clumping state is maintained and the good treatment effect after use.
Patent Information
- Application Number
- CN202380030730.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-08
- Filing Date
- 2023-04-06
- Publication Date
- 2024-11-12
AI Technical Summary
It is difficult to maintain a clump when discarded by the existing post-treatment material for absorbent articles, and the absorbent articles after use cannot be fully fixed, which affects the appearance and usage experience.
The nonwoven fabric layer and the outer packaging body of the absorbent article are used to form a joint to fix the absorbent article by ultrasonic welding or hot welding technology. And the folded structure and the design of the elastomer layer are maintained in a clump state.
The clumping and appearance optimization of the post-treatment material for absorbent items when discarded is achieved, providing a good hand touch and fixing effect, ensuring that the absorbent items can be processed smoothly after use.
Smart Images

Figure CN118946335A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an absorbent article post-treatment material, an absorbent article having the absorbent article post-treatment material, and a method for producing the same. Background Art
[0002] Absorbent articles such as diapers and sanitary products usually have an absorbent pad that absorbs and retains the excrement discharged from the wearer to the outside of the body, and an outer packaging body that supports the absorbent pad on its inner surface. The absorbent article after use is fixed in a balled state in such a way that the absorbent pad becomes the inside, and is discarded. As a method for fixing the absorbent article after use, a scheme of providing a post-processing belt for the absorbent article has been proposed. The absorbent article directly contacts the skin, so a raw material that is softer and feels better on the skin is used in the outer packaging body. Therefore, a post-processing belt that is also soft and feels good on the skin is proposed (for example, patent document 1). However, the absorbent article obtained by using a softer raw material as an outer packaging body is sometimes unable to fully fix the absorbent article after use. In addition, sometimes the post-processing belt itself cannot be fully fixed to the outer packaging body. Therefore, a post-processing means is sought that can fix and discard the absorbent article in a balled state even if the absorbent article is obtained by using a soft raw material in the outer packaging body and feels good on the skin.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2021-194256 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] The present invention has been made to solve the above-mentioned conventional problems, and an object of the present invention is to provide a post-treatment material for absorbent articles which has excellent appearance and touch and can be fixed / maintained in a balled state when discarded.
[0008] Solutions for solving problems
[0009] The absorbent article post-treatment material according to the embodiment of the present invention comprises a nonwoven fabric layer, a resin layer, and a joining portion, wherein the nonwoven fabric layer comprises a resin layer having a density of 15 kg / m 3 ~120kg / m 3 The nonwoven fabric contains chemical fibers, the resin layer contains an elastomer layer, and the joint part is joined to the outer packaging body of the absorbent article. The nonwoven fabric layer is the outermost surface of the post-processing material for the absorbent article, and the joint part is a part that can be welded by ultrasonic welding or thermal welding.
[0010] In one embodiment, the nonwoven fabric is a spunlace nonwoven fabric, a carded nonwoven fabric, a hot air nonwoven fabric or a spunlace entangled nonwoven fabric.
[0011] In one embodiment, the chemical fiber is an olefin resin fiber.
[0012] In one embodiment, the chemical fiber is a polypropylene resin fiber.
[0013] In one embodiment, the nonwoven fabric contains 30% by weight or more of polypropylene resin fibers.
[0014] In one embodiment, the elastomer layer includes a styrene-based elastomer or an olefin-based elastomer.
[0015] In one embodiment, the elastomer layer includes an olefin-based elastomer.
[0016] In one embodiment, the olefin-based elastomer is a propylene-based elastomer.
[0017] In one embodiment, the above-mentioned post-treatment material for an absorbent article comprises a folded structure.
[0018] In one embodiment, the absorbent article post-treatment material is in a strip shape with a length of 50 mm to 250 mm.
[0019] In one embodiment, the basis weight of the absorbent article post-treatment material is 50 g / m 2 ~150g / m 2 .
[0020] In one embodiment, the post-treatment material for absorbent articles has an elongation at break of 150% to 600%.
[0021] In one embodiment, the maximum strength of the absorbent article post-treatment material is 2 N / 10 mm or more.
[0022] In one embodiment, the post-elongation stress of the absorbent article post-treatment material is 0.5 N / 10 mm or more.
[0023] In one embodiment, the elongation of the absorbent article post-treatment material under a load of 2N is 30% or more.
[0024] Another aspect of the present invention provides an absorbent article having an outer packaging body and the absorbent article post-treatment material.
[0025] In one embodiment, in the absorbent article, the outermost surface of the outer packaging body is a nonwoven fabric having a density of 15 kg / m 3~120kg / m 3 .
[0026] In one embodiment, the absorbent article is a pants-type diaper.
[0027] Another aspect of the present invention provides a method for manufacturing an absorbent article. The method comprises: laminating a nonwoven fabric layer and a resin layer including an elastomer layer to produce a laminate, wherein the nonwoven fabric layer includes a resin layer having a density of 15 kg / m 3 ~120kg / m 3 The laminate is connected to the outer packaging of the absorbent article by ultrasonic welding or thermal welding.
[0028] Effects of the Invention
[0029] According to the present invention, there can be provided a post-treatment material for absorbent articles which has excellent appearance and touch and can be fixed / maintained in a balled state when discarded. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a schematic perspective view of an absorbent article including the absorbent article post-treatment material according to the embodiment of the present invention.
[0031] Figure 2 This is a schematic cross-sectional view of the post-treatment material for an absorbent article according to an embodiment of the present invention.
[0032] Figure 3 This is a schematic cross-sectional view showing the state of the absorbent article post-treatment material according to the embodiment of the present invention when in use.
[0033] Figure 4 This is a schematic perspective view showing an absorbent article fixed with the absorbent article post-treatment material according to the embodiment of the present invention.
[0034] Figure 5 Yes means Figure 4 The schematic perspective view of the back side of the absorbent article fixed with the post-treatment material for the absorbent article is shown. DETAILED DESCRIPTION
[0035] A. Overview of post-treatment materials for absorbent articles
[0036] The post-treatment material for absorbent articles (hereinafter also referred to as "post-treatment material") according to an embodiment of the present invention comprises a nonwoven fabric layer, a resin layer, and a joining portion. The nonwoven fabric layer comprises a resin layer having a density of 15 kg / m 3 ~120kg / m 3The nonwoven fabric contains chemical fibers, the resin layer contains an elastomer layer, and the joint is joined to the outer packaging of the absorbent article. The nonwoven fabric layer is the outermost surface of the post-processing material for the absorbent article. The joint is a portion that can be welded by ultrasonic welding or thermal welding. If the outermost surface of the post-processing material is a density of 15kg / m 3 ~120kg / m 3 If a nonwoven fabric is used, a post-processing material with excellent appearance and touch can be provided. In addition, if the joint portion of the absorbent article that is joined to the outer packaging body is a portion that can be welded to the outer packaging body by ultrasonic welding or thermal welding, the post-processing material can be firmly fixed to the absorbent article. The post-processing material of an embodiment of the present invention is easy to stretch and easy to post-process during use, and after being fixed, the absorbent article can be kept in a balled state, for example. Typically, the post-processing material of an embodiment of the present invention is in the form of a strip. For example, the above-mentioned joint portion is provided at both ends of the post-processing material in the form of a strip.
[0037] Figure 1 2 is a schematic perspective view of an absorbent article having a post-processing material for an absorbent article according to an embodiment of the present invention. In the illustrated example, the absorbent article 200 is a pants-type diaper. The absorbent article 200 as a pants-type diaper has an outer packaging body composed of an abdominal side outer member 210 and a back side outer member 220 of the wearer. Figure 2 It is a schematic cross-sectional view of the post-processing material for absorbent articles according to the embodiment of the present invention. It should be noted that the illustrated example shows a state in which the joint portion 30 is joined to the back-side external component 220 of the outer packaging body. In the illustrated example, in order to illustrate the structure of the post-processing material according to the embodiment of the present invention, there is a space between the post-processing material 100 and the back-side external component 220. In the actual use method, the folded post-processing material 100 can be in contact with the outer packaging body (for example, the back-side external component 220) until it is used as the post-processing material. In the illustrated example, the post-processing material 100 for absorbent articles is in the shape of a strip, which includes a resin layer 10 including an elastomer layer and non-woven fabric layers 20a, 20b. The non-woven fabric layer 20a is the outermost layer of the post-processing material 100, and includes a density of 15kg / m 3 ~120kg / m 3And a nonwoven fabric containing chemical fibers. If there is such a laminated structure, a post-processing material comprising a joint portion that can be welded to an absorbent article by ultrasonic welding or thermal welding can be obtained. In addition, if the nonwoven fabric is the outermost surface, a post-processing material with excellent appearance and hand touch can be provided. In the example shown in the figure, both sides of the resin layer 10 including the elastomer layer are nonwoven fabric layers, but the nonwoven fabric layer 20b on the outer packaging side of the absorbent article can be omitted. The post-processing material 100 includes a joint portion 30 joined to the outer packaging of the absorbent article (for example, the back side external member 220). In the example shown in the figure, the joint portion 30 is arranged at both ends of the length direction of the post-processing material 100. In the example shown in the figure, the back side external member 220 of the absorbent article 200 is a nonwoven fabric. When the outer packaging is a nonwoven fabric, especially a nonwoven fabric with excellent softness, it is sometimes impossible to firmly fix the post-processing material 100 to the outer packaging. When the joint 30 can be welded by ultrasonic welding or heat welding, even if the outer packaging body is a nonwoven fabric with excellent softness, the post-processing material and the absorbent article can be firmly fixed. The outer packaging body supports an absorbent pad (not shown) that absorbs excrement, etc. inside (the side in contact with the wearer). In the example shown in the figure, the post-processing material 100 is joined to the upper part of the back side external member 220 (the waist part 230 side of the absorbent article 200). The post-processing material 100 is joined to any and appropriate position of the absorbent article 200 according to the size, etc.
[0038] In the example shown in the figure, the post-processing material 100 is in a strip shape. The strip-shaped post-processing material 100 has two folding structures at both ends, namely, a Z-shape (right side of the example shown in the figure) or a reverse Z-shape (left side of the example shown in the figure). The post-processing material 100 having the folding structure has excellent handling properties of the absorbent article until it is used, and when used for post-processing, the post-processing material can be unfolded and easily fixed after use.
[0039] An example of a method for performing post-processing using the post-processing material according to the embodiment of the present invention will be described. Figure 3It is a schematic cross-sectional view showing the form of the absorbent article post-processing material described in an embodiment of the present invention when in use. In the illustrated example, during post-processing, the folded structure is unfolded by stretching the portion of the post-processing material 100 that is not fixed to the back side external member 220 toward the upper part (for example, in the direction opposite to the outer packaging body). The unfolded post-processing material 100 forms an annular structure with the back side external member 220 of the outer packaging body. As described above, the post-processing material 100 includes a resin layer 10 containing an elastomer layer. The post-processing material 100 including the resin layer 10 containing an elastomer layer can be stretched compared to the original length by further stretching after unfolding. As a result, the hollow portion of the annular structure formed by the post-processing material 100 and the back side external member 220 can be enlarged, and the absorbent article that is kneaded into a ball can be easily passed through the annular structure. Figure 4 This is a schematic perspective view showing an absorbent article fixed with the absorbent article post-treatment material according to the embodiment of the present invention. Figure 5 Yes means Figure 4 The schematic perspective view of the back of the absorbent article fixed with the post-treatment material for absorbent articles is shown in FIG. By stopping the extension of the post-treatment material 100, the stretched post-treatment material is restored to its original length due to the elastic recovery of the resin layer (specifically, the elastomer layer contained in the resin layer). As a result, the balled absorbent article can be fixed in a balled state and can be easily discarded. Figure 4 As shown in the figure, the post-processing material 100 is joined to the back side outer member 220 by the joining portion 30, and even when the post-processing material 100 is stretched for fixing, the joining state between the absorbent article and the post-processing material can be well maintained. Figure 5 As shown in the figure, on the surface opposite to the joint 30, the center of the balled absorbent article is maintained fixed by the elastically restored post-processing material 100, for example, it is possible to prevent the fixed state from loosening when discarded and exposing the internal absorbent pad to the surface.
[0040] The post-processing material 100 can be set to any and appropriate size that can fix the absorbent article after use and fix / maintain the balled state when discarded. As described above, in one embodiment, the post-processing material 100 is in the form of a strip. The length of the strip-shaped post-processing material is preferably 50 mm or more, more preferably 70 mm or more, and further preferably 100 mm or more. In addition, the length of the strip-shaped post-processing material is preferably 250 mm or less, more preferably 230 mm or less, and further preferably 200 mm or less. In one embodiment, the length of the strip-shaped post-processing material is preferably 50 mm to 250 mm, more preferably 70 mm to 230 mm, and further preferably 100 mm to 200 mm. When the length of the post-processing material is less than 50 mm, it is possible that the hollow part becomes smaller and the balled absorbent article is difficult to fix. When the length of the post-processing material exceeds 250 mm, the productivity of the post-processing material decreases and the cost may increase. The width of the post-processing material is, for example, 8 mm or more, preferably 9 mm or more. The width of the post-processing material is, for example, 30 mm or less, and preferably 25 mm or less. In one embodiment, the width of the post-processing material is, for example, 8 mm to 30 mm, preferably 9 mm to 25 mm. When the width of the post-processing material is within the above range, the balled absorbent article can be fixed and held.
[0041] The basis weight of the post-processed material is preferably 50 g / m 2 More preferably 70g / m 2 More preferably, 90 g / m 2 In addition, the basis weight of the post-processing material is preferably 150 g / m 2 Below, more preferably 130g / m 2 Below, more preferably 120g / m 2 In one embodiment, the basis weight of the post-processing material is 50 g / m 2 ~150g / m 2 , more preferably 70g / m 2 ~130g / m 2 , more preferably 90g / m 2 ~120g / m 2 The basis weight of the post-processed material is less than 50g / m 2 When the post-processing material is more than 150 g / m 2 The cost may become higher.
[0042] The elongation at break of the post-processing material is preferably 150% or more, more preferably 170% or more, and further preferably 180% or more. In addition, the elongation at break of the post-processing material is preferably 600% or less, more preferably 580% or less, and further preferably 560% or less. In one embodiment, the elongation at break of the post-processing material is preferably 150% to 600%, more preferably 170% to 580%, and further preferably 180% to 560%. If the elongation at break is within the above range, the post-processing material can be easily unfolded / stretched, and the absorbent article can be easily fixed. In this specification, the elongation at break refers to: the elongation at break when a sample obtained by cutting a width of 10 mm and a length of 10 cm in a manner that the direction orthogonal to the flow direction of the post-processing material becomes the long side is set in a tensile testing machine in a manner that the distance between the chucks is 50 mm, and stretched at a tensile speed of 500 mm / min until it breaks.
[0043] The maximum strength of the post-processing material is preferably 2N / 10mm or more, more preferably 3N / 10mm or more, and further preferably 4N / 10mm or more. If the maximum strength is within the above range, the breakage of the post-processing material during post-processing can be suppressed. The maximum strength of the post-processing material is as large as possible, for example, 50N / 10mm or more. In one embodiment, the maximum strength of the post-processing material is preferably 2N / 10mm to 50N / 10mm, more preferably 3N / 10mm to 40N / 10mm, and further preferably 4N / 10mm to 30N / 10mm. In this specification, the maximum strength refers to: a sample obtained by cutting a width of 10mm and a length of 10cm in a manner that the direction orthogonal to the flow direction of the post-processing material becomes the long side is arranged in a tensile testing machine in a manner that the distance between the chucks becomes 50mm, and is stretched to the maximum strength at a tensile speed of 500mm / minute until it breaks.
[0044] The post-elongation stress of the post-processing material is preferably 0.5N / 10mm or more, more preferably 0.7N / 10mm or more, and further preferably 0.8N / 10mm or more. In addition, the post-elongation stress of the post-processing material is preferably 4N / 10mm or less, and more preferably 3N / 10mm or less. In one embodiment, the post-elongation stress of the post-processing material is preferably 0.5N / 10mm to 4N / 10mm, more preferably 0.7N / 10mm to 4N / 10mm, and further preferably 0.8N / 10mm to 3N / 10mm. If the post-elongation stress is within the above range, the state in which the balled absorbent article is fixed can be well maintained. In this specification, the post-elongation stress refers to the stress when a sample obtained by cutting the sample with a width of 10 mm and a length of 10 cm in a manner that the direction perpendicular to the flow direction of the post-processed material becomes the long side is set in a tensile testing machine in a manner that the distance between chucks becomes 50 mm, and is stretched to an elongation of 100% at a tensile speed of 500 mm / min and maintained for 10 minutes, and then restored to the initial distance between chucks.
[0045] The elongation of the post-processing material under a 2N load is preferably 30% or more, more preferably 35% or more, and further preferably 40% or more. In addition, the elongation under a 2N load is preferably 200% or less, more preferably 150% or less, and further preferably 100% or less. In one embodiment, the elongation of the post-processing material under a 2N load is 30% to 200%, more preferably 35% to 150%, and further preferably 40% to 100%. If the elongation under a 2N load is within the above range, the post-processing material can be easily unfolded and the absorbent article can be easily fixed. In this specification, the elongation under a 2N load refers to: a sample obtained by cutting a width of 10 mm and a length of 10 cm in a manner that the direction orthogonal to the flow direction of the post-processing material becomes the long side is set in a tensile testing machine in a manner that the distance between the chucks becomes 50 mm, and is stretched at a tensile speed of 500 mm / min until the load reaches 2N.
[0046] The thickness of the post-processing material can be set to an arbitrary and appropriate value. The thickness of the post-processing material is preferably 0.5 mm or more, more preferably 0.7 mm or more, and further preferably 0.8 mm or more. In addition, the thickness of the post-processing material is preferably 2 mm or less, more preferably 1.5 mm or less, and further preferably 1.2 mm or less. In one embodiment, the thickness of the post-processing material is preferably 0.5 mm to 2 mm, more preferably 0.7 mm to 1.5 mm, and further preferably 0.8 mm to 1.2 mm. By making the thickness within the above range, it can be suitably used as a component of an absorbent article. In this specification, the thickness of the post-processing material refers to: using a digital microscope (e.g., a digital microscope "VHX-1000" manufactured by Keyence Corporation), photographing a cross-section of the post-processing material, and measuring it using image analysis software. The value obtained. It should be noted that in the thickness measurement, when the outermost surface of the post-processed material is a nonwoven fabric, in the side section of the nonwoven fabric (the upper or lower part of the post-processed material), 10 parallel lines whose intersections with the fibers are set as the upper side and the lower side, and the length between the upper side and the lower side is set as the thickness of the post-processed material.
[0047] B. Nonwoven fabric layer
[0048] The nonwoven fabric layer is the outermost layer of the post-processing material. The nonwoven fabric layer contains a density of 15 kg / m 3 ~120kg / m 3 And nonwoven fabric containing chemical fibers. Preferably: density is 15kg / m 3 ~120kg / m 3 The nonwoven fabric containing chemical fibers becomes the outermost surface of the post-processing material. The nonwoven fabric has excellent softness and hand touch, and when joined to an absorbent article, the fusion appearance with the nonwoven fabric used in the outer packaging of the absorbent article is also excellent. The nonwoven fabric layer can be a single layer or a laminate of two or more layers. When it is a laminate of two or more layers, the nonwoven fabric that becomes the outermost surface only needs to have a density of 15 kg / m 3 ~120kg / m 3 And the non-woven fabric containing chemical fibers can be used.
[0049] The nonwoven fabric is preferably a spunlace nonwoven fabric, a carded nonwoven fabric, a hot air nonwoven fabric or a spunlace entangled nonwoven fabric. If it is such a nonwoven fabric, the appearance of the nonwoven fabric surface is excellent and it can also be integrated with the outer packaging body of the absorbent article.
[0050] As mentioned above, the nonwoven fabric is a nonwoven fabric containing chemical fibers. If it is a nonwoven fabric of chemical fibers, it can be well joined to the outer packaging body of the absorbent article by ultrasonic welding or thermal welding. As the raw materials of chemical fibers, for example, olefins such as polypropylene and polyethylene; polyesters such as polyethylene terephthalate; polyamide, polyurethane, rayon, nylon, acrylic, their copolymers or their blends, etc. can be listed. Olefin resin fibers such as polypropylene and polyethylene can be preferably used, and polypropylene resin fibers are more preferably used. If it is a nonwoven fabric containing olefin resin fibers, chemical odors can be suppressed and it can be well joined to the outer packaging body of the absorbent article.
[0051] The nonwoven fabric preferably comprises more than 30% by weight of the polypropylene resin fiber constituting the fiber of the nonwoven fabric, more preferably comprises more than 45% by weight, and further preferably comprises more than 80% by weight. In the nonwoven fabric, as the fiber constituting the nonwoven fabric, 100% by weight of the polypropylene resin fiber can be included. In one embodiment, the nonwoven fabric comprises 30% to 100% by weight of the polypropylene resin fiber constituting the fiber of the nonwoven fabric, more preferably comprises 45% to 100% by weight, and further preferably comprises 80% to 100% by weight. If the content ratio of the polypropylene resin fiber is the above range, chemical odor can be suppressed and the outer packaging body of the absorbent article can be well joined.
[0052] In the fiber constituting the nonwoven fabric, in the scope that does not damage the effect of the present invention, can comprise arbitrary and suitable other components.As this other component, can list out for example other polymer, thickener, plasticizer, antideterioration agent, pigment, dye, antioxidant, antistatic agent, lubricant, foaming agent, heat stabilizer, light stabilizer, inorganic filler, organic filler etc.They can be only 1 kind, also can be 2 kinds or more.The containing ratio of other components is preferably below 10 weight %, more preferably below 7 weight %, further preferably below 5 weight %, particularly preferably below 2 weight %, most preferably below 1 weight %.
[0053] The density of nonwoven fabric is 15kg / m 3 ~120kg / m 3 The density of the nonwoven fabric is preferably 20 kg / m 3 More preferably 23kg / m 3 In addition, the density of the nonwoven fabric is preferably 115 kg / m 3 Below, more preferably 110kg / m 3 If the density of the nonwoven fabric is within the above range, a post-processed material having excellent appearance and hand feel can be obtained. In one embodiment, the density of the nonwoven fabric is preferably 20 kg / m 3 ~115kg / m3 , more preferably 23kg / m 3 ~110kg / m 3 In this specification, the density of nonwoven fabric (kg / m 3 ) refers to the basis weight of nonwoven fabric (Xg / m 2 ) and the value calculated based on the thickness (Y mm) of the nonwoven fabric measured by the method described below. More specifically, the density (kg / m 3 ) in X / Y (kg / m 3 ) form to calculate.
[0054] Method for measuring thickness of nonwoven fabric: Use a digital microscope (e.g., digital microscope "VHX-1000" manufactured by Keyence Corporation) to photograph the cross section of the post-processed material, and use image analysis software to measure the thickness of the nonwoven fabric. It should be noted that in the thickness measurement, when the resin layer is in contact with the nonwoven fabric, the boundary between the resin layer and the nonwoven fabric is set as the outermost surface, or, when the nonwoven fabrics are in contact with each other, at the upper and lower parts of the cross section of the nonwoven fabric, parallel lines with 10 intersections with the fibers are set as the upper side and the lower side, respectively, and the length between the upper side and the lower side is set as the thickness of the nonwoven fabric.
[0055] The basis weight of the nonwoven fabric is preferably 15 gsm (g / m 2 ) or more, more preferably 20gsm or more, and further preferably 25gsm or more. In addition, the basis weight of the nonwoven fabric is preferably 50gsm or less, more preferably 45gsm or less, and further preferably 40gsm or less. In one embodiment, the basis weight of the nonwoven fabric is 15gsm to 50gsm, more preferably 20gsm to 45gsm, and further preferably 25gsm to 40gsm. The basis weight of the nonwoven fabric can be measured by any and appropriate method. For example, it can be measured by the following method. For cutting the nonwoven fabric into 100cm 2 The weight of the sample was measured using an electronic balance and converted into g / m 2 Unit (gsm), from which the basis weight of the nonwoven fabric can be measured.
[0056] C. Resin layer including elastomer layer
[0057] The resin layer including the elastomer layer may be composed of only the elastomer layer, or may be a laminate of the elastomer layer and other resin layers. The other resin layers may be composed of any and appropriate resins, for example, non-elastomeric resins. In one embodiment, the resin layer has a three-layer structure of an elastomer layer and surface layers arranged on both sides of the elastomer layer.
[0058] The elastomer layer is formed using any and appropriate elastomer resin. As the elastomer resin that becomes the main component of the elastomer layer, for example, olefin elastomers, styrene elastomers, vinyl chloride elastomers, urethane elastomers, ester elastomers, amide elastomers, etc. are listed. Preferably, olefin elastomers or styrene elastomers are used.
[0059] By using olefin elastomer, the post-processing material can be well joined to the outer packaging body, and the chemical odor from the post-processing material can be suppressed. As olefin elastomer, for example, olefin block copolymers, olefin random copolymers, ethylene copolymers, propylene copolymers, ethylene olefin block copolymers, propylene olefin block copolymers, ethylene olefin random copolymers, propylene olefin random copolymers, ethylene propylene random copolymers, ethylene (1-butene) random copolymers, ethylene (1-pentene) olefin block copolymers, ethylene (1-hexene) random copolymers, ethylene (1-heptene) olefin block copolymers, ethylene (1-octene) olefin block copolymers, ethylene (1-nonene) olefin block copolymers, ethylene (1-decene) olefin block copolymers, propylene ethylene olefin block copolymers, ethylene (α-olefin) copolymers, ethylene (α-olefin) random copolymers, ethylene (α-olefin) block copolymers, amorphous polypropylene, their combinations with polyethylene (LLDPE, LDPE, HDPE, etc.), their combinations with polypropylene, or their combinations, etc. The olefin-based elastomer may be used alone or in combination of two or more.
[0060] The density of the olefin elastomer is preferably 0.830 g / cm 3 More preferably 0.835 g / cm 3 More preferably, 0.840 g / cm 3 Above, most preferably 0.845 g / cm 3 In addition, the density of the olefin-based elastomer is preferably 0.90 g / cm 3 Below, more preferably 0.89 g / cm 3 Below, more preferably 0.88 g / cm 3 In one embodiment, the density of the olefin-based elastomer is preferably 0.830 g / cm 3 ~0.90g / cm 3 , more preferably 0.835 g / cm 3 ~0.89g / cm 3 , more preferably 0.840 g / cm 3 ~0.89g / m 3 , particularly preferably 0.845 g / cm 3 ~0.88g / cm 3By setting the density within the above range, it is possible to provide a post-processing material for absorbent articles that can fix / hold absorbent articles in a balled state when discarded. Furthermore, thermal stability and storage stability can be improved. In addition, the process of manufacturing the elastomer layer can be further simplified, and processing costs can be further reduced.
[0061] The melt flow rate (MFR) of the olefin elastomer at 230°C and 2.16 kgf is preferably 1.0 g / 10 min or more, more preferably 2.0 g / 10 min or more. In addition, the MFR of the olefin elastomer at 230°C and 2.16 kgf is preferably 25.0 g / 10 min or less, more preferably 23.0 g / 10 min or less, 21.0 g / 10 min or less, particularly preferably 20.0 g / 10 min or less, and most preferably 19.0 g / 10 min or less. In one embodiment, the MFR of the olefin elastomer at 230°C and 2.16kgf is preferably 1.0g / 10min to 25.0g / 10min, more preferably 2.0g / 10min to 23.0g / 10min, further preferably 2.0g / 10min to 21.0g / 10min, particularly preferably 2.0g / 10min to 20.0g / 10min, and most preferably 2.0g / 10min to 19.0g / 10min. By making the MFR within the above range, a post-processing material for absorbent articles that can fix / maintain absorbent articles in a balled state when discarded can be provided. Furthermore, thermal stability and storage stability can be improved. In addition, the process in the manufacture of the elastomer layer can be further simplified, and processing costs can be further suppressed.
[0062] As the above-mentioned olefin elastomer, α-olefin elastomer is preferably used. Among the α-olefin elastomers, at least one selected from ethylene elastomer, propylene elastomer, and 1-butene elastomer is more preferably used. By using such an α-olefin elastomer as an olefin elastomer, it is possible to provide a post-processing material for absorbent articles that can fix / maintain absorbent articles in a clumped state when discarded. Furthermore, thermal stability and storage stability can be improved. In addition, the process in the manufacture of the elastomer layer and the resin layer can be further simplified, and processing costs can be further suppressed.
[0063] As the α-olefin elastomer, commercially available products can be used. Examples of commercially available products include the "Tafmer" (registered trademark) series manufactured by Mitsui Chemicals (e.g., Tafmer PN-2070, Tafmer PN-3560, etc.); and the "Vistamaxx" (registered trademark) series manufactured by ExxonMobil (e.g., Vistamaxx 3000, Vistamaxx 6202, Vistamaxx 7010, etc.).
[0064] The α-olefin elastomer is preferably produced using a metallocene catalyst. The α-olefin elastomer produced using a metallocene catalyst can provide a post-processing material that can fix / maintain the absorbent article in a balled state when discarded. Furthermore, thermal stability and storage stability can be improved. In addition, the process in the production of the elastomer layer can be further simplified, and processing costs can be further suppressed.
[0065] As styrene-based elastomers, for example, SIS-based elastomers, SBS-based elastomers, etc. can be cited. In addition, as styrene-based elastomers, SIS-based elastomers with specific molecular structures can be used. Specifically, SIS-based elastomers can include SIS-based elastomers (hereinafter also referred to as specific SIS-based elastomers) comprising styrene-isoprene-styrene block copolymer molecular structures having different terminal styrene block chain lengths. By using such SIS-based elastomers, it is possible to provide a post-processing material in which absorbent articles are fixed / maintained in a clumped state when discarded and which has a more excellent skin feel. Only one specific SIS-based elastomer can be used, or two or more can be used in combination.
[0066] Examples of the specific SIS-based elastomer include "Quintac 3390 (SL-159)" (styrene content = 48 wt%) and "Quintac 3620" (styrene content = 14 wt%), both of which are trade names and are manufactured by ZEON Corporation of Japan.
[0067] The MFR of the specific SIS elastomer at 200°C and 5 kgf is preferably 5.0 g / 10 minutes or more, more preferably 6.0 g / 10 minutes or more, and even more preferably 8.0 g / 10 minutes or more. In addition, the MFR of the specific SIS elastomer is preferably 25.0 g / 10 minutes or less, more preferably 23.0 g / 10 minutes or less, even more preferably 21.0 g / 10 minutes or less, particularly preferably 20.0 g / 10 minutes or less, and most preferably 18.0 g / 10 minutes or less. In one embodiment, the MFR of the specific SIS elastomer at 200°C and 5 kgf is preferably 5.0 g / 10 min to 25.0 g / 10 min, more preferably 6.0 g / 10 min to 23.0 g / 10 min, further preferably 8.0 g / 10 min to 21.0 g / 10 min, particularly preferably 8.0 g / 10 min to 20.0 g / 10 min, and most preferably 8.0 g / 10 min to 18.0 g / 10 min. By setting the MFR to the above range, a post-processing material that can fix / maintain the absorbent article in a balled state when discarded and has a better skin feel can be provided. In addition, the manufacturing process of the elastomer layer can be further simplified, and the processing cost can be further suppressed.
[0068] The content of the elastomer resin as the main component in the elastomer layer is preferably 50% by weight or more, more preferably 70% by weight or more, and further preferably 90% by weight or more. In addition, the content of the elastomer resin as the main component is preferably 100% by weight or less, and more preferably 95% by weight or less. By setting the content of the elastomer resin as the main component within the above range, the elastomer layer can exhibit sufficient elastomer properties.
[0069] The elastomer layer may contain any and appropriate other components within the range that does not impair the effect of the present invention. As such other components, for example, other polymers, thickeners, plasticizers, anti-degradation agents, pigments, dyes, antioxidants, antistatic agents, lubricants, foaming agents, heat stabilizers, light stabilizers, inorganic fillers, organic fillers, etc. can be listed. They can be only one kind or two or more kinds. The content ratio of other components in the elastomer layer is preferably 10% by weight or less, more preferably 7% by weight or less, further preferably 5% by weight or less, particularly preferably 2% by weight or less, and most preferably 1% by weight or less.
[0070] As other polymers, any and appropriate polymers can be used. For example, a non-elastomeric resin used in the surface layer described later can be used. The non-elastomeric resin can be used in any and appropriate amount. For example, the non-elastomeric resin contained in the elastomer resin has a content ratio of 50% by weight or less, and is used in a manner such that the total content ratio of the non-elastomeric resin and the above-mentioned elastomer resin is 100% by weight.
[0071] The thickness of the elastomer layer is preferably 20 μm or more, more preferably 30 μm or more. In addition, the thickness of the elastomer layer is preferably 200 μm or less, more preferably 160 μm or less, further preferably 140 μm or less, particularly preferably 120 μm or less, and most preferably 100 μm or less. In one embodiment, the thickness of the elastomer layer is preferably 20 μm to 200 μm, more preferably 20 μm to 160 μm, further preferably 30 μm to 140 μm, particularly preferably 30 μm to 120 μm, and most preferably 30 μm to 100 μm. If the thickness of the elastomer layer is within this range, a post-processing material that can fix / maintain the absorbent article in a clumped state when discarded can be provided.
[0072] The elastic body layer may be a single layer or may be two or more layers. In the case of a laminate of two or more layers, the laminate may have a plurality of layers composed of the same elastic body or a plurality of layers composed of different elastic bodies.
[0073] In one embodiment, the resin layer is composed of three layers. In this embodiment, the resin layer is composed of an intermediate layer and surface layers arranged on both sides of the intermediate layer. The intermediate layer preferably contains a white pigment. By containing a white pigment, an appearance performance suitable for sanitary products can be obtained.
[0074] When the resin layer is composed of three layers, at least one of the surface layer and the middle layer can be a layer composed of the above-mentioned elastomer. The surface layers on both sides of the middle layer can be composed of an elastomeric resin, and the surface layers on both sides can be composed of a non-elastomeric resin. A surface layer composed of an elastomeric resin can be arranged on one side of the middle layer, and a surface layer composed of a non-elastomeric resin can be arranged on the other side. By making the surface layer composed of an elastomeric resin, the stretchability of the post-processing material is improved, and it is easy to fix / maintain it in a balled state when discarding sanitary products. As a result, it is easier to discard sanitary products. By making the surface layer composed of a non-elastomeric resin, it is possible to suppress adhesion when the resin layer is made into a winding body. In addition, the processability (cutting property) of the resin layer can be improved. Preferably, the middle layer is composed of an elastomeric resin, and the surface layers on both sides of the middle layer are composed of a non-elastomeric resin.
[0075] As the non-elastomeric resin, any appropriate resin may be used. In the present specification, the non-elastomeric resin refers to a resin other than the above-mentioned elastomeric resin. As the non-elastomeric resin, a non-elastomeric olefin-based resin is preferably used.
[0076] Examples of the non-elastomeric olefin resins include homopolymers of α-olefins, copolymers of two or more α-olefins, block polypropylene, random polypropylene, copolymers of one or more α-olefins and other vinyl monomers, etc. Examples of the copolymerization form in the copolymer include block form and random form.
[0077] Examples of the α-olefin include α-olefins having 2 to 12 carbon atoms. Examples of such α-olefins include ethylene, propylene, 1-butene, and 4-methyl-1-pentene.
[0078] Examples of homopolymers of α-olefins include polyethylene (PE), homopolypropylene (PP), poly(1-butene), and poly(4-methyl-1-pentene). Examples of polyethylene (PE) include low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE). The structure of homopolypropylene (PP) may be any of isotactic, atactic, and syndiotactic.
[0079] Examples of the copolymer of two or more α-olefins include ethylene / propylene copolymers, ethylene / 1-butene copolymers, ethylene / propylene / 1-butene copolymers, ethylene / α-olefin copolymers having 5 to 12 carbon atoms, and propylene / α-olefin copolymers having 5 to 12 carbon atoms.
[0080] Examples of the copolymer of one or more α-olefins and other vinyl monomers include ethylene / vinyl acetate copolymers, ethylene / alkyl acrylate copolymers, ethylene / alkyl methacrylate copolymers, and ethylene-non-conjugated diene copolymers.
[0081] As the non-elastomeric olefin resin, HDPE, LDPE, LLDPE, homopolypropylene (h-PP), block polypropylene (b-PP), random polypropylene (r-PP) and mixtures thereof are preferably used. By using these resins, it is possible to suppress the adhesion when the resin layer is made into a winding body. In addition, the processability (cutting property) of the resin layer can be improved. Furthermore, the chemical odor from the post-processing material can be suppressed. In addition, it can be well bonded with the outer packaging body of the absorbent article.
[0082] In one embodiment, the non-elastomeric resin is preferably a propylene resin, more preferably a random polypropylene. The content of the random polypropylene in the non-elastomeric resin is preferably 50% by weight or more, more preferably 70% by weight or more, and further preferably 90% by weight or more.
[0083] The resin layer can include any and appropriate other components within the scope of not damaging the effect of the present invention. As such other components, for example, release agents, ultraviolet light absorbers, heat stabilizers, fillers, lubricants, colorants (dyes, etc.), antioxidants, anti-eye mucus agents, anti-adhesion agents, foaming agents, polyethyleneimine, etc. can be listed. They can be only one or more than two. The proportion of other components in the resin layer is preferably less than 10 weight %, more preferably less than 7 weight %, further preferably less than 5 weight %, particularly preferably less than 2 weight %, and most preferably less than 1 weight %.
[0084] When the elastomer layer has an intermediate layer and a surface layer, the thickness of the intermediate layer and the surface layer can be set to any and appropriate values in such a way that the thickness of the elastomer layer is within the above range. The thickness of the intermediate layer is preferably 18 μm or more, more preferably 28 μm or more. In addition, the thickness of the intermediate layer is preferably 94 μm or less, more preferably 56 μm or less, and further preferably 46 μm or less. In one embodiment, the thickness of the intermediate layer is preferably 18 μm to 94 μm, more preferably 28 μm to 56 μm. The thickness of the surface layer is preferably 1 μm or more. In addition, the thickness of the surface layer is preferably 4 μm or less, more preferably 3 μm or less, and further preferably 2 μm or less. In one embodiment, the thickness of the surface layer is preferably 1 μm to 4 μm, more preferably 1 μm to 3 μm, and further preferably 1 μm to 2 μm. The thickness of the surface layer arranged on both sides of the intermediate layer is preferably set to the same thickness.
[0085] D.Joint
[0086] The joint is a part that can be welded by ultrasonic welding or thermal welding. If it is a joint that can be welded by ultrasonic welding or thermal welding, even when a soft nonwoven fabric is used as the outer packaging body of the absorbent article, the post-processing material can be firmly joined to the absorbent article. In addition, by not using an adhesive or bonding agent, the manufacturing process can be reduced, and the environmental burden caused by chemical substances can be reduced. For example, if a nonwoven fabric layer containing a nonwoven fabric containing chemical fibers is laminated with a resin layer containing an elastomer layer to obtain a post-processing material, a post-processing material containing a joint can be made.
[0087] Typically, the joint is formed at both ends of the strip-shaped post-processing material in the longitudinal direction. The joint can be set to any appropriate size (area). The area of the joint is preferably 25 mm 2 More than 30 mm is more preferred 2 In addition, the area of the joint is preferably 200m 2 Less than, more preferably 100m 2 In one embodiment, the area of the joint is preferably 25 mm 2 ~200mm 2 , preferably 30 mm 2 ~100mm 2 If the size of the joining portion is within the above range, the post-processing material and the absorbent article can be firmly joined, and the post-processing material can be prevented from falling off from the absorbent article during post-processing. It should be noted that when joining by the embossed pattern described later, the size of the portion forming the embossed pattern can be within the above range.
[0088] The joint portion may be joined over the entire surface or may be a joint portion having an embossed pattern that has been embossed. The embossed pattern may be in any appropriate shape. Specific examples of the embossed pattern include, for example, a continuous lattice, a discontinuous lattice, a continuous curve, a discontinuous curve, a continuous zigzag, a discontinuous zigzag, a continuous straight line, a discontinuous straight line, a circle (e.g., a dot), an ellipse, a hollow circle, a hollow ellipse, an arc, a hollow arc, and the like.
[0089] The ratio of the area of the welded portion based on the embossed pattern to the area of the entire joint portion (hereinafter sometimes referred to as the "embossed welded area ratio") is preferably 10% or more, more preferably 15% or more, further preferably 20% or more, and particularly preferably 30% or more. In addition, the embossed welded area ratio is preferably 100% or less, more preferably 80% or less, further preferably 60% or less, and particularly preferably 50% or less. In one embodiment, the embossed welded area ratio is preferably 10% to 100%, more preferably 15% to 80%, further preferably 20% to 60%, and particularly preferably 30% to 50%. If the embossed welded area ratio is within the above range, the post-processing material can be firmly joined to the absorbent article, and the post-processing material can be prevented from falling off from the absorbent article during post-processing.
[0090] The embossing depth and the thickness of the welded portion based on the embossing pattern can be set to any appropriate value. The embossing depth is, for example, 0.1 mm to 2.0 mm. The thickness of the welded portion based on the embossing pattern is, for example, 100 μm or less.
[0091] D-1. Ultrasonic welding
[0092] The ultrasonic bonding can be performed by any appropriate method. If the bonding portion is formed by ultrasonic bonding, the post-processing material and the absorbent article can be more firmly bonded. Furthermore, the generation of unique odors from adhesives and adhesives can be further suppressed, and the environmental burden caused by adhesives and adhesives can be suppressed. In addition, the manufacturing process can be reduced.
[0093] Specifically, ultrasonic welding is performed by placing the components to be joined (such as the outer packaging of post-processing materials and absorbent articles) between a component that sends vibration energy through ultrasound (commonly referred to as a "horn") and a roller-shaped component (commonly referred to as an "anvil"). Usually, the horn is vertically arranged above the components to be joined and the anvil. The horn usually vibrates at 20,000 Hz to 40,000 Hz and conducts energy to the components to be joined under pressure, usually in the form of frictional heat. Using frictional heat and pressure, a portion of at least one of the components to be joined is softened or melted, thereby joining the layers.
[0094] The pressing force between the horn and the anvil in ultrasonic welding is preferably 100N to 1500N, more preferably 300N to 1300N, further preferably 500N to 1100N, and particularly preferably 700N to 1000N. By setting the pressing force between the horn and the anvil in ultrasonic welding within the above range, the softness is further improved, and a better hand touch can be achieved. In addition, the production speed can be further increased.
[0095] In one embodiment, ultrasonic welding is typically performed by a method known as "continuous ultrasonic welding joining". Continuous ultrasonic welding joining is typically used to seal a joining object component that can be supplied to a joining device approximately continuously. In continuous ultrasonic welding joining, the horn is typically fixed and the joining object component moves directly below it. A continuous ultrasonic welding joining uses a fixed horn and a rotating anvil surface. In continuous ultrasonic welding joining, the joining object component is stretched between the horn and the rotating anvil. The horn typically extends toward the joining object component and along the length direction, and the vibration moves axially along the horn to the material.
[0096] In another embodiment, the horn is of a rotating type, cylindrical, and rotates around its longitudinal axis. The input vibration exists in the axial direction of the horn, and the output vibration exists in the radial direction of the horn. The horn is arranged next to the anvil, and the anvil can also rotate in such a way that the joining object member passes between the cylindrical surfaces at a linear velocity substantially equal to the tangential velocity of the cylindrical surface.
[0097] Ultrasonic welding is described in, for example, Japanese Patent Application Laid-Open Nos. 2008-526552, 2010-195044, 2013-231249, 2015-16294, and U.S. Patent No. 5,976,316, and the disclosures thereof are incorporated herein by reference.
[0098] In one embodiment, the surface of the rotary anvil preferably has an embossed pattern. A specific example of such an embossed pattern is as described above. The embossed pattern on the surface of the rotary anvil is disclosed, for example, in Japanese Patent Publication No. 2017-65253. The disclosure thereof is incorporated herein by reference.
[0099] The shape of the front end portion (the portion in contact with the member to be joined) of the convex portion constituting the embossed pattern can be set to an arbitrary and appropriate shape, for example, a circle. When using an embossed pattern with a circular front end portion, the diameter of the circular portion is preferably greater than 0.4 mm, more preferably greater than 0.45 mm, and further preferably greater than 0.5 mm. In addition, the diameter of the circular portion is preferably less than 1 mm, more preferably less than 0.9 mm, and further preferably less than 0.8 mm. By making the diameter within the above range, the productivity and bonding strength of the post-processing material can be taken into account. The embossing depth is preferably greater than 0.5 mm. In addition, the embossing depth is preferably less than 1.5 mm, and more preferably less than 1 mm. By making the embossing depth within the above range, the productivity and bonding strength of the post-processing material can be taken into account.
[0100] In addition, from the viewpoint of stabilizing the quality of the obtained post-processing material, it is preferred to adjust the temperature of the anvil to an arbitrary and appropriate temperature and perform ultrasonic welding. When the deviation of the anvil temperature is too large, there is a problem that the bonding strength also deviates and the post-processing material with stable quality cannot be obtained. The temperature of the anvil can be set to 5°C to 90°C, for example, with an absolute thermometer, and the temperature is adjusted in a manner that the temperature of the anvil becomes the set temperature ±5°C. By making the temperature of the anvil within the above range, it is possible to prevent the reduction in productivity caused by condensation, etc., and it is possible to prevent the adverse effects on the product characteristics caused by the curing of the resin layer containing the nonwoven fabric and the elastomer layer.
[0101] D-2. Thermal welding
[0102] The joining by heat fusion can be performed by any appropriate method. For example, the heat fusion portion can be formed by forming the joining portion using a heated embossing pattern roll. The heating temperature is preferably 150°C to 220°C, more preferably 160°C to 210°C, and further preferably 170°C to 200°C.
[0103] E. Method for manufacturing post-processed materials
[0104] The post-processing material can be manufactured by any and appropriate method. For example, (1) a method of laminating a resin layer containing an elastomer layer formed by extruding from a T-die of an extruder with a non-woven fabric layer extracted from a roll; (2) a method of simultaneously extruding and laminating a resin layer containing an elastomer layer and a non-woven fabric layer; (3) a method of bonding a resin layer containing an elastomer layer and a non-woven fabric layer prepared separately with an adhesive; (4) a method of bonding a resin layer containing an elastomer layer and a non-woven fabric layer based on heat lamination or ultrasound. As a bonding method, ultrasonic bonding (ultrasonic fusion bonding) can be preferably cited. If ultrasonic bonding is used, no adhesive is used, so the process of forming an adhesive layer can be omitted, and carbon dioxide emissions can be reduced. In addition, the methods of heat lamination and ultrasonic bonding that can reduce the environmental burden caused by chemical substances and the pollution caused to other materials during the manufacturing stage are as described above.
[0105] In one embodiment of the present invention, the nonwoven fabric layer and the resin layer including the elastomer layer can be bonded by any and appropriate adhesive. Preferably, a hot melt adhesive is used. By using a hot melt adhesive, the necessity of adding a thickener as a component of the resin layer is reduced, for example, the extrusion stability is improved, and the problem of the thickener adhering to the forming roller can be suppressed. In addition, the problem of production line contamination caused by volatile component contamination caused by the thickener can be suppressed.
[0106] The hot melt adhesive can be applied to the entire surface of the nonwoven fabric layer or to a portion of the nonwoven fabric layer. When the hot melt adhesive is applied to a portion of the nonwoven fabric layer, the hot melt adhesive is preferably applied in a manner that includes at least the end of the nonwoven fabric layer. The hot melt adhesive can be applied to the nonwoven fabric and / or the resin layer by any and appropriate method.
[0107] As the hot melt adhesive, any and appropriate adhesive can be used. For example, hot melt adhesives containing styrene elastomers, hot melt adhesives containing olefin polymers, etc. can be listed. Preferably, it is a hot melt adhesive containing a styrene polymer. As such a styrene polymer, for example, a polymer containing SIS, a polymer containing SBS, their respective hydrogenates and their blends can be listed. The hot melt adhesive can be used only one type, or two or more types can be used in combination. In addition, when the hot melt adhesive contains a styrene polymer, the styrene polymer can be only one type, or it can be two or more types. When the hot melt adhesive contains a styrene polymer, the content of the styrene polymer in the hot melt adhesive is preferably 10% by weight to 90% by weight.
[0108] Hot melt adhesive can also include any and appropriate other components. As such other components, for example liquid paraffin, thickener, antioxidant, ultraviolet absorber, light stabilizer, fluorescent agent etc. can be listed. Such other components can be only one kind, or more than two kinds. These other components can be used in any and appropriate amount.
[0109] The post-processed material may be further activated after lamination. The activation process may be performed by any and appropriate method. Specifically, the post-processed material may be stretched along the width direction and / or the length direction, and the fiber structure of a portion of the nonwoven fabric layer may be mechanically destroyed. The elongation of the post-processed material after the activation process is further improved, and the post-processing of the balled absorbent article may be performed more easily.
[0110] F. Absorbent articles
[0111] The absorbent article of the embodiment of the present invention comprises an outer packaging body and the above-mentioned post-processing material. By having the above-mentioned post-processing material, an absorbent article that can be easily post-processed can be provided. As the absorbent article, for example, shorts-type diapers, belt-type diapers, sanitary products, etc. can be listed. Preferably, shorts-type diapers. Hereinafter, the absorbent article as shorts-type diapers will be specifically described.
[0112] The structure of the shorts-type diaper is not particularly limited, and all known structures can be used. Examples of shorts-type diapers include diapers with an absorbent pad and an outer packaging body, the outer packaging body supporting the absorbent pad on its inner surface and having a shorts-type outer shape. The absorbent pad at least includes: a liquid-permeable top sheet, a liquid-impermeable back sheet, and an absorbent body arranged between them and absorbing and retaining body fluids that penetrate through the top sheet. The outer packaging body is divided into, for example: an abdominal external member that mainly abuts against the wearer's abdomen; a dorsal external member that mainly abuts against the wearer's back; and a lower crotch member sandwiched between the abdominal external member and the dorsal external member, mainly abutting against the wearer's crotch, and mainly supporting the absorbent pad. The dorsal external member can be composed of multiple parts. As the part constituting the dorsal external member, for example, a back layer sheet external member and a waist portion external member can be listed. The post-processing material can be joined to the back layer sheet external member or to the waist portion external member. Alternatively, one end of the post-processing material may be joined to the back layer sheet external member, and the other end may be joined to the waist portion external member. The outer packaging body may include an outer packaging body having a side seal portion that joins two edges of the ventral outer member and the dorsal outer member in the width direction, and having a waist opening and a pair of leg openings in the width direction. Here, the ventral outer member and the dorsal outer member may be roughly symmetrical with the crotch member as the center.
[0113] The outermost surface of the outer packaging body is preferably a nonwoven fabric, and more preferably a density of 15 kg / m 3 ~120kg / m 3 When the nonwoven fabric is the outermost surface of the outer packaging body, an absorbent article with good touch and excellent softness can be provided. The density of the nonwoven fabric is preferably 20 kg / m 3 More preferably 23kg / m 3 In addition, the density of the nonwoven fabric is preferably 115 kg / m 3 Below, more preferably 110kg / m 3 If the density of the nonwoven fabric is within the above range, the appearance and hand feel are excellent. In one embodiment, the density of the nonwoven fabric is preferably 20 kg / m 3 ~115kg / m 3 , more preferably 23kg / m 3 ~110kg / m 3 .
[0114] The most superficial nonwoven fabric that becomes the outer packaging body is preferably spunlace nonwoven fabric, carded nonwoven fabric, hot air nonwoven fabric or spun-laid spunlace interwoven nonwoven fabric. As the nonwoven fabric used in the outer packaging body, the nonwoven fabric identical with the nonwoven fabric used in the above-mentioned post-processing material can be listed. The nonwoven fabric used in the post-processing material can be the same as or different from the nonwoven fabric used in the outer packaging body.
[0115] In the absorbent article according to the embodiment of the present invention, the post-processing material is joined by ultrasonic welding or thermal welding. The method of ultrasonic welding or thermal welding is as described above.
[0116] Example
[0117] Hereinafter, the present invention will be specifically described by examples, but the present invention is not limited to these examples at all. It should be noted that the evaluation methods in the examples etc. are as follows. In addition, if not specifically described, parts refer to parts by weight, and % refers to % by weight.
[0118] [Example 1]
[0119] The resin layer (hereinafter also referred to as elastic film) was extruded and molded using two types of three-layer (A layer / B layer / A layer) extrusion T-die molding machines. Specifically, 100 parts by weight of olefin resin 1 (manufactured by SCG Performance Chemicals, trade name: P756C) were added to the A layer of the extruder, 46.5 parts by weight of olefin elastomer 1 (manufactured by ExxonMobil, trade name: Vistamaxx 6202), 46.5 parts by weight of olefin elastomer 2 (manufactured by Mitsui Chemicals, trade name: Tafmer PN-3560), and 7 parts by weight of white pigment (titanium oxide, manufactured by Ampacet, trade name: White PE MB 111413) were added to the B layer of the extruder, and a film with a basis weight of 45 g / m was extruded and molded. 2 (A layer / B layer / A layer=4% / 92% / 4%) Elastic film 1. Extrusion temperature was carried out under the following conditions: A layer: 200°C, B layer: 230°C, die temperature: 230°C.
[0120] Nonwoven fabric A (polypropylene (PP) carded type, basis weight = 24 gsm) was directly laminated on both sides of the obtained elastic film 1, and ultrasonic bonding was performed in a manner that they were completely bonded. Ultrasonic bonding was performed by ultrasonic welding lamination in a three-layered state of nonwoven fabric 1 / elastic film / nonwoven fabric 2 using an ultrasonic welding device (manufactured by Herrmann, device name: MICROBOND (ULTRABOND48:20)) at a frequency of 20 kHz (output intensity: 1800 W) and a line speed of 100 m / min. The embossed pattern roller used in the welding was a roller having a dot pattern with a welding area of 8% and a diameter of 0.7 mm. Thereafter, activation treatment was performed to obtain a post-treated material 1.
[0121] [Example 2]
[0122] Post-treated material 2 was obtained in the same manner as in Example 1 except that 100 parts by weight of olefin resin 1 (manufactured by SCG Performance Chemicals, trade name: P756C) was used in layer A of the extruder, 46.5 parts by weight of styrene elastomer 1 (manufactured by ZEON Corporation, trade name: Quintac 3620) and 46.5 parts by weight of styrene elastomer 2 (manufactured by ZEON Corporation, trade name: Quintac 3390) were used in layer B of the extruder to prepare an elastic film.
[0123] [Example 3]
[0124] The same operation as in Example 2 was performed except that the elastic film and the nonwoven fabric were heat-fused to obtain a post-processed material 3. The heat-fusion was performed by heat-fusion lamination in a three-layered state of nonwoven fabric 1 / elastic film / nonwoven fabric 2 under the conditions of a treatment temperature of 200°C, a line pressure of 160 N / mm, and a treatment speed of 50 m / min. The embossed pattern roll used in the fusion was a roll having a fusion area of 8% and a dot pattern of 0.7 mm in diameter. Next, an activation treatment was performed to obtain a post-processed material 3.
[0125] [Example 4]
[0126] The same operation as in Example 2 was performed except that the elastic film and the nonwoven fabric were laminated with the aid of an adhesive to obtain a post-processed material 4. The lamination with the adhesive was performed by laminating the nonwoven fabric on both sides of the elastic film using a roller. At this time, a hot melt adhesive (Nitto Bento Company, trade name: AC280) coating (15g / m 2 ) into stripes (adhesive width: 1 mm, interval: 1 mm). Next, activation treatment was performed to obtain post-processed material 4.
[0127] [Example 5]
[0128] A post-treated material 5 was obtained in the same manner as in Example 2 except that nonwoven fabric B (PP spunlace type, basis weight = 35 gsm) was laminated on one surface of the elastic film instead of nonwoven fabric A.
[0129] [Example 6]
[0130] A post-treated material 6 was obtained in the same manner as in Example 2 except that the nonwoven fabric B was laminated on both surfaces of the elastic film.
[0131] [Example 7]
[0132] A post-treated material 7 was obtained in the same manner as in Example 2 except that nonwoven fabric C (PP-polyethylene terephthalate (PET) spunlace type (PP fiber content: 50 wt%), basis weight = 35 gsm) was laminated on both surfaces of the elastic film.
[0133] [Example 8]
[0134] A post-treated material 8 was obtained in the same manner as in Example 2 except that nonwoven fabric D (PP spunlace type, basis weight = 25 gsm) was laminated on both surfaces of the elastic film.
[0135] (Comparative Example 1)
[0136] A post-treated material C1 was obtained in the same manner as in Example 2 except that the nonwoven fabric was not laminated (the resin layer was provided alone).
[0137] (Comparative Example 2)
[0138] A post-treated material C2 was obtained in the same manner as in Example 2 except that nonwoven fabric E (PP spunbond type, basis weight = 20 gsm) was laminated on both surfaces of the elastic film.
[0139] (Comparative Example 3)
[0140] A post-treated material C3 was obtained in the same manner as in Example 4 except that a nonwoven fabric F (cotton spunlace type, basis weight = 35 gsm) was laminated on both surfaces of the elastic film.
[0141] (Comparative Example 4)
[0142] An attempt was made to produce a post-treated material in the same manner as in Example 2 except that the nonwoven fabric F was laminated on both surfaces of the elastic film. However, the nonwoven fabric and the elastic film were not bonded to each other, and no post-treated material was obtained.
[0143] (Comparative Example 5)
[0144] A post-processed material C5 was obtained in the same manner as in Example 2 except that nonwoven fabric G (PE-PET hot air type, basis weight = 25 gsm) was used as the nonwoven fabric layer.
[0145] (Reference example)
[0146] The post-processed material prepared in Example 1 has a thickness of 40 g / m after drying. 2 Adhesive application (Nitto Bento The post-processing material was laminated on a diaper. However, the laminated post-processing material was peeled off from the diaper and could not be used as the post-processing material.
[0147] [evaluate]
[0148] The post-processed materials obtained in Examples, Comparative Examples, and Reference Examples were subjected to the following evaluations.
[0149] <Tensile test>
[0150] The tensile test is evaluated by subjecting the obtained post-processed material to the following test. The post-processed material is cut into a width of 10 mm and a length of 10 cm in a manner that the direction (CD) perpendicular to the film flow direction (MD) becomes the long side to prepare a sample. Each sample is set in a tensile testing machine (ZwickRoell, product name: Z00051kN) in a manner that the distance between the chucks becomes 50 mm, and is stretched to break at a tensile speed of 500 mm / min. The maximum strength, elongation at break, and elongation at 2N are measured at this time. Five samples are used for evaluation respectively, and the average value is used.
[0151] <10-minute retention test>
[0152] The 10-minute holding test is evaluated by subjecting the obtained post-processed material to the following test. The post-processed material is cut into a width of 10 mm and a length of 10 cm in a manner that the direction (CD) perpendicular to the film flow direction (MD) becomes the long side to make a sample. Each sample is set in a tensile testing machine (ZwickRoell, product name: Z0005 1kN) in a manner that the distance between the chucks is 50 mm, and stretched at a tensile speed of 500 mm / min until the elongation reaches 100%. Thereafter, after holding at an elongation of 100% for 10 minutes, return to the initial distance between the chucks. Measure the stress (stress after elongation) after 10 minutes at this time. In addition, the deformation after 10 minutes is calculated by measuring the deformation of the sample after holding for 10 minutes using a ruler. 5 samples are used for evaluation respectively, and the average value is used.
[0153] <Adhesion to Diaper Outer Package>
[0154] The post-processed material cut into 10 mm width in the MD direction was bonded to a commercially available carded nonwoven fabric (24 g / m 2 When the bonded post-treatment material was stretched in the CD direction and no peeling from the nonwoven fabric was observed, it was rated as ○ (good), and when no bonding was achieved and peeling was easily observed, it was rated as × (there is room for improvement).
[0155] <Appearance>
[0156] In the evaluation of the adhesion of the above-mentioned diaper outer packaging body, when attached to a non-woven fabric, if the outermost surface of the laminate (the side observed from the outside) is formed by a non-woven fabric and is light and soft, it is set to ○○ (very good); when it is formed by a non-woven fabric but feels hard, it is set to ○ (good); when it is formed by a film, it is set to × (there is room for improvement).
[0157] <Ease of discarding>
[0158] When the maximum strength is 3N / 10mm or more, the elongation at break is 150% or more, and the elongation at 2N is 65% or more, it is set to ○○○ (best); when the maximum strength is 3N / 10mm or more, the elongation at break is 150% or more, and the elongation at 2N is 60% or more, it is set to ○○ (very good); when the maximum strength is 3N / 10mm or more, the elongation at break is 150% or more, and the elongation at 2N is 50% or more, it is set to ○ (good); when each evaluation is below the above range, it is set to × (there is room for improvement).
[0159] <Keep Characteristics>
[0160] When the stress after 10 minutes was 1 N / 10 mm or more and the deformation after 10 minutes was 50% or less, it was rated as ○ (good), and otherwise it was rated as × (there is room for improvement).
[0161] <Nonwoven fabric thickness>
[0162] The cross section of the post-processed material was photographed at a magnification of 100 times using a digital microscope "VHX-1000" manufactured by Keyence Corporation, and the thickness of the nonwoven fabric was measured using the image analysis software of the device. It should be noted that in the thickness measurement, when the resin layer (elastic film) is in contact with the nonwoven fabric, the boundary between the resin layer and the nonwoven fabric is set as the outermost surface, or, when the nonwoven fabrics are in contact with each other, at the upper and lower parts of the cross section of the nonwoven fabric, parallel lines with 10 intersections with the fibers are set as the upper and lower sides, respectively, and the length between the upper and lower sides is set as the thickness of the nonwoven fabric. The thickness of the nonwoven fabric is measured under the condition that the number of samples is 3 or more, and the average value is set as the thickness of the nonwoven fabric.
[0163] [Table 1]
[0164]
[0165] Industrial Applicability
[0166] The absorbent article post-treatment material according to the embodiment of the present invention can be used for any appropriate article that can effectively utilize the effects of the present invention. Representative examples of the absorbent article of the present invention include diapers (pants-type diapers, belt-type diapers).
[0167] Description of Reference Numerals
[0168] 100 Post-processing materials for absorbent articles
[0169] 10Resin layer including elastomer layer
[0170] 20a Nonwoven fabric layer
[0171] 20b nonwoven fabric layer
[0172] 30Joint
[0173] 200 absorbent articles
Claims
1. A post-treatment material for an absorbent article, comprising a nonwoven fabric layer, a resin layer and a joining portion, wherein the nonwoven fabric layer comprises a density of 15 kg / m 3 ~120kg / m 3 The nonwoven fabric contains chemical fibers, the resin layer contains an elastomer layer, and the joint portion is joined to the outer packaging body of the absorbent article. The nonwoven fabric layer is the outermost surface of the post-treatment material for the absorbent article. The joining portion is a portion configured to be weldable by ultrasonic welding or thermal welding.
2. The post-treatment material for absorbent articles according to claim 1, in, The nonwoven fabric is a spunlace nonwoven fabric, a carded nonwoven fabric, a hot air nonwoven fabric or a spunlace interwoven nonwoven fabric.
3. The post-treatment material for absorbent articles according to claim 1 or 2, in, The chemical fiber is an olefin resin fiber.
4. The post-treatment material for absorbent articles according to claim 3, in, The chemical fiber is polypropylene resin fiber.
5. The post-treatment material for absorbent articles according to claim 4, in, The nonwoven fabric contains 30% by weight or more of polypropylene resin fibers.
6. The post-treatment material for absorbent articles according to any one of claims 1 to 5, in, The elastomer layer includes a styrene-based elastomer or an olefin-based elastomer.
7. The post-treatment material for absorbent articles according to claim 6, in, The elastomer layer includes an olefin-based elastomer.
8. The post-treatment material for absorbent articles according to claim 7, in, The olefin-based elastomer is a propylene-based elastomer.
9. The post-treatment material for an absorbent article according to any one of claims 1 to 8, comprising a folded structure.
10. The post-treatment material for absorbent articles according to any one of claims 1 to 9, which is in a strip shape and has a length of 50 mm to 250 mm.
11. The post-treatment material for absorbent articles according to any one of claims 1 to 10, which has a basis weight of 50 g / m 2 ~150g / m 2 .
12. The post-treatment material for absorbent articles according to any one of claims 1 to 11, which has an elongation at break of 150% to 600%.
13. The post-treatment material for absorbent articles according to any one of claims 1 to 12, which has a maximum strength of 2 N / 10 mm or more.
14. The absorbent article post-treatment material according to any one of claims 1 to 13, which has a post-elongation stress of 0.5 N / 10 mm or more.
15. The post-treatment material for absorbent articles according to any one of claims 1 to 14, wherein the elongation under a load of 2N is 30% or more.
16. An absorbent article comprising an outer packaging body and the absorbent article post-treatment material according to any one of claims 1 to 15.
17. The absorbent article according to claim 16, in, The outer surface of the outer packaging body is a non-woven fabric with a density of 15 kg / m 3 ~120kg / m 3 .
18. The absorbent article according to claim 16 or 17, which is a pants-type diaper.
19. A method for manufacturing an absorbent article, comprising: include: A nonwoven fabric layer and a resin layer including an elastomer layer are laminated to produce a laminate, wherein the nonwoven fabric layer includes a resin layer having a density of 15 kg / m 3 ~120kg / m 3 And nonwoven fabrics containing chemical fibers, The laminate is joined to the outer packaging body of the absorbent article by ultrasonic welding or thermal welding.